Preparation process of optical diaphragm with efficient heating function

By using precision magnetron coating technology of indium tin oxide and silicon oxide materials on the window sheet and precision steel screen printing technology, combined with chemical tempering and annealing treatment, the problems of slow heating speed and unstable structure in the existing technology are solved, and the problem of Highly efficient heating and long-life optical window sheets.

CN119082670APending Publication Date: 2024-12-06JIANGXI JINGCHUANG TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410974429.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The window sheet with existing heating functions has problems such as slow heating speed, uneven regional heating, poor structural faults and resistance stability, resulting in unstable performance and short service life.

Method used

The high-precision conductive film is prepared by using indium tin oxide and silicon oxide materials through precision magnetron coating technology, and the silver paste is printed on the surface of the glass substrate with precision steel screen printing technology to form an efficient heating structure, and the film layer is lifted through chemical tempering and annealing treatment. Density, cancel the ink layer and directly make a conductive film, and design and optimize the resistance value and power-on position.

Benefits of technology

It achieves fast heating speed, uniform heating throughout the region, high product stability and long service life, and solves the problems of unstable heating function and poor weather resistance in the prior art.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082670A_ABST
    Figure CN119082670A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation process of an optical diaphragm with an efficient heating function. The preparation process comprises the following steps: 1) physical polishing; 2) chemical tempering; 3) manufacturing a conductive film layer; 4) annealing; 5) silver paste printing; (6) black oil printing; 7) manufacturing an AR film; and (8) AR + AF film plating is carried out, and the final optical diaphragm is obtained. Compared with the prior art, the heating device has the advantages of high heating speed, good stability, long service life and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a process for preparing an optical window piece, and in particular to a process for preparing an optical window piece with a high-efficiency heating function. Background Art

[0002] The development of windows with heating function is based on a variety of practical needs and technical development backgrounds. In the aviation field, when the aircraft is flying at high altitude, the outside temperature is extremely low, and the cockpit windows are prone to ice or fog, which seriously affects the pilot's vision and threatens flight safety. To solve this problem, the development of windows with heating function has become an inevitable demand. In the automotive industry, under bad weather conditions, car windows are prone to frost and fog, affecting the driver's vision. With the continuous advancement of automotive technology and the improvement of people's requirements for driving safety, heated car windows have emerged to ensure that drivers can have a clear view in all weather conditions. In the industrial field, some production processes need to be carried out under specific temperature and humidity conditions. If the observation window is frosted, fogged or condensed due to temperature changes, it will interfere with the monitoring of the production process. In order to achieve precise production control and quality monitoring, it is necessary to develop windows with heating function to maintain good observation conditions. Therefore, windows with heating function and stable and reliable performance are urgently needed by various industries.

[0003] However, most of the window pieces with heating functions on the market currently have the following defects: 1. The window piece is coated with silver paste around the window, and then the silver paste is energized to generate heat to heat the entire window, but this method has a slow heating speed and there is a problem of uneven regional heating; 2. Many heating function window pieces use conductive materials on ink, which has structural fault problems, resulting in poor resistance stability and unstable heating function. At the same time, it is affected by the poor weather resistance of ink, resulting in a short product life; 3. The power-on position of the heating function window piece is not designed reasonably, resulting in poor product performance stability. Summary of the invention

[0004] The purpose of the present invention is to overcome the defects of the above-mentioned prior art and provide a process for preparing an optical window with efficient heating function.

[0005] The purpose of the present invention can be achieved by the following technical solutions:

[0006] A process for preparing an optical window with a high-efficiency heating function, the process comprising the following steps:

[0007] 1) Physical polishing: The glass substrate is subjected to double-sided rotating physical polishing by a polishing machine using a polishing liquid prepared from polyurethane polishing leather and cerium oxide polishing powder as the processing material;

[0008] 2) Chemical tempering: Sodium ions in the glass are exchanged with potassium ions in the tempering solution;

[0009] 3) Conductive film layer preparation: One side of the glass substrate is selected as the A side, and is placed in a coating fixture. A sputtering coating machine is used. Under vacuum conditions, ICP energy bombardment is used. Indium tin oxide and silicon oxide are two coating materials that are alternately sputtered on the surface of the substrate under the reaction of chemical vapor deposition to form a conductive film.

[0010] 4) Annealing: After the film deposition in the sputtering coating machine is completed, the product is taken out and placed in a high-temperature annealing furnace for annealing and crystallization under a nitrogen protective atmosphere to obtain a semi-finished window piece;

[0011] 5) Silver paste printing: According to the product structure design requirements, at the edge of the window piece, the conductive silver paste is directly printed on the surface of the conductive film through precision steel screen printing technology as the energized welding point;

[0012] 6) Black ink printing: Select the opposite side of side A as side B, and print black ink on side B using precision steel screen printing technology;

[0013] 7) AR film production: an evaporation coating machine is used on the surface of the conductive film. Under vacuum conditions, ion source energy bombardment is used to form an anti-reflection and anti-reflection film by physical vapor deposition using silicon oxide and titanium oxide as coating materials;

[0014] 8) AR+AF film coating: The same evaporation coating machine vacuum coating technology is used on the B side, with silicon oxide, titanium oxide and anti-fouling film particles as coating materials to make a layer of AR+AF film to obtain the final optical window piece.

[0015] Furthermore, the conductive film in 3) is a transparent film with a thickness of 60 nm.

[0016] Furthermore, the annealing condition in 4) is annealing at 300° C. for 4 hours.

[0017] Furthermore, the thickness of the conductive film, the optimal position of silver paste printing and the corresponding resistance value are obtained by the following calculation formula:

[0018]

[0019] Where R is the resistance value, R f is the square resistance, L is the distance between the two silver paste electrodes, W is the film width of the conductive film between the two electrodes, ρ is the film resistivity of the conductive film, and d is the thickness of the conductive film.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] 1. Fast heating speed and uniform heating in the whole area: The present invention uses indium tin oxide and silicon oxide as materials and adopts precision magnetron coating technology to prepare a high-precision, high-strength conductive film that can evenly cover the entire window area without interfering with the line of sight in the window area. Then silver paste is printed at both ends as welding points. After power is turned on, the entire window area of ​​the entire optical window can be quickly heated and heated to remove frost, water vapor, etc. on the window.

[0022] 2. Good product stability: The present invention makes the conductive film directly on the surface of the glass substrate instead of making it on the surface ink. The surface flatness of the substrate is much better than that of the ink, eliminating the influence of the ink on the conductive material, so that the product performance consistency and stability are high.

[0023] 3. Longer product life: The optical window piece of the present invention eliminates the ink on the surface of the substrate, and the conductive film is directly and evenly made on the surface of the substrate, eliminating the damage to the conductive material caused by the poor weather resistance of the ink during the outdoor use of the product, thereby greatly improving the service life of the product.

[0024] 4. Product design optimization: The present invention summarizes the optimal power-on (silver paste printing) position design and conductive film thickness design, and the corresponding resistance value law through calculation simulation and actual verification of the resistance value design of the optical window with heating function, so as to solve the problem of product performance stability from the product design perspective. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 is a process flow chart of the present invention;

[0026] Figure 2 It is a schematic diagram of the product structure of the present invention;

[0027] Figure 3 A physical picture of the product of the present invention;

[0028] Figure 4 It is a schematic diagram of the initial resistance distribution of a conventional optical window and the optical window of the present invention;

[0029] Figure 5 It is a schematic diagram of the resistance variation of the conventional optical window and the optical window of the present invention after the weather resistance test;

[0030] Figure 6 It is a schematic diagram of the design of the optical window of the present invention. DETAILED DESCRIPTION

[0031] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to the following embodiments.

[0032] Example

[0033] like Figures 1 to 3 As shown, a process for preparing an optical window sheet with a high-efficiency heating function, the preparation process comprises the following steps:

[0034] 1) Physical polishing: Due to the impurities and unevenness on the surface of the glass substrate, a polishing liquid composed of polyurethane polishing leather and cerium oxide polishing powder is used as the processing material. Under the action of a polishing machine, the glass substrate is subjected to double-sided rotating physical polishing to remove the uneven parts and impurities on the surface of the substrate, thereby improving the flatness and smoothness of the substrate surface;

[0035] 2) Chemical tempering: Sodium ions in the glass are exchanged with potassium ions in the tempering liquid. Since the radius of potassium ions is larger than that of sodium ions, the difference in ion volume is used to form embedded extrusion stress on the surface layer of the glass, which plays a role in improving the strength of the substrate.

[0036] 3) Conductive film (ITO) film production: One side of the glass substrate is selected as the A side, which is placed in a coating fixture and a sputtering coating machine is used. Under vacuum conditions, ICP energy bombardment is used to alternately sputter indium tin oxide and silicon oxide coating materials on the surface of the substrate under the reaction of chemical vapor deposition to form a 60nm thick conductive film that is uniform, compact and transparent, so that the window has the function of uniform heating over the entire area;

[0037] 4) Annealing: After the film deposition in the sputtering coating machine is completed, the product is taken out and placed in a high-temperature annealing furnace for annealing and crystallization under a nitrogen atmosphere to obtain a semi-finished window piece. The annealing condition is annealing at 300°C for 4 hours. Through annealing, the density and strength of the film layer are improved. It can better adapt to various extreme environments;

[0038] 5) Silver paste printing: According to the product structure design requirements, at the edge of the window piece, the conductive silver paste is directly printed on the surface of the conductive film through precision steel screen printing technology as the power welding point to achieve the function of electrical connection;

[0039] 6) Black ink printing: Select the opposite side of the A side as the B side, and use the precision steel screen printing technology to print black ink on the B side to play a shielding role. After the product is assembled, the silver paste and internal structure of the A side will not be visible from the B side (appearance surface);

[0040] 7) AR film (anti-reflection and anti-reflection film) production: an evaporation coating machine is used on the surface of the conductive film. Under vacuum conditions, ion source energy bombardment is used to make a layer of anti-reflection and anti-reflection film by physical vapor deposition of silicon oxide and titanium oxide as coating materials, so as to reduce the reflectivity of the conductive film and increase the light transmittance of the window hole;

[0041] 8) AR+AF (anti-fingerprint film) coating: The vacuum coating technology of the evaporation coating machine is also used on the B side. Silicon oxide, titanium oxide and anti-fouling film particles are used as coating materials to make a layer of AR+AF film to obtain the final optical window piece. While increasing the overall light transmittance, it also has waterproof, anti-fouling and scratch-resistant properties.

[0042] like Figure 4 As shown, from the comparison of the initial resistance values ​​of the same batch of products, the resistance concentration of the present invention is significantly better than that of the traditional optical window piece, which shows that the optical window piece of the present invention has good structural stability.

[0043] like Figure 5 As shown, from the comparison of the resistance change after the weather resistance test, the variable mean and variable dispersion of the present invention are better than those of the traditional optical window film, indicating that the performance stability and life span of the product of the present invention in later use are better.

[0044] Through the calculation simulation and actual verification of the resistance value design of the heating function window, the optimal power-on (silver paste printing) position design and the conductive film thickness design, as well as the corresponding resistance value law, are summarized to solve the problem of product performance stability from the product design perspective; the thickness of the conductive film, the optimal position of silver paste printing and the corresponding resistance value law are obtained by the following calculation formula:

[0045]

[0046] Where R is the resistance value, R f is the square resistance, L is the distance between the two silver paste electrodes, W is the film width of the conductive film between the two electrodes, ρ is the film resistivity of the conductive film, and d is the thickness of the conductive film.

[0047] like Figure 6 As shown, the spacing between the two silver paste printing positions of the optical window is L, and the spacing between the non-silver paste printing positions of the optical window is W. According to the above formula, if you want to increase the resistance of the optical window, you have to reduce the ITO film thickness. The thinner the ITO film thickness, the worse the stability of the optical window. And the larger the aspect ratio of the silver paste design position of the optical window, the easier it is to increase the ITO resistance value. Therefore, the silver paste is printed at both ends of the long direction of the optical window as much as possible to maximize the L / W ratio. The larger the ratio, the larger the resistance specification for the same film thickness. And if you want to increase the resistance, the smaller the amount of ITO film thickness that needs to be reduced.

[0048] Table 1 below lists in detail the theoretical resistance data obtained for different L / W values ​​and different ITO film thicknesses.

[0049] Table 1 Reference table of resistance values ​​of different L / W values ​​and different ITO film thicknesses

[0050]

[0051] As shown in Table 1, the ITO film thickness is relatively stable when it is above 40nm; at the same time, the optimal L / W value of the silver paste design is between 0.8-1.2.

[0052] The preparation process of the optical window with heating function of the present invention makes the product more efficient and more practical in practical application through the development and application of conductive film and product design optimization. At the same time, the structural optimization greatly improves the performance stability and service life of the product, and improves the performance and practicality of the window with heating function.

[0053] The preferred specific embodiments of the present invention are described in detail above. It should be understood that a person skilled in the art can make many modifications and changes based on the concept of the present invention without creative work. Therefore, any technical solution that can be obtained by a person skilled in the art through logical analysis, reasoning, or limited experiments based on the concept of the present invention on the basis of the prior art should be within the scope of protection determined by the claims.

Claims

1. A process for preparing an optical window with efficient heating function, characterized in that: The preparation process comprises the following steps: 1) Physical polishing: The glass substrate is subjected to double-sided rotating physical polishing by a polishing machine using a polishing liquid prepared from polyurethane polishing leather and cerium oxide polishing powder as the processing material; 2) Chemical tempering: Sodium ions in the glass are exchanged with potassium ions in the tempering solution; 3) Conductive film layer preparation: One side of the glass substrate is selected as the A side, and is placed in a coating fixture. A sputtering coating machine is used. Under vacuum conditions, ICP energy bombardment is used. Indium tin oxide and silicon oxide are two coating materials that are alternately sputtered on the surface of the substrate under the reaction of chemical vapor deposition to form a conductive film. 4) Annealing: After the film deposition in the sputtering coating machine is completed, the product is taken out and placed in a high-temperature annealing furnace for annealing and crystallization under a nitrogen protective atmosphere to obtain a semi-finished window piece; 5) Silver paste printing: According to the product structure design requirements, at the edge of the window piece, the conductive silver paste is directly printed on the surface of the conductive film through precision steel screen printing technology as the energized welding point; 6) Black ink printing: Select the opposite side of side A as side B, and print black ink on side B using precision steel screen printing technology; 7) AR film production: an evaporation coating machine is used on the surface of the conductive film. Under vacuum conditions, ion source energy bombardment is used to form an anti-reflection and anti-reflection film by physical vapor deposition using silicon oxide and titanium oxide as coating materials; 8) AR+AF film coating: The same evaporation coating machine vacuum coating technology is used on the B side, with silicon oxide, titanium oxide and anti-fouling film particles as coating materials to make a layer of AR+AF film to obtain the final optical window piece.

2. The process for preparing an optical window with high-efficiency heating function according to claim 1, characterized in that: The conductive film in 3) is a transparent film with a thickness of 60nm.

3. The process for preparing an optical window with high-efficiency heating function according to claim 1, characterized in that: The annealing condition in 4) is annealing at 300° C. for 4 hours.

4. The process for preparing an optical window with high-efficiency heating function according to claim 2, characterized in that: The thickness of the conductive film, the optimal position of silver paste printing and the corresponding resistance value are obtained by the following calculation formula: Where R is the resistance value, R f is the square resistance, L is the distance between the two silver paste electrodes, W is the film width of the conductive film between the two electrodes, ρ is the film resistivity of the conductive film, and d is the thickness of the conductive film.