Composite catalyst as well as preparation method and application thereof

A composite CoP/Ni2P catalyst derived from MOFs addresses the inefficiencies of the Haber-Bosch process by providing high ammonia yield and low energy consumption through a novel synthesis method, enhancing electron transfer and reducing environmental impact.

CN119082779APending Publication Date: 2024-12-06BOZHOU SHANGDA ENG TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411023924.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The traditional Haber-Bosch process for ammonia synthesis requires high temperatures and pressures, consumes significant energy and fossil fuels, and emits large amounts of CO2, while alternative methods like bio-enzyme and photocatalytic nitrogen fixation face efficiency and scalability challenges.

Method used

A composite catalyst of CoP and Ni2P derived from MOFs is synthesized through a method involving Ni-Ni HCP nanoplates, etching with tannic acid, and high-temperature phosphating, creating a two-dimensional structure with sulfur vacancies and heterojunctions for enhanced electron transfer.

Benefits of technology

The catalyst achieves high ammonia yield and Faradaic efficiency with low energy consumption and emissions, supporting sustainable industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082779A_ABST
    Figure CN119082779A_ABST
Patent Text Reader

Abstract

The invention provides a composite catalyst and a preparation method and application thereof, the catalyst obtained by the preparation method takes a two-dimensional Ni-based HCP as a matrix, has a hollow composite structure, sulfur vacancies and heterojunctions, significantly optimizes the microstructure of the catalyst and improves the electron transfer efficiency. According to the invention, the specific surface area of the catalyst is increased, sufficient contact between reactants and active sites is promoted, and the energy barrier of the reaction is reduced by regulating and controlling the electronic structure. Moreover, a two-dimensional nano-plate Ni-Ni HCP is synthesized by adopting a simple wet chemical method, Co < 2 + > is uniformly adsorbed on the surface of the Ni-Ni HCP to form ZIF-67 by utilizing the electrostatic attraction effect of PVP, then the ZIF-67 is converted into a hollow structure through a tannic acid etching technology, and the ZIF-67 is phosphorized at high temperature to obtain the CoP / Ni2P composite material with excellent performance. The catalyst exhibits an ammonia yield of up to 9.8 [mu] g h <-1 >. Mg <-1 > cat and a Faraday efficiency of 9.5% at a potential of-0.3 V vs RHE.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of new nano materials, and in particular to the technical field of synthesizing ammonia (NH3) by electrocatalytic nitrogen reduction reaction (NRR). Background Art

[0002] Ammonia (NH3), as a multifunctional chemical, plays an important role in the global industrial system. In the agricultural field, ammonia and its derivatives constitute the cornerstone of fertilizers, especially the production of nitrogen fertilizers, which is directly related to the guarantee of global food security. More than 80% of synthetic ammonia is used for this purpose, ensuring that the growing population can get adequate nutrition supply. In addition, ammonia is an indispensable raw material for many industries such as pharmaceuticals and chemicals. From basic chemicals such as nitric acid and explosives to the synthesis of complex drug molecules, ammonia is indispensable. What is more striking is that ammonia is regarded as a highly potential clean energy carrier and storage medium due to its high energy density, environmental friendliness (the combustion products are only water and nitrogen) and relatively low energy storage cost (compared to hydrogen), which provides new ideas for future energy transformation and sustainable development.

[0003] Although ammonia has broad application prospects, its traditional production method - the Haber-Bosch process - faces many challenges. First, the method has strict requirements on reaction conditions, requiring high temperature (300-500°C) and high pressure (150-200 atmospheres) environment, which not only increases the energy consumption and cost of the production process, but also makes the equipment complex and difficult to maintain. Secondly, the Haber-Bosch process is highly dependent on fossil fuels (mainly natural gas), consuming about 1% of the world's natural gas and 1% of the total energy each year, while emitting a large amount of carbon dioxide, exacerbating the global greenhouse effect and climate change problems.

[0004] With the global pursuit of carbon neutrality goals and the increasing emphasis on renewable energy, it has become particularly urgent to find an ammonia synthesis technology that can be carried out under mild conditions, with renewable raw materials and a green and environmentally friendly production process. At present, although a variety of alternatives have been proposed, such as bio-enzyme nitrogen fixation, photocatalytic nitrogen fixation and electrocatalytic ammonia synthesis, these methods still face many technical bottlenecks and economic challenges in practical applications. For example, although the bio-enzyme nitrogen fixation method is environmentally friendly, its nitrogen fixation efficiency is low and it is difficult to meet the needs of large-scale industrial production. The photocatalytic nitrogen fixation method is limited by the intermittent nature and conversion efficiency of solar energy.

[0005] As for the electrocatalytic ammonia synthesis method, since the N≡N bond is one of the most stable chemical bonds and is difficult to break at room temperature, it is more likely to undergo a competitive hydrogen evolution reaction, resulting in poor NRR selectivity; therefore, the electrocatalytic ammonia synthesis method requires an efficient catalyst and a stable electrolysis system to achieve economically feasible ammonia production. Summary of the invention

[0006] In order to overcome the deficiencies of the prior art and develop an ammonia synthesis technology that can be carried out under mild conditions and achieve high efficiency, low energy consumption and low emissions, the present invention provides a composite catalyst of CoP and Ni2P derived from MOFs, a preparation method and application thereof.

[0007] The first aspect of the present invention is to provide a method for preparing a composite catalyst of CoP and Ni2P derived from MOFs, the steps comprising:

[0008] Provide Ni-Ni HCP (Ni-Ni Hofmann-type coordination polymer) nanoplates;

[0009] Ni-Ni HCP nanoplates, cobalt (Co 2+ ) salt and dimethylimidazole are mixed in a first solvent to obtain a Ni-Ni HCP / ZIF-67 composite;

[0010] The Ni-Ni HCP / ZIF-67 complex is etched with tannic acid to obtain Ni-Ni HCP / ZIF-67-TA; the Ni-Ni HCP / ZIF-67-TA is subjected to high temperature phosphating to obtain a CoP / Ni2P composite material, i.e. a composite catalyst of CoP and Ni2P.

[0011] In a preferred embodiment, the method for preparing the Ni-Ni HCP nanoplate comprises the following steps: 2+ ) salt, citrate, and potassium tetracyanonickelate are mixed in a second solvent to obtain Ni-Ni Hofmann coordination polymer nanoplates, namely Ni-Ni HCP nanoplates.

[0012] Preferably, the nickel salt may be an inorganic acid salt or an organic acid salt, and is preferably one or more combinations selected from Ni(NO3)2, NiCO3, NiSO4, NiCl2, NiBr2, Ni(CH3COO)2, and Ni(HCOO)2.

[0013] Preferably, the nickel salt may be provided in the form of a hydrate, an aqueous solution or an alcohol solution.

[0014] Preferably, the citrate is selected from one or more combinations of calcium citrate, potassium citrate, ammonium citrate, sodium dihydrogen citrate and sodium citrate.

[0015] Preferably, the citrate may be provided in the form of a hydrate, an aqueous solution or an alcohol solution.

[0016] In a preferred embodiment, the nickel (Ni 2+) salt, citrate, and potassium tetracyanonitric acid are mixed in the second solvent and the first dispersant is also added.

[0017] Preferably, the first dispersant is selected from one or more combinations of polyvinyl pyrrolidone (PVP), sodium dodecyl sulfate (SDS), polyethylene glycol (PEG), sodium polystyrene sulfonate (PSS), polyacrylic acid (PAA), and polyethyleneimine (PEI).

[0018] More preferably, the weight average molecular weight (Mw) of the first dispersant is 5000-60000 g / mol, preferably 10000-50000 g / mol, more preferably 20000-40000 g / mol.

[0019] Preferably, the nickel (Ni 2+ ) salt, citrate, and potassium tetracyanonitric acid are mixed in a second solvent, the steps comprising,

[0020] Nickel (Ni 2+ ) salt and citrate are first mixed in part of the second solvent to obtain solution A;

[0021] mixing potassium tetracyanonickelate with a portion of the second solvent to obtain a solution B;

[0022] The B solution is mixed with the A solution, and more preferably, the B solution is poured into the A solution.

[0023] More preferably, the first dispersant is mixed with nickel (Ni 2+ ) salt and citrate are mixed together in a second solvent to obtain the A solution.

[0024] Preferably, the nickel (Ni 2+ ) salt, citrate, and potassium tetracyanonickelate are mixed in the second solvent and then aged.

[0025] More preferably, the nickel (Ni 2+ ) salt, citrate, potassium tetracyanonickelate, and the first dispersant are mixed in the second solvent, and then the aging is performed.

[0026] More preferably, the aging temperature is 5-50°C, preferably 10-40°C, more preferably 20-30°C, more preferably 20-25°C.

[0027] More preferably, the aging time is 12-40 h, preferably 16-30 h, more preferably 20-24 h.

[0028] More preferably, the Ni-Ni HCP nanoplate is mixed with cobalt (Co 2+ ) Salt and dimethylimidazole must be cleaned before mixing.

[0029] More preferably, the cleaning solvent used for cleaning the Ni-Ni HCP nanoplate is one or more of water, ethanol and methanol.

[0030] More preferably, the cleaned Ni-Ni HCP nanoplate is further dried.

[0031] More preferably, the drying temperature of the Ni-Ni HCP nanoplate is 50-100°C, preferably 55-80°C, more preferably 60-70°C.

[0032] More preferably, the drying time of the Ni-Ni HCP nanoplate is 8-48 h, preferably 12-36 h, and more preferably 16-24 h.

[0033] Preferably, the second solvent can be one or more of water, alcohol, ether, ester, ketone, nitrile, halogenated hydrocarbon, aromatic hydrocarbon, and ionic liquid, and is preferably selected from: water, N,N-dimethylformamide, methanol, ethanol, ether, tetrahydrofuran, acetonitrile, valeronitrile, methoxypropionitrile, butyronitrile, adiponitrile, benzyl cyanide, chloroacetonitrile, dichloromethane, carbon tetrachloride, ethyl acetate, acetone, N-methylpyrrolidone, toluene, ionic liquid (such as 1-butyl-3-methylimidazolium hexafluorophosphate) and one or more combinations of solvents mixed.

[0034] Preferably, the cobalt salt may be an inorganic acid salt or an organic acid salt, and is preferably one or more combinations selected from Co(NO3)2, CoCO3, CoSO4, CoCl2, CoBr2, Co(CH3COO)2, and Co(HCOO)2.

[0035] Preferably, the cobalt salt may be provided in the form of a hydrate, an aqueous solution or an alcohol solution.

[0036] Preferably, the first solvent can be one or more of water, alcohol, ether, ester, ketone, nitrile, halogenated hydrocarbon, aromatic hydrocarbon, and ionic liquid, and is preferably selected from: water, N,N-dimethylformamide, methanol, ethanol, ether, tetrahydrofuran, acetonitrile, valeronitrile, methoxypropionitrile, butyronitrile, adiponitrile, benzyl cyanide, chloroacetonitrile, dichloromethane, carbon tetrachloride, ethyl acetate, acetone, N-methylpyrrolidone, toluene, ionic liquid (such as 1-butyl-3-methylimidazolium hexafluorophosphate) and one or more combinations of solvents mixed.

[0037] In a preferred embodiment, the Ni-Ni HCP nanoplate, cobalt (Co 2+ ) salt and dimethylimidazole are mixed in the first solvent and a second dispersant is also added.

[0038] Preferably, the second dispersant is selected from one or more combinations of polyvinyl pyrrolidone (PVP), sodium dodecyl sulfate (SDS), polyethylene glycol (PEG), sodium polystyrene sulfonate (PSS), polyacrylic acid (PAA), and polyethyleneimine (PEI).

[0039] Preferably, the Ni-Ni HCP nanoplate, cobalt salt and dimethylimidazole are mixed in a first solvent, and the steps include:

[0040] Dispersing the Ni-Ni HCP nanoplates in a portion of the first solvent to obtain a first solution;

[0041] Mixing cobalt salt and dimethylimidazole in part of the first solvent to obtain a second solution;

[0042] The first solution is mixed with the second solution, preferably, the second solution is added to the first solution and mixed.

[0043] More preferably, the second dispersant is mixed with the Ni-Ni HCP nanoplates in the portion of the first solvent to obtain the first solution.

[0044] More preferably, the cobalt salt is mixed in part of the first solvent to obtain a cobalt salt solution.

[0045] More preferably, dimethylimidazole is mixed in part of the first solvent to obtain a dimethylimidazole solution.

[0046] More preferably, the cobalt salt solution and the dimethylimidazole solution are added to the first solution at the same time and mixed to obtain the Ni-NiHCP / ZIF-67 composite.

[0047] More preferably, the Ni-Ni HCP / ZIF-67 composite is cleaned before etching.

[0048] More preferably, the cleaning solvent used for cleaning the Ni-Ni HCP / ZIF-67 composite is one or more of water, ethanol and methanol.

[0049] More preferably, the washed Ni-Ni HCP / ZIF-67 composite is further dried.

[0050] More preferably, the drying temperature of the Ni-Ni HCP / ZIF-67 composite is 50-100°C, preferably 55-80°C, more preferably 60-70°C.

[0051] In a preferred embodiment, the tannic acid etches the Ni-Ni HCP / ZIF-67 complex, and the steps include:

[0052] dispersing the Ni-Ni HCP / ZIF-67 complex in a third solvent to obtain a third solution;

[0053] providing a solution of tannic acid dispersed in a third solvent, i.e., a tannic acid solution;

[0054] adding alkali to the tannic acid solution and adjusting the pH value to a preset value to obtain a fourth solution;

[0055] The fourth solution is added to the third solution to react and obtain the Ni-Ni HCP / ZIF-67-TA.

[0056] Preferably, the third solvent can be one or more of water, alcohol, ether, ester, ketone, nitrile, halogenated hydrocarbon, aromatic hydrocarbon, and ionic liquid, and is preferably selected from: water, N,N-dimethylformamide, methanol, ethanol, ether, tetrahydrofuran, acetonitrile, valeronitrile, methoxypropionitrile, butyronitrile, adiponitrile, benzyl cyanide, chloroacetonitrile, dichloromethane, carbon tetrachloride, ethyl acetate, acetone, N-methylpyrrolidone, toluene, ionic liquid (such as 1-butyl-3-methylimidazolium hexafluorophosphate) and one or more combinations of solvents mixed.

[0057] Preferably, the tannic acid concentration of the tannic acid solution is 10-50 mmol / L, preferably 15-40 mmol / L, more preferably 24-30 mmol / L.

[0058] Preferably, the base is provided in the form of a solid, an aqueous solution, or an alcoholic solution.

[0059] Preferably, the base is provided in the form of an aqueous solution or an alcohol solution. More preferably, the concentration of the base (in terms of free OH dissolved in the solution) is - The molecular weight of the present invention is 1-10 mol / L, preferably 2-8 mol / L, and more preferably 4-6 mol / L.

[0060] Preferably, the base is selected from one or more of sodium hydroxide (NaOH), potassium hydroxide (KOH), sodium carbonate (Na2CO3), sodium bicarbonate (NaHCO3), and aqueous ammonia (NH3·H2O).

[0061] Preferably, the preset pH value is 7-14, preferably 8-12, and more preferably 8-10.

[0062] Preferably, the fourth solution is added to the third solution in a dropwise manner.

[0063] Preferably, the Ni-Ni HCP / ZIF-67-TA is cleaned before high-temperature phosphating.

[0064] More preferably, the cleaning solvent used for cleaning the Ni-Ni HCP / ZIF-67-TA is one or more of water, ethanol and methanol.

[0065] More preferably, the washed Ni-Ni HCP / ZIF-67-TA is further dried.

[0066] More preferably, the drying temperature of the Ni-Ni HCP / ZIF-67-TA is 50-100°C, preferably 55-80°C, and more preferably 60-70°C.

[0067] More preferably, the drying time of the Ni-Ni HCP / ZIF-67-TA is 8-48 h, preferably 10-36 h, and more preferably 12-24 h.

[0068] In a preferred embodiment, the high temperature phosphating step comprises:

[0069] Ni-Ni HCP / ZIF-67-TA and phosphate were calcined in a closed environment to obtain a composite catalyst of CoP and Ni2P.

[0070] Preferably, the phosphate is selected from phosphate (PO4 3- ), phosphite (PO2 - ), hypophosphite (PO2 3- )

[0071] Specifically, the phosphate includes one or more combinations of trisodium phosphate, tripotassium phosphate, potassium dihydrogen phosphate, sodium dihydrogen phosphate, dipotassium hydrogen phosphate, disodium hydrogen phosphate, sodium hypophosphite, potassium hypophosphite, sodium phosphite, and potassium phosphite.

[0072] Preferably, the calcination temperature is 300-600°C, preferably 400-500°C, more preferably 450-480°C.

[0073] Preferably, the calcination time is 60-300 min, preferably 100-200 min, more preferably 120-150 min.

[0074] Preferably, the heating rate of the calcination is 1-5°C / min, preferably 1.5-3°C / min, more preferably 2-2.5°C / min.

[0075] The second aspect of the present invention is to provide a composite catalyst of CoP and Ni2P, wherein the mass ratio of CoP to Ni2P in the composite catalyst is (1-20):1, preferably (1-15):1, and more preferably (1-10):1.

[0076] Preferably, the porosity of the composite catalyst is 10-70%, preferably 20-60%, more preferably 30-50%.

[0077] Preferably, the pore size of the composite catalyst is 5-80 nm, preferably 10-75 nm, more preferably 20-70 nm.

[0078] Preferably, the particle size of the composite catalyst is 0.5-8 μm, preferably 1-6 μm, more preferably 2-5 μm.

[0079] Preferably, the composite catalyst of CoP and Ni2P is obtained based on the aforementioned preparation method.

[0080] The third aspect of the present invention is to provide an application of a composite catalyst of CoP and Ni2P derived from MOFs, and the composite catalyst can be used for electrocatalytic synthesis of ammonia. Alternatively, the third aspect of the present invention provides a method for electrocatalytic synthesis of ammonia, comprising electrocatalysis using a composite catalyst of CoP and Ni2P derived from MOFs.

[0081] Compared with the prior art, the beneficial technical effects of the present invention are as follows:

[0082] The present invention provides a method for preparing a composite catalyst of CoP and Ni2P derived from MOFs. The catalyst obtained by the preparation method has a two-dimensional Ni-based HCP as a matrix, has a hollow composite structure, sulfur vacancies, and a heterojunction, which significantly optimizes the microscopic morphology of the catalyst and improves the electron transfer efficiency.

[0083] The present invention not only increases the specific surface area of ​​the catalyst and promotes sufficient contact between reactants and active sites, but also reduces the energy barrier of the reaction by regulating the electronic structure.

[0084] In addition, the present invention adopts a simple wet chemical method to synthesize the two-dimensional nanoplate Ni-Ni HCP, and utilizes the electrostatic attraction of PVP to make Co 2+ The ZIF-67 was uniformly adsorbed on the surface of Ni-Ni HCP, and then the ZIF-67 was converted into a hollow structure (honeycomb) by tannic acid etching technology, and then phosphated at high temperature to obtain CoP / Ni2P composite materials with excellent performance. At a potential of -0.3 V vs RHE, the catalyst showed a high conductivity of 9.8 μg h -1 mg -1 The high ammonia yield and Faradaic efficiency of CAT of 9.5% provide a new pathway for the electrocatalytic nitrogen reduction reaction (NRR) to synthesize ammonia with high efficiency, low energy consumption and low emissions.

[0085] In addition, the present invention not only helps to alleviate the global energy crisis and climate change pressure, but also provides strong technical support for the sustainable development of multiple industries such as agriculture, chemical industry, and pharmaceuticals.

[0086] In the present application, in the Ni-Ni Hofmann-type coordination polymer nanoplate, Ni-Ni represents the interaction between nickel ions as coordination centers; and the nanoplate refers to the two-dimensional flat structure of the material at the nanoscale.

[0087] In this application specification, "ZIF-67" is a metal organic framework, which is formed by metal ions and organic ligands (such as 2-methylimidazole Im) connected by coordination bonds to form a three-dimensional network structure.

[0088] In this application specification, MOFs derivatives are the process of using metal-organic frameworks (MOFs) as precursors or sacrificial templates to prepare materials with specific morphology, structure and performance through a series of physical or chemical processes (such as pyrolysis, solvent thermal, chemical vapor deposition, etc.). This derivatization process not only retains some excellent properties of MOFs materials, such as high specific surface area, porous structure, adjustable pore size and chemical functionality, but also overcomes the deficiencies of MOFs materials in terms of conductivity and stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0089] Figure 1 (a) is the XRD diffraction pattern of Ni-Ni HCP, Ni-Ni HCP / ZIF-67 and Ni-Ni HCP / ZIF-67-TA; (b) is the XRD diffraction pattern of CoP / Ni2P composite structure; Figure 1 (a) Figure 1 The vertical axis of (b) is intensity.

[0090] Figure 2 In the figure, (ab) are TEM images of CoP / Ni2P obtained in Example 1 of the present invention; (ce) is HRTEM image of CoP / Ni2P obtained in Example 1 of the present invention; (f) is element mapping image of CoP / Ni2P obtained in Example 1 of the present invention; (g) is energy dispersion X-ray spectrum image of CoP / Ni2P obtained in Example 1 of the present invention.

[0091] Figure 3In the figure, (a) is the UV-visible absorption spectrum of standard solutions with different NH3 concentrations, with the horizontal axis being the wavelength; (b) is the ammonia standard curve, with the horizontal axis being the NH3 concentration; (c) is the UV-visible absorption spectrum of standard solutions with different N2H4 concentrations, with the horizontal axis being the wavelength; (d) is the N2H4 calibration curve, with the horizontal axis being the N2H4 concentration and the vertical axis being the absorbance.

[0092] Figure 4 In the figure, (a) is the linear sweep voltammetric curve of CoP / Ni2P obtained in Example 1 of the present invention in 0.10M Na2SO4 electrolyte saturated with Ar and N2, respectively, with the abscissa being the potential and the ordinate being the current density; (b) is the it curve of CoP / Ni2P obtained in Example 1 of the present invention after electrolysis for 2h at different potentials, with the abscissa being the time and the ordinate being the current density; (c) is the UV-Vis absorption spectrum of CoP / Ni2P obtained in Example 1 of the present invention after electrolysis for 2h at different potentials, with the abscissa being the wavelength and the ordinate being the absorbance; (d) is the V NH3 and Fe, the horizontal axis is potential, and the vertical axis is NH3 yield.

[0093] Figure 5Middle: (a) is the current density curve of CoP / Ni2P after reacting for 12 hours at -0.30V vs.RHE potential, with time on the horizontal axis and current density on the vertical axis; (b) is the cycle stability test of CoP / Ni2P at -0.30V vs.RHE potential, with cycle number on the horizontal axis, NH3 yield on the left side of the vertical axis, and Faradaic efficiency on the right side; (c) is the NH3 yield and Fes of CoP / Ni2P after alternating cycles of N2 saturated and Ar saturated electrolytes for 2 hours at -0.30V vs.RHE potential, with potential on the horizontal axis, NH3 yield on the left side of the vertical axis, and Faradaic efficiency on the right side; (d) is the NH3 yield of CoP / Ni2P at -0.30V vs.RHE potential. Ammonia production after 2 h of electrolysis in N2-saturated and Ar-saturated Na2SO4 electrolytes at vs. RHE voltage, and ammonia production at open circuit voltage in N2-saturated Na2SO4 electrolyte. The ordinate is ammonia yield (NH3yield).

[0094] Figure 6 This is a schematic diagram of the structure of Example 1 of the present invention. DETAILED DESCRIPTION

[0095] The embodiments of the present invention provide a composite catalyst of CoP and Ni2P derived from MOFs, a preparation method thereof, and an application thereof. In order to make the purpose, technical scheme, and effect of the present invention clearer and more specific, the present invention is further described in detail with reference to the accompanying drawings and examples. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0096] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged under appropriate circumstances. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0097] Example 1

[0098] This embodiment provides a method for preparing CoP / Ni2P, such as Figure 6 As shown, the steps include:

[0099] (1) Preparation of Ni-Ni HCP: 0.37 g of nickel acetate tetrahydrate, 0.56 g of trisodium citrate dihydrate, and 3 g of polyvinyl pyrrolidone K-30 (Mw=40000) were dissolved in 20 mL of deionized water to form solution A, and 0.36 g of potassium tetracyanonitric acid was dissolved in 20 mL of deionized water to form solution B. Under stirring, solution B was added to solution A within 5 seconds. After continuous stirring for 1 min, the mixed solution was aged at room temperature for 24 h, and the precipitate was collected by centrifugation, washed with water and ethanol, and dried at 70°C overnight to obtain Ni-Ni HCP nanoplates (Ni-Ni Hofmann-type coordination polymer nanoplates).

[0100] (2) Preparation of Ni-Ni HCP / ZIF-67: 60 mg of Ni-Ni HCP was dissolved in 25 mL of methanol, and 0.6 g of polyvinyl pyrrolidone (PVP) was added and vigorously stirred to form a uniform solution. The solution was allowed to stand for 10 min to obtain dispersion A'.

[0101] 0.3 g Co(NO3)2·6H2O and 4.44 g dimethylimidazole (2-MeIm) were dispersed in 25 mL methanol and 50 mL methanol to obtain solutions B' and C'. Solutions B' and C' were added to the uniform solution A' at the same time, stirred for 2 h, and the product was collected by centrifugation, washed with methanol by centrifugation for 3 times, and dried in an oven at 60 ° C to obtain Ni-Ni HCP / ZIF-67 composite.

[0102] (3) Preparation of Ni-Ni HCP / ZIF-67-TA (Ni-Ni HCP / ZIF-67 etched by tannic acid TA): 100 mg Ni-Ni HCP / ZIF-67 was added with 5 mL deionized water and dispersed evenly by ultrasonication to form solution A. 6 mL tannic acid solution (24 mmol / L) was taken with a pipette and the pH of the solution was adjusted with potassium hydroxide solution (6 mol / L) until the pH reached 8, forming solution B.

[0103] Solution B" was added dropwise into solution A" using a syringe, and magnetic stirring was continued for 10 min. The product was collected by centrifugation, washed twice with water and then twice with ethanol, and dried in vacuo at 60°C for 12 h to obtain Ni-Ni HCP / ZIF-67-TA.

[0104] (4) Preparation of CoP / Ni2P: 10 mg Ni-Ni HCP / ZIF-67-TA and 100 mg sodium hypophosphite (NaH2PO2·H2O) were placed at both ends of a porcelain boat, respectively. The boat was sealed with a glass sheet, and the end containing sodium hypophosphite was placed at the bottom of a quartz tube, which was then placed in a tube furnace. Finally, the system was heated to 450°C (2°C min-1 ), and calcined at 450℃ for 120min to synthesize CoP / Ni2P composite materials.

[0105] Figure 1 The XRD diffraction patterns of (a) Ni-Ni HCP, Ni-Ni HCP / ZIF-67 and Ni-Ni HCP / ZIF-67-TA obtained in Example 1 of the present invention are presented; (b) XRD diffraction pattern of CoP / Ni2P composite structure. The physical structure of the precursor is analyzed by XRD. As shown in Figure a, XRD diffraction patterns of precursors such as Ni-Ni HCP, Ni-Ni HCP / ZIF-67 and Ni-Ni HCP / ZIF-67-TA are shown. It can be seen from the figure that the positions of the diffraction peaks corresponding to the (121), (112), (200), (013), (240) and (242) crystal planes of Ni-Ni HCP are in good agreement with the diffraction peaks of Ni(H2O)2[Ni(CN)4]·H2O. For Ni-Ni HCP / ZIF-67, the diffraction peaks of Ni-Ni HCP and ZIF-67 can be found, which proves that ZIF-67 is successfully loaded on Ni-Ni HCP. The diffraction peak of Ni-Ni HCP is weakened, which may be due to the surface ZIF-67 covering the diffraction peak of Ni-Ni HCP. Ni-Ni HCP / ZIF-67 is etched with tannic acid solution to etch ZIF-67 into a hollow structure to obtain Ni-Ni HCP / ZIF-67-TA. For Ni-Ni HCP / ZIF-67-TA, although the diffraction peaks of Ni-Ni HCP and ZIF-67 are weakened, the peak position is clearly present and similar to that of Ni-Ni HCP / ZIF-67. This shows that ZIF-67 has been successfully etched and Ni-Ni HCP / ZIF-67 has been converted into Ni-Ni HCP / ZIF-67-TA. After tannic acid etching, the diffraction peak position of Ni-Ni HCP was exposed again, and its peak intensity increased significantly. For the final sample CoP / Ni2P after phosphating at 450℃, its XRD is shown in Figure b. Compared with the standard cards of CoP (JCPDS No. 29-0497) and Ni2P (JCPDS No. 03-0953), its diffraction peaks at 2θ = 31.6°, 36.3°, 48.1°, and 56.7° are consistent with the (011), (111), (211), and (301) crystal planes of CoP, and the diffraction peaks at 2θ = 40.7°, 44.6°, 47.3°, and 54.1° are consistent with the (111), (201), (210), and (300) crystal planes of Ni2P, proving that Ni-NiHCP / ZIF-67-TA was successfully phosphated and CoP / Ni2P composite materials were successfully prepared.

[0106] Figure 2 The (ab) TEM images of CoP / Ni2P obtained in Example 1 of the present invention are presented; (ce) HRTEM image; (f) element mapping image; (g) energy dispersive X-ray spectrum image. Ni-Ni HCP / ZIF-67-TA was phosphated at 450°C to obtain the final sample CoP / Ni2P. It was deeply analyzed using TEM and HRTEM. As shown in Figure a, the morphological characteristics of CoP / Ni2P are that Ni2P nanoplates are used as carriers, and hollow three-dimensional structure CoP is loaded thereon, and its edge portion is wrapped by a layer of hollow three-dimensional structure. For ease of observation, the connection between the nanoplate and the hollow structure is enlarged as the observation point to obtain Figure b, and it can be observed that the outer hollow structure is composed of many small nanoparticles. Such a structure is conducive to the penetration and diffusion of electrolytes, improves the nitrogen adsorption efficiency, and improves the performance of electrocatalytic synthesis of ammonia. Figure b is further enlarged to obtain Figure c, which shows clear lattice fringes (Figure de), where the lattice fringes corresponding to Figure d are spaced apart by 2.3mm. The (211) crystal plane belonging to CoP, the crystal plane spacing corresponding to Figure e is It belongs to the (111) crystal plane of Ni2P, which is consistent with the XRD results, verifying the successful preparation of the catalyst CoP / Ni2P. In order to further understand the element distribution of CoP / Ni2P, a series of tests such as element mapping and EDX were performed. The element mapping diagram is shown in Figure f. The red area represents Co, the yellow area represents Ni, and the green area represents P. It can be found that Ni, Co, and P in CoP / Ni2P are evenly distributed. Figure g calibrates the mass percentage of each element in CoP / Ni2P. Ni:Co:P is 43.8:21.6:34.5, and the atomic ratio is consistent with CoP / Ni2P.

[0107] Figure 3 The following are the UV-visible absorption spectra of (a) standard solutions of different NH3 concentrations obtained in Example 1 of the present invention; (b) ammonia standard curve; (c) UV-visible absorption spectra of standard solutions of different N2H4 concentrations; (d) N2H4 calibration curve. In order to study the electrocatalytic synthesis of ammonia performance of CoP / Ni2P under nitrogen, an H-type electrolyzer was used to electrochemically test the CoP / Ni2P material in a 0.1M Na2SO4 solution. In order to calculate the ammonia yield, an ammonia standard solution was first prepared using ammonium chloride and 0.1M Na2SO4, and the indole blue method was used. After adding the developer, the solution was allowed to stand for 2 hours, and its absorbance was tested at a wavelength of 655nm to obtain an ammonia standard curve. As shown in Figure a, it is the UV-visible absorption spectra of ammonia standard solutions of different concentrations. As the ammonia concentration increases, the absorbance value of the solution increases. The concentration and absorbance of the ammonia standard solution were linearly fitted. The results are shown in Figure b. The concentration and absorbance of the ammonia standard solution have a good linear fitting relationship (y = 0.4734x + 0.02651, R2 =0.999). In order to detect whether hydrazine is produced as a byproduct during the electrochemical test, similar to the ammonia standard curve, a series of hydrazine standard solutions are prepared with hydrazine sulfate (N2H4·H2SO4) and 0.1MNa2SO4. The hydrazine series standard solutions are reacted with a color developer using the Watt and Chrisp spectrophotometry method, and the absorbance is tested at 455nm to obtain a hydrazine standard curve. As shown in Figure c, the UV-visible absorption spectra of hydrazine standard solutions with different concentration gradients obtained after staining with a color developer show that the absorbance value increases with increasing concentration. A hydrazine standard curve with a good linear relationship (y=1.0983x+0.02867, R 2 =0.998), as shown in Figure d.

[0108] Figure 4 The following are the CoP / Ni2P obtained in Example 1 of the present invention: (a) linear sweep voltammetric curves in 0.10M Na2SO4 electrolyte saturated with Ar and N2, respectively; (b) it curves after electrolysis for 2 h at different potentials; (c) UV-Vis absorption spectra after electrolysis for 2 h at different potentials; (d) V after electrochemical reaction at different potentials NH3and FEs. Before the NRR test, in order to determine the effective activity window of the catalyst, an LSV test was performed first. In a 0.1M Na2SO4 electrolyte, the working electrode loaded with CoP / Ni2P was subjected to LSV tests in N2-saturated and Ar-saturated atmospheres, respectively. As shown in Figure a, its LSV current density in a N2-saturated atmosphere is larger than that of Ar, which preliminarily reflects the NRR activity of the catalyst. As the voltage increases, the polarization curves of N2 and Ar gradually overlap, thereby determining that the appropriate potential for electrocatalytic synthesis of ammonia is -0.1 to -0.5V vs.RHE. In order to further explore the NRR performance of the catalyst CoP / Ni2P, electrochemical tests at different potentials (-0.1, -0.2, -0.3, -0.4, -0.5V vs.RHE) were carried out in a N2-saturated 0.1M Na2SO4 electrolyte, and the test time at each potential was 2 hours. As can be seen from Figure b, during the 2-hour constant potential electrolysis process, the current density curve did not fluctuate significantly and remained stable at all potentials, which shows that the catalyst CoP / Ni2P has excellent stability. The electrolyte after different constant potential electrolysis was subjected to the indoxyl blue method, and the corresponding color developer was added. It was left to stand for 2 hours under natural conditions away from light, and then its absorbance was measured using a UV spectrophotometer to calculate the ammonia yield. As shown in Figure c, it is the UV-visible absorption spectrum of the electrolyte after catalyst electrolysis. At -0.3 V vs. RHE, the absorbance reached the maximum value, indicating that the ammonia yield was the highest at this potential. The ammonia standard curve was then used to convert the absorbance into ammonia yield. As shown in Figure d, it can be found that at -0.3 V vs. RHE, the ammonia yield was the highest, reaching 9.8 μg h -1 mg -1 cat , and further calculations were performed to obtain the Faraday efficiency. It can be seen that at -0.3V vs. RHE, the Faraday efficiency is the highest, reaching 9.5%. From the figure, it can be found that after -0.3V vs. RHE, the voltage increases, and the Faraday efficiency and ammonia yield of CoP / Ni2P decrease instead. This is because, as the voltage increases, NRR no longer dominates, and the hydrogen evolution reaction (HER) gradually increases, which further verifies the LSV test results.

[0109] Figure 5The results of Example 1 of the present invention are presented as follows: (a) the current density curve of CoP / Ni2P after 12 hours of reaction at -0.30V vs.RHE potential; (b) the cycle stability test of CoP / Ni2P at -0.30V vs.RHE potential; (c) the NH3 yield and FEs of CoP / Ni2P after alternating cycles of N2-saturated and Ar-saturated electrolytes for 2 hours at -0.30V vs.RHE potential; (d) the ammonia yield of CoP / Ni2P after 2 hours of electrolysis in N2-saturated and Ar-saturated Na2SO4 electrolytes at -0.30V vs.RHE voltage, and the ammonia yield at open circuit voltage in N2-saturated Na2SO4 electrolytes. The durability and stability of the catalyst are also important factors for evaluating the performance of the catalyst. To further verify the good stability of the catalyst, CoP / Ni2P was subjected to a 12-hour NRR test under 0.1M Na2SO4 electrolyte N2 conditions at a potential of -0.3V vs. RHE, and the current density curve that changes with time at the corresponding potential was obtained as shown in Figure a. It can be seen from the figure that the current density is relatively stable during the 12-hour electrochemical test, which indicates that CoP / Ni2P has good nitrogen reduction stability and durability during long-term electrochemical testing. As shown in Figure b, the catalyst CoP / Ni2P has remained almost unchanged after 6 NRR cycle tests with NH3 yield and FE. This further shows that the catalyst CoP / Ni2P has good NRR catalytic activity and can still maintain the initial ammonia yield and Faraday efficiency after a long period of testing. In order to further determine that the NRR process is the only way to generate NH3, a series of control experiments are required. First, the working electrode loaded with CoP / Ni2P is alternately inserted into the N2-saturated and Ar-saturated 0.1MNa2SO4 electrolytes, and the ammonia yield and Faraday efficiency of the catalyst at a potential of -0.3V vs.RHE are tested, and Figure c is obtained. As can be seen from the figure, there is considerable ammonia yield and Faraday efficiency in the N2-saturated atmosphere, but there is almost no ammonia yield and Faraday efficiency in the Ar atmosphere. Secondly, the ammonia yield and Faraday efficiency of CoP / Ni2P electrolysis for 2h are obtained in the N2-saturated electrolyte, the Ar-saturated electrolyte, and the open circuit voltage, respectively. As shown in Figure d, it can be intuitively seen that a certain amount of ammonia is produced in the nitrogen-saturated electrolyte, while no ammonia is produced in the argon-saturated atmosphere and the open circuit voltage. This further illustrates that the ammonia produced comes from the process of electrocatalytic nitrogen reduction, rather than from external environmental pollution.

[0110] In summary, Example 1 of the present invention synthesized a catalyst CoP / Ni2P composite material for electrocatalytic nitrogen reduction by a simple method. This composite material is composed of a two-dimensional nanoplate Ni2P and a hollow structure CoP loaded thereon. The two-dimensional nanoplate Ni2P has a large specific surface area, provides more adsorption active sites, and supports CoP. The hollow structure CoP gives the catalyst a larger specific surface area, which is beneficial to the penetration of the electrolyte and the adsorption and storage of nitrogen, thereby improving the electrocatalytic nitrogen reduction activity. The synergistic effect between Ni2P and CoP jointly regulates the electron transfer of the catalyst. It is precisely because of the large specific surface area of ​​the two-dimensional material, the hollow structure of CoP, and the synergy between the two that the CoP / Ni2P catalyst can achieve an ammonia yield of 9.8 μg h at a potential of -0.3Vvs.RHE. -1 mg -1 cat, the Faraday efficiency reaches 9.5%. This provides a new approach for the electrocatalytic nitrogen reduction reaction (NRR) technology to synthesize ammonia (NH3).

[0111] Example 2

[0112] (1) Preparation of Ni-Ni HCP: 0.46 g of nickel acetate tetrahydrate, 0.75 g of trisodium citrate dihydrate, and 3.2 g of polyvinyl pyrrolidone K-30 (Mw=30000) were dissolved in 20 mL of deionized water to form solution A, and 0.36 g of potassium tetracyanonitric acid was dissolved in 20 mL of deionized water to form solution B. Under stirring, solution B was added to solution A within 5 seconds. After continuous stirring for 1 min, the mixed solution was aged at room temperature for 24 h, and the precipitate was collected by centrifugation, washed with water and ethanol, and dried at 70°C overnight to obtain Ni-Ni HCP nanoplates (Ni-Ni Hofmann-type coordination polymer nanoplates).

[0113] (2) Preparation of Ni-Ni HCP / ZIF-67: 70 mg of Ni-Ni HCP was dissolved in 25 mL of methanol, 0.5 g of polyvinyl pyrrolidone (PVP) was added, and the mixture was vigorously stirred to form a uniform solution. The solution was allowed to stand for 10 min to obtain dispersion A'.

[0114] 0.4 g Co(NO3)2·6H2O and 5.92 g dimethylimidazole (2-MeIm) were dispersed in 25 mL methanol and 50 mL methanol to obtain solutions B' and C'. Solutions B' and C' were added to the uniform solution A' at the same time, stirred for 2 h, and the product was collected by centrifugation, washed with methanol by centrifugation for 3 times, and dried in an oven at 60 ° C to obtain Ni-Ni HCP / ZIF-67 composite.

[0115] (3) Preparation of Ni-Ni HCP / ZIF-67-TA (Ni-Ni HCP / ZIF-67 etched by tannic acid TA): 135 mg Ni-Ni HCP / ZIF-67 was added with 5 mL deionized water and dispersed evenly by ultrasonication to form solution A. 6 mL tannic acid solution (24 mmol / L) was taken with a pipette and the pH of the solution was adjusted with potassium hydroxide solution (4.8 mol / L) until the pH reached 8, forming solution B.

[0116] Solution B" was added dropwise into solution A" using a syringe, and magnetic stirring was continued for 10 min. The product was collected by centrifugation, washed twice with water and then twice with ethanol, and dried in vacuo at 60°C for 12 h to obtain Ni-Ni HCP / ZIF-67-TA.

[0117] (4) Preparation of CoP / Ni2P: 10 mg Ni-Ni HCP / ZIF-67-TA and 100 mg sodium hypophosphite (NaH2PO2·H2O) were placed at both ends of a porcelain boat, respectively. The boat was sealed with a glass sheet, and the end containing sodium hypophosphite was placed at the bottom of a quartz tube, which was then placed in a tube furnace. Finally, the system was heated to 400 °C (1.5 °C min -1 ), and continuously calcined at 400℃ for 100min to synthesize CoP / Ni2P composite materials.

[0118] Example 3

[0119] (1) Preparation of Ni-Ni HCP: 0.56 g of nickel acetate tetrahydrate, 0.85 g of trisodium citrate dihydrate, and 4.2 g of polyvinyl pyrrolidone K-30 (Mw=25000) were dissolved in 50 mL of deionized water to form solution A, and 0.56 g of potassium tetracyanonitric acid was dissolved in 20 mL of deionized water to form solution B. Under stirring, solution B was added to solution A within 5 seconds. After continuous stirring for 1 min, the mixed solution was aged at room temperature for 24 h, and the precipitate was collected by centrifugation, washed with water and ethanol, and dried at 75°C overnight to obtain Ni-Ni HCP nanoplates (Ni-Ni Hofmann-type coordination polymer nanoplates).

[0120] (2) Preparation of Ni-Ni HCP / ZIF-67: 65 mg of Ni-Ni HCP was dissolved in 25 mL of methanol, and 0.6 g of polyvinyl pyrrolidone (PVP) was added and vigorously stirred to form a uniform solution. The solution was allowed to stand for 10 min to obtain dispersion A'.

[0121] 0.5 g Co(NO3)2·6H2O and 4.83 g dimethylimidazole (2-MeIm) were dispersed in 25 mL methanol and 50 mL methanol to obtain solutions B' and C'. Solutions B' and C' were added to the uniform solution A' at the same time, stirred for 2 h, and the product was collected by centrifugation, washed with methanol by centrifugation for 3 times, and dried in an oven at 60 ° C to obtain Ni-Ni HCP / ZIF-67 composite.

[0122] (3) Preparation of Ni-Ni HCP / ZIF-67-TA (Ni-Ni HCP / ZIF-67 etched by tannic acid TA): 140 mg Ni-Ni HCP / ZIF-67 was added with 10 mL deionized water and dispersed evenly by ultrasonication to form solution A. 8 mL tannic acid solution (24 mmol / L) was taken with a pipette and the pH of the solution was adjusted with potassium hydroxide solution (4.8 mol / L) until the pH reached 8, forming solution B.

[0123] Solution B" was added dropwise into solution A" using a syringe, and magnetic stirring was continued for 10 min. The product was collected by centrifugation, washed twice with water and then twice with ethanol, and dried in a vacuum at 65°C for 24 h to obtain Ni-Ni HCP / ZIF-67-TA.

[0124] (4) Preparation of CoP / Ni2P: 15 mg Ni-Ni HCP / ZIF-67-TA and 100 mg sodium hypophosphite (NaH2PO2·H2O) were placed at both ends of a porcelain boat, respectively. The boat was sealed with a glass sheet, and the end containing sodium hypophosphite was placed at the bottom of a quartz tube, which was then placed in a tube furnace. Finally, the system was heated to 450°C (2°C min -1 ), and calcined at 450℃ for 100min to synthesize CoP / Ni2P composite materials.

[0125] Example 4

[0126] (1) Preparation of Ni-Ni HCP: 0.36 g of nickel acetate tetrahydrate, 0.65 g of trisodium citrate dihydrate, and 4.8 g of polyvinyl pyrrolidone K-30 (Mw=35000) were dissolved in 20 mL of deionized water to form solution A, and 0.36 g of potassium tetracyanonitric acid was dissolved in 20 mL of deionized water to form solution B. Under stirring, solution B was added to solution A within 5 seconds. After continuous stirring for 1 min, the mixed solution was aged at room temperature for 24 h, and the precipitate was collected by centrifugation, washed with water and ethanol, and dried at 75°C overnight to obtain Ni-Ni HCP nanoplates (Ni-Ni Hofmann-type coordination polymer nanoplates).

[0127] (2) Preparation of Ni-Ni HCP / ZIF-67: 80 mg of Ni-Ni HCP was dissolved in 25 mL of methanol, and 0.8 g of polyvinyl pyrrolidone (PVP) was added and vigorously stirred to form a uniform solution. The solution was allowed to stand for 10 min to obtain dispersion A'.

[0128] 0.5 g Co(NO3)2·6H2O and 6.12 g dimethylimidazole (2-MeIm) were dispersed in 25 mL methanol and 50 mL methanol to obtain solutions B' and C'. Solutions B' and C' were added to the uniform solution A' at the same time, stirred for 2 h, and the product was collected by centrifugation, washed with methanol by centrifugation for 3 times, and dried in an oven at 60 ° C to obtain Ni-Ni HCP / ZIF-67 composite.

[0129] (3) Preparation of Ni-Ni HCP / ZIF-67-TA (Ni-Ni HCP / ZIF-67 etched by tannic acid TA): 135 mg Ni-Ni HCP / ZIF-67 was added with 5 mL deionized water and dispersed evenly by ultrasonication to form solution A. 6 mL tannic acid solution (24 mmol / L) was taken with a pipette and the pH of the solution was adjusted with potassium hydroxide solution (4.8 mol / L) until the pH reached 8, forming solution B.

[0130] Solution B" was added dropwise into solution A" using a syringe, and magnetic stirring was continued for 10 min. The product was collected by centrifugation, washed twice with water and then twice with ethanol, and dried in vacuo at 60°C for 36 h to obtain Ni-Ni HCP / ZIF-67-TA.

[0131] (4) Preparation of CoP / Ni2P: 12 mg Ni-Ni HCP / ZIF-67-TA and 120 mg sodium hypophosphite (NaH2PO2·H2O) were placed at both ends of a porcelain boat, respectively. The boat was sealed with a glass sheet, and the end containing sodium hypophosphite was placed at the bottom of a quartz tube, which was then placed in a tube furnace. Finally, the system was heated to 350°C (1.0°C min -1 ), and calcined at 350℃ for 120min to synthesize CoP / Ni2P composite materials.

[0132] Example 5

[0133] (1) Preparation of Ni-Ni HCP: 0.65 g of nickel acetate tetrahydrate, 0.95 g of trisodium citrate dihydrate, and 3.2 g of polyvinyl pyrrolidone K-30 (Mw=40000) were dissolved in 20 mL of deionized water to form solution A, and 0.56 g of potassium tetracyanonitric acid was dissolved in 20 mL of deionized water to form solution B. Under stirring, solution B was added to solution A within 5 seconds. After continuous stirring for 1 min, the mixed solution was aged at room temperature for 24 h, and the precipitate was collected by centrifugation, washed with water and ethanol, and dried at 90°C overnight to obtain Ni-Ni HCP nanoplates (Ni-Ni Hofmann-type coordination polymer nanoplates).

[0134] (2) Preparation of Ni-Ni HCP / ZIF-67: 80 mg of Ni-Ni HCP was dissolved in 25 mL of methanol, 0.3 g of polyvinyl pyrrolidone (PVP) was added, and the mixture was vigorously stirred to form a uniform solution. The solution was allowed to stand for 10 min to obtain dispersion A'.

[0135] 0.3g Co(NO3)2·6H2O and 5.5g dimethylimidazole (2-MeIm) were dispersed in 25mL methanol and 50mL methanol to obtain solutions B' and C'. Solutions B' and C' were added to the uniform solution A' at the same time, stirred for 2h, and the product was collected by centrifugation, washed with methanol by centrifugation for 3 times, and dried in an oven at 60℃ to obtain Ni-Ni HCP / ZIF-67 composite.

[0136] (3) Preparation of Ni-Ni HCP / ZIF-67-TA (Ni-Ni HCP / ZIF-67 etched by tannic acid TA): 135 mg Ni-Ni HCP / ZIF-67 was added with 5 mL deionized water and dispersed evenly by ultrasonication to form solution A. 10 mL tannic acid solution (24 mmol / L) was taken with a pipette and the pH of the solution was adjusted with potassium hydroxide solution (4.8 mol / L) until the pH reached 8, forming solution B.

[0137] Solution B" was added dropwise into solution A" using a syringe, and magnetic stirring was continued for 10 min. The product was collected by centrifugation, washed twice with water and then twice with ethanol, and dried in vacuo at 50°C for 48 h to obtain Ni-Ni HCP / ZIF-67-TA.

[0138] (4) Preparation of CoP / Ni2P: 10 mg Ni-Ni HCP / ZIF-67-TA and 100 mg sodium hypophosphite (NaH2PO2·H2O) were placed at the two ends of a porcelain boat, respectively. The boat was sealed with a glass sheet, and the end containing sodium hypophosphite was placed at the bottom of a quartz tube, which was then placed in a tube furnace. Finally, the system was heated to 300 °C (1.5 °C min -1), and calcined at 300℃ for 150min to synthesize CoP / Ni2P composite materials.

[0139] Example 6

[0140] (1) Preparation of Ni-Ni HCP: 0.36 g of nickel acetate tetrahydrate, 0.65 g of trisodium citrate dihydrate, and 4.5 g of polyvinyl pyrrolidone K-30 (Mw=45000) were dissolved in 20 mL of deionized water to form solution A, and 0.48 g of potassium tetracyanonitric acid was dissolved in 20 mL of deionized water to form solution B. Under stirring, solution B was added to solution A within 5 seconds. After continuous stirring for 1 min, the mixed solution was aged at room temperature for 24 h, and the precipitate was collected by centrifugation, washed with water and ethanol, and dried at 60°C overnight to obtain Ni-Ni HCP nanoplates (Ni-Ni Hofmann-type coordination polymer nanoplates).

[0141] (2) Preparation of Ni-Ni HCP / ZIF-67: 60 mg of Ni-Ni HCP was dissolved in 25 mL of methanol, and 0.6 g of polyvinyl pyrrolidone (PVP) was added and vigorously stirred to form a uniform solution. The solution was allowed to stand for 10 min to obtain dispersion A'.

[0142] 0.5 g Co(NO3)2·6H2O and 6.85 g dimethylimidazole (2-MeIm) were dispersed in 25 mL methanol and 50 mL methanol to obtain solutions B' and C'. Solutions B' and C' were added to the uniform solution A' at the same time, stirred for 2 h, and the product was collected by centrifugation, washed with methanol by centrifugation for 3 times, and dried in an oven at 75 ° C to obtain Ni-Ni HCP / ZIF-67 composite.

[0143] (3) Preparation of Ni-Ni HCP / ZIF-67-TA (Ni-Ni HCP / ZIF-67 etched by tannic acid TA): 135 mg Ni-Ni HCP / ZIF-67 was added with 5 mL deionized water and dispersed evenly by ultrasonication to form solution A. 10 mL tannic acid solution (24 mmol / L) was taken with a pipette and the pH of the solution was adjusted with potassium hydroxide solution (5.6 mol / L) until the pH reached 8, forming solution B.

[0144] Solution B" was added dropwise into solution A" using a syringe, and magnetic stirring was continued for 10 min. The product was collected by centrifugation, washed twice with water and three times with methanol, and dried in vacuo at 60°C for 24 h to obtain Ni-Ni HCP / ZIF-67-TA.

[0145] (4) Preparation of CoP / Ni2P: 15 mg Ni-Ni HCP / ZIF-67-TA and 150 mg sodium hypophosphite (NaH2PO2·H2O) were placed at both ends of a porcelain boat, respectively. The boat was sealed with a glass sheet, and the end containing sodium hypophosphite was placed at the bottom of a quartz tube, which was then placed in a tube furnace. Finally, the system was heated to 400 °C (1.5 °C min -1 ), and calcined at 400 °C for 120 min to synthesize CoP / Ni2P composite materials.

[0146] The specific embodiments of the present invention are described in detail above, but they are only examples, and the present invention is not limited to the specific embodiments described above. For those skilled in the art, any equivalent modifications and substitutions made to the present invention are also within the scope of the present invention. Therefore, the equalization changes and modifications made without departing from the spirit and scope of the present invention should be included in the scope of the present invention.

Claims

1. A method for preparing a composite catalyst, comprising the steps of: include: Provide Ni-Ni HCP nanoplates; Mixing Ni-Ni HCP nanoplates, cobalt salt, and dimethylimidazole in a first solvent to obtain a Ni-Ni HCP / ZIF-67 composite; The Ni-Ni HCP / ZIF-67 composite was etched with tannic acid to obtain Ni-Ni HCP / ZIF-67-TA. The Ni-Ni HCP / ZIF-67-TA was phosphated at high temperature to obtain CoP / Ni 2 P composite material, namely CoP and Ni 2 The composite catalyst of P.

2. The preparation method according to claim 1, It is characterized in that The preparation method of the Ni-Ni HCP nanoplate comprises the following steps: Mixing nickel salt, citrate and potassium tetracyanonickelate in a second solvent to obtain a Ni-Ni Hofmann-type coordination polymer nanoplate, i.e., a Ni-Ni HCP nanoplate; and / or Before the nickel salt, citrate and potassium tetracyanonickelate are mixed in the second solvent, the nickel salt and citrate may be mixed in part of the second solvent to obtain solution A; and / or mixing potassium tetracyanonickelate with a portion of the second solvent to obtain a solution B; Solution B was mixed with solution A to obtain Ni-Ni HCP nanoplates.

3. The preparation method according to claim 2, It is characterized in that After the nickel salt, citrate and potassium tetracyanonickelate are mixed in the second solvent, aging is performed; and / or The aging temperature is 5-50°C, preferably 10-40°C, more preferably 20-30°C, more preferably 20-25°C; and / or The aging time is 12-40 hours, preferably 16-30 hours, and more preferably 20-24 hours.

4. The preparation method according to claim 1, It is characterized in that Before the Ni-Ni HCP nanoplates, cobalt salt and dimethylimidazole are mixed in the first solvent, the Ni-Ni HCP nanoplates can be dispersed in the first solvent to obtain a first solution; preferably, The Ni-Ni HCP nanoplate and the second dispersant may be mixed in a first solvent to obtain a first solution; Mixing cobalt salt and dimethylimidazole in a first solvent to obtain a second solution; The second solution is added to the first solution and mixed to obtain a Ni-Ni HCP / ZIF-67 composite; preferably, Mixing a cobalt salt in a first solvent to obtain a cobalt salt solution, and mixing dimethylimidazole in the first solvent to obtain a dimethylimidazole solution; The cobalt salt solution and the dimethylimidazole solution are added to the first solution at the same time and mixed to obtain a Ni-Ni HCP / ZIF-67 composite.

5. The preparation method according to claim 1, It is characterized in that The tannic acid etches the Ni-Ni HCP / ZIF-67 complex, and the steps include: dispersing the Ni-Ni HCP / ZIF-67 complex in a third solvent to obtain a third solution; providing a solution of tannic acid dispersed in a third solvent, i.e., a tannic acid solution; adding alkali to the tannic acid solution and adjusting the pH value to a preset value to obtain a fourth solution; adding the fourth solution to the third solution to obtain Ni-Ni HCP / ZIF-67-TA; and / or The concentration of the tannic acid solution is 10-50 mmol / L, preferably 15-40 mmol / L, more preferably 24-30 mmol / L; and / or The OH of the base - The concentration is 1-10 mol / L, preferably 2-8 mol / L, more preferably 4-6 mol / L; and / or The preset pH value is 7-14, preferably 8-12, more preferably 8-10; preferably, The fourth solution is added to the third solution in a dropwise manner.

6. The preparation method according to claim 1, It is characterized in that The high temperature phosphating step comprises: calcining Ni-NiHCP / ZIF-67-TA and phosphate in a closed environment to obtain CoP and Ni 2 The composite catalyst of P.

7. The preparation method according to claim 6, It is characterized in that The phosphate is selected from one or more combinations of phosphates, phosphites, and hypophosphites; Specifically, the phosphate is preferably selected from one or more combinations of trisodium phosphate, tripotassium phosphate, potassium dihydrogen phosphate, sodium dihydrogen phosphate, dipotassium hydrogen phosphate, disodium hydrogen phosphate, sodium hypophosphite, potassium hypophosphite, sodium phosphite, and potassium phosphite.

8. The preparation method according to claim 6, It is characterized in that The calcination temperature is 300-600°C, preferably 400-500°C, more preferably 450-480°C; and / or The calcination time is 60-300 min, preferably 100-200 min, more preferably 120-150 min; and / or The heating rate of the calcination is 1-5°C / min, preferably 1.5-3°C / min, more preferably 2-2.5°C / min.

9. A composite catalyst, It is characterized in that Obtained based on the preparation method according to any one of claims 1 to 8.

10. Use of the composite catalyst according to claim 9, It is characterized in that The composite catalyst can be applied to synthesizing ammonia by electrocatalysis.