Preparation method of self-supporting graded Ni5P4 / Co3O4 / NF heterostructure electrode material

By forming Ni5P4/Co3O4/NF heterostructure electrode material on nickel foam, the problems of low catalyst activity and electrode material stability in alkaline media are solved, and efficient catalytic performance and stability are achieved, which is suitable for alkaline hydrogen evolution reaction.

CN119082782APending Publication Date: 2024-12-06HUBEI UNIV OF AUTOMOTIVE TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411192655.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In alkaline media, existing catalysts have low activity during hydrolysis and Hads desorption, resulting in low alkaline hydrogen evolution reaction efficiency, and the mechanical strength of the electrode material is related to service life, affecting the catalytic reaction.

Method used

By loading Co(OH)2 on nickel foam, calcining obtains Co3O4/NF composite electrode material, then hydrothermal reaction is carried out in situ Ni(OH)2 nanosheets, and phosphating to form Ni5P4/Co3O4/NF heterostructure electrode material. Optimize catalytic performance.

Benefits of technology

It achieves efficient catalytic performance and stability in alkaline media, the reaction starting potential is close to 0V, the Tafel slope is low, the current density is high, and the operation is stable under high current density, which extends the service life of the electrode.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082782A_ABST
    Figure CN119082782A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a self-supporting graded Ni5P4 / Co3O4 / NF heterostructure electrode material, which comprises the following steps: loading Co (OH) 2 on foamed nickel, calcining to obtain a Co3O4 / NF composite electrode material, loading an ultrathin Ni (OH) 2 nanosheet on the surface of a Co3O4 nanowire in situ through a hydrothermal reaction, and finally phosphorizing to obtain the Ni5P4 / Co3O4 / NF heterostructure electrode material. The process of the preparation method is easy to control, the structure of the prepared heterostructure electrode material is that a nanorod array formed by combining ultrathin Ni5P4 nanosheets and Co3O4 nanowires is integrated on a foamed nickel current collector, and the electrode material shows excellent catalytic performance and also has good rapid reaction kinetics and stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of hydrogen evolution electrocatalytic materials and relates to a method for preparing a self-supporting graded Ni5P4 / Co3O4 / NF heterostructure electrode material. Background Art

[0002] Using clean renewable electricity to drive water splitting to produce hydrogen has the advantages of abundant raw materials, controllable reaction, no carbon emissions, and high product purity. It is the most promising way to produce "green hydrogen" on a large scale. Due to the strong corrosion resistance of acidic media to catalysts and reaction equipment, the cost of hydrogen production is greatly increased. Therefore, the alkaline hydrogen evolution reaction has attracted widespread attention from researchers in recent years. However, the alkaline hydrogen evolution reaction involves an additional water dissociation process (Volmer step: H2O+e - →H ads +OH - ), which requires a large overpotential for rapid HER to occur. Therefore, even the most advanced platinum catalysts have a catalytic activity 2 to 3 orders of magnitude lower in alkaline media than in acidic media. In addition, H ads The desorption of the intermediates to generate H2 determines the kinetics of the entire HER process. Therefore, it is necessary to rationally design advanced electrocatalysts based on cheap transition metals to promote water dissociation and H2 generation. ads Desorption is the key to alkaline water electrolysis reaction.

[0003] At present, various transition metal compounds have been reported in an attempt to improve their intrinsic catalytic activity, including metal hydroxides, oxides, nitrides, sulfides, phosphides, etc. Among them, transition metal phosphides (M x P y ) are considered to be a promising new generation of HER catalysts due to their adjustable electronic structure, diverse composition and good electronic conductivity. Unfortunately, their intrinsic activity is still far behind that of Pt-based catalysts. Constructing a heterogeneous interface can enable directional electron transfer between the two components, thereby regulating the electronic structure of the catalytic active sites, which is an effective way to improve catalytic performance. For example, Jiao Lifang et al. prepared a multi-heterostructured Mo-doped Ni2P / Fe on NiFe foam. x P electrocatalysts enhance the water dissociation and *OH desorption capabilities of active sites through multiple strategies such as heteroatom doping, heterogeneous interfaces, and P vacancies. Although this strategy can effectively regulate the d-band center of the active site and improve the intrinsic activity of the catalyst, the number of intrinsic active sites is small. On the other hand, since the adsorption and desorption of intermediates involved in the catalytic reaction occur at the solid-liquid interface between the catalyst and the electrolyte, the mass transfer capacity of the electrode and the escape rate of the product gas seriously affect the occurrence of the catalytic reaction, and the mechanical strength of the electrode is closely related to its service life.

[0004] Therefore, reasonable electrode materials are an important factor to be considered in catalyst design. Based on the above background, the present invention is committed to developing and preparing cheap, efficient and stable alkaline hydrogen evolution reaction electrocatalysts. Summary of the invention

[0005] In view of the above technical problems, the present invention aims to provide a method for preparing a self-supporting graded Ni5P4 / Co3O4 / NF heterostructure electrode material, by loading Co(OH)2 on nickel foam and obtaining a Co3O4 / NF composite electrode material through calcination, then in-situ loading ultrathin Ni(OH)2 nanosheets on the surface of Co3O4 nanowires through a hydrothermal reaction, and then obtaining a Ni5P4 / Co3O4 / NF heterostructure electrode material through phosphating; the heterostructure electrode material exhibits excellent catalytic performance, good rapid reaction kinetics and stability.

[0006] To achieve the above object, the technical solution adopted by the present invention is:

[0007] A method for preparing a self-supporting hierarchical Ni5P4 / Co3O4 / NF heterostructure electrode material is carried out in the following steps in sequence:

[0008] a. Preparation of Co(OH)2 / NF composite electrode material: ultrasonically clean nickel foam with acetone, ethanol, hydrochloric acid and water in sequence to remove stains and oxides on the surface, dissolve Co(NO3)2·6H2O, NH4F and CO(NH2)2 in deionized water, stir thoroughly and transfer them to a reactor together with the clean nickel foam, react at 100-150°C for 3-9h, cool to room temperature and wash the electrode with ethanol and deionized water several times to remove residual solution, then vacuum dry at 60°C overnight to obtain Co(OH)2 / NF composite electrode material;

[0009] b. Preparation of Co3O4 / NF composite electrode material: calcining the Co(OH)2 / NF composite electrode material in air to obtain the Co3O4 / NF composite electrode material;

[0010] c. Preparation of Ni(OH)2 / Co3O4 / NF heterostructure electrode material: Dissolve Ni(NO3)2·6H2O, NH4F and CO(NH2)2 in deionized water, transfer to a reactor after sufficient stirring, immerse the prepared Co3O4 / NF composite electrode therein, react at 100-150°C for 3-9h, cool to room temperature, wash the electrode with ethanol and deionized water several times to remove the residual solution, and then vacuum dry at 60°C overnight to obtain Ni(OH)2 / Co3O4 / NF heterostructure electrode material;

[0011] d. Preparation of Ni5P4 / Co3O4 / NF heterostructure electrode material: NaPO2H2 was placed upstream of the gas flow of the tube furnace, and the prepared Ni(OH)2 / Co3O4 / NF heterostructure electrode material was placed downstream of the tube furnace, and annealed in Ar atmosphere to obtain Ni5P4 / Co3O4 / NF heterostructure electrode material.

[0012] As a limitation of the preparation method of the present invention, in step a, the mass ratio of Co(NO3)2·6H2O, NH4F and CO(NH2)2 is (100-200):42:171.

[0013] In this step, the mass ratio of the three raw materials will affect the size of the Co(OH)2 nanowires. CO(NH2)2 will be hydrolyzed in the reactor to generate ammonia water, which will then react with Co(NO3)2·6H2O to generate Co(OH)2. The role of NH4F is mainly to regulate the morphology of the product, thereby forming Co(OH)2 nanowires.

[0014] As another limitation of the preparation method of the present invention, in step b, the calcination temperature is 200-400° C. and the time is 1-3 hours.

[0015] As a third limitation of the preparation method of the present invention, in step c, the molar ratio of Ni(NO3)2·6H2O, NH4F and CO(NH2)2 is (3-6):32:47.5.

[0016] In this step, the molar ratio of the three substances will affect the size of Ni(OH)2 nanosheets. CO(NH2)2 will be hydrolyzed in the reactor to generate ammonia water, which will then react with Ni(NO3)2·6H2O to generate Ni(OH)2. The role of NH4F is mainly to regulate the morphology of the product, thereby forming Ni(OH)2 nanosheets.

[0017] As the fourth limitation of the preparation method of the present invention, in step d, the mass ratio of NaPO2H2 to Ni5P4 / Co3O4 / NF is (1-3):10.

[0018] As a fifth limitation of the preparation method of the present invention, in step d, the annealing temperature is 300-400° C., and the time is 1-3 hours.

[0019] As the last limitation of the preparation method of the present invention, the structure of the Ni5P4 / Co3O4 / NF heterostructure electrode material is a nanorod array formed by combining ultrathin Ni5P4 nanosheets and Co3O4 nanowires, which is integrated on a foam nickel current collector.

[0020] The heterostructure electrode material prepared by the present invention is an ultra-thin Ni5P4 nanosheet array integrated on the surface of Co3O4 nanowires, wherein the Co3O4 nanowires are in-situ grown on nickel foam. Since the Co3O4 nanowires limit the growth of Ni(OH)2 precursors, the ultra-thin Ni(OH)2 formed is easily fully phosphated to form Ni5P4, rather than conventional Ni2P compounds. Compared with Ni2P, Ni5P4 has a higher P atomic ratio, and its strong electronegativity can absorb electrons from metal atoms, thereby resulting in a rich Ni valence state, which is beneficial to promoting the HER half-reaction in the water decomposition process.

[0021] As a further limitation of the preparation method of the present invention:

[0022] (i) In step b, the calcination heating rate is 5°C / min.

[0023] The calcination process of the present invention is crucial for the morphology formation of the Co3O4 / NF composite electrode material. In this process, Co(OH)2 is dehydrated and oxidized to form Co3O4. If the calcination temperature is too high, the electrode will become brittle, and if the calcination temperature is too low, the dehydration of Co(OH)2 will be incomplete.

[0024] (ii) In step d, the heating rate of the annealing process is 2°C / min.

[0025] The phosphating annealing process of the present invention is crucial for the final formation of Ni5P4 on Co3O4 / NF, and it affects the formation of the morphology of the Ni5P4 / Co3O4 / NF heterostructure electrode material. In this process, NaPO2H2 is decomposed by heat to generate PH3 gas, which reacts with Ni(OH)2 nanosheets on the surface of the Ni(OH)2 / Co3O4 / NF electrode to generate Ni5P4. When the annealing temperature is too high, the decomposition rate of NaPO2H2 will be too fast, and thus phosphating cannot be fully performed. When the annealing temperature is too low, the decomposition conditions of NaPO2H2 cannot be reached, and the phosphating process cannot occur.

[0026] The above technical solution of the present invention is taken as a whole, and each step is closely related and influences each other, which jointly determine the morphological characteristics and performance of the product.

[0027] The above technical solution has the following advantages or beneficial effects:

[0028] 1. The self-supported hierarchical Ni5P4 / Co3O4 / NF heterostructure electrode material prepared by the present invention has a special hierarchical structure that provides channels for electrolyte transmission and gas escape, greatly increases the specific surface area, and exposes abundant active sites.

[0029] 2. The seamlessly integrated Ni5P4 / Co3O4 heterogeneous interface effectively reduces the contact resistance and charge transfer resistance, and the stable interface structure ensures the stability of the catalyst.

[0030] 3. The charge reconstruction between Ni5P4 / Co3O4 effectively regulates the adsorption energy of active sites and optimizes the intrinsic catalytic activity of Ni5P4.

[0031] 4. The self-supported hierarchical Ni5P4 / Co3O4 / NF heterostructure electrode material prepared by the present invention exhibits excellent catalytic performance. The reaction starting potential is close to 0V, and only 190mV and 230mV overpotentials are required to achieve 500mA cm -2 and 1000mA cm -2 Current density; Tafel slope as low as 76.6mV dec -1 ; at 1000mA cm -2 There is no obvious attenuation when running for 50h under high current density.

[0032] The invention is suitable for preparing self-supporting graded Ni5P4 / Co3O4 / NF heterostructure electrode materials.

[0033] The technical solution of the present invention will be further described in detail below in conjunction with the accompanying drawings and specific implementation methods. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 LSV curves of NF, Co3O4 / NF, Ni2P / NF, and Ni5P4 / Co3O4 / NF electrode materials prepared in Comparative Examples 1, 2, 3 and Example 1 of the present invention as alkaline hydrogen evolution catalysts;

[0035] Figure 2 This is a flow chart of preparing Ni5P4 / Co3O4 / NF heterostructure electrode material in Example 1 of the present invention;

[0036] Figure 3 This is a SEM image of the Co(OH)2 / NF composite electrode material prepared in Example 1 of the present invention;

[0037] Figure 4 This is a SEM image of the Co3O4 / NF composite electrode material prepared in Example 1 of the present invention;

[0038] Figure 5 This is the XRD pattern of the Co3O4 / NF composite electrode material prepared in Example 1 of the present invention;

[0039] Figure 6 This is a SEM image of the Ni5P4 / Co3O4 / NF heterostructure electrode material prepared in Example 1 of the present invention;

[0040] Figure 7 This is the XRD pattern of the Ni5P4 / Co3O4 / NF heterostructure electrode material prepared in Example 1 of the present invention;

[0041] Figure 8 This is a SEM image of the Ni2P / NF composite electrode material prepared in Comparative Example 3 of the present invention;

[0042] Fig. 9 The XRD diagram of the Ni2P / NF composite electrode material prepared in Comparative Example 3 of the present invention;

[0043] Fig.10 The full XPS spectra of Co3O4 / NF, Ni2P / NF and Ni5P4 / Co3O4 / NF electrode materials prepared in Comparative Examples 2 and 3 and Example 1 of the present invention;

[0044] Fig.11 HRTEM image of the Ni5P4 / Co3O4 / NF heterostructure electrode material prepared in Example 1 of the present invention;

[0045] Fig.12 High-resolution Ni 2p XPS spectra of Co3O4 / NF, Ni2P / NF and Ni5P4 / Co3O4 / NF electrode materials prepared in Comparative Examples 2 and 3 and Example 1 of the present invention;

[0046] Fig.13 High-resolution Co 2p XPS spectra of Co3O4 / NF, Ni2P / NF and Ni5P4 / Co3O4 / NF electrode materials prepared in Comparative Examples 2 and 3 and Example 1 of the present invention;

[0047] Fig.14 High-resolution P 2p XPS spectra of Co3O4 / NF, Ni2P / NF and Ni5P4 / Co3O4 / NF electrode materials prepared in Comparative Examples 2 and 3 and Example 1 of the present invention;

[0048] Fig.15 High-resolution O1s XPS spectra of Co3O4 / NF, Ni2P / NF and Ni5P4 / Co3O4 / NF electrode materials prepared in Comparative Examples 2 and 3 and Example 1 of the present invention;

[0049] Fig.16 It is a comparison chart of the HER catalytic performance of NF, Co3O4 / NF, Co3O4 / NF and Ni5P4 / Co3O4 / NF electrode materials prepared in Comparative Examples 1, 2, 3 and Example 1 of the present invention;

[0050] Fig.17The Tafel slope curves of the NF, Co3O4 / NF, Co3O4 / NF and Ni5P4 / Co3O4 / NF electrode materials prepared in Comparative Examples 1, 2, 3 and Example 1 of the present invention;

[0051] Fig.18 The EIS graphs of NF, Co3O4 / NF, Co3O4 / NF and Ni5P4 / Co3O4 / NF electrode materials prepared in Comparative Examples 1, 2, 3 and Example 1 of the present invention;

[0052] Fig.19 CV curves of the NF electrode material prepared in Comparative Example 1 of the present invention at different scan rates;

[0053] Fig. 20 CV curves of the Ni2P / NF composite electrode material prepared in Comparative Example 3 of the present invention at different scan rates;

[0054] Fig.21 CV curves of the Co3O4 / NF composite electrode material prepared in Comparative Example 2 of the present invention at different scan rates;

[0055] Fig. 22 CV curves of the Ni5P4 / Co3O4 / NF heterostructure electrode material prepared in Example 1 of the present invention at different scan rates;

[0056] Fig.23 is the Cdl of the NF, Co3O4 / NF, Co3O4 / NF and Ni5P4 / Co3O4 / NF electrode materials prepared in Comparative Examples 1, 2, 3 and Example 1 of the present invention;

[0057] Fig.24 It is a comparison chart of ECSA of NF, Co3O4 / NF, Co3O4 / NF and Ni5P4 / Co3O4 / NF electrode materials prepared in Comparative Examples 1, 2, 3 and Example 1 of the present invention;

[0058] Fig.25 The specific activity polarization curves of the NF, Co3O4 / NF, Co3O4 / NF and Ni5P4 / Co3O4 / NF electrode materials prepared in Comparative Examples 1, 2, 3 and Example 1 of the present invention;

[0059] Fig.26 It is a comparison chart of the specific activities of NF, Co3O4 / NF, Co3O4 / NF and Ni5P4 / Co3O4 / NF electrode materials prepared in Comparative Examples 1, 2, 3 and Example 1 of the present invention at an overpotential of 250 mV;

[0060] Fig. 27 This is a graph showing the stability test results of the Ni5P4 / Co3O4 / NF heterostructure electrode material prepared in Example 1 of the present invention;

[0061] Fig.28 This is a comparison diagram of the LSV curves of the Ni5P4 / Co3O4 / NF heterostructure electrode material prepared in Example 1 of the present invention before and after the stability test;

[0062] Fig.29 This is a SEM image of the Ni5P4 / Co3O4 / NF heterostructure electrode material prepared in Example 1 of the present invention after stability testing;

[0063] Fig.30 This is a SEM image of the Ni5P4 / Co3O4 / NF heterostructure electrode material prepared in Example 2 of the present invention;

[0064] Fig.31 This is a SEM image of the Ni5P4 / Co3O4 / NF heterostructure electrode material prepared in Example 3 of the present invention. DETAILED DESCRIPTION

[0065] The following embodiments are only some embodiments of the present invention, rather than all embodiments. Therefore, the detailed description in the embodiments of the present invention provided below is not intended to limit the scope of the present invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without making creative work belong to the protection scope of the present invention.

[0066] In the present invention, unless otherwise specified, all equipment and raw materials can be purchased from the market or are commonly used in the industry. The methods in the following embodiments are all conventional methods in the art unless otherwise specified.

[0067] Example

[0068] Example 1

[0069] This embodiment prepares a self-supporting hierarchical Ni5P4 / Co3O4 / NF heterostructure electrode material, and the preparation process and steps are as follows:

[0070] a. Preparation of Co(OH)2 / NF composite electrode material: ultrasonically clean the nickel foam with acetone, ethanol, hydrochloric acid and water in sequence to remove stains and oxides on the surface, dissolve 1.66g Co(NO3)2·6H2O, 0.42g NH4F and 1.71g CO(NH2)2 in 60mL deionized water, stir well and transfer together with the clean nickel foam to a 100mL reactor, react at 120℃ for 6h, cool to room temperature and wash the electrode with ethanol and deionized water several times to remove residual solution, then vacuum dry at 60℃ overnight to obtain Co(OH)2 / NF composite electrode material;

[0071] b. Preparation of Co3O4 / NF composite electrode material: calcining the Co(OH)2 / NF composite electrode material at 350°C for 2h in air at a calcination heating rate of 5°C / min to obtain the Co3O4 / NF composite electrode material;

[0072] c. Preparation of Ni(OH)2 / Co3O4 / NF heterostructure electrode material: 0.45mmol Ni(NO3)2·6H2O, 3.2mmolNH4F and 4.75mmol CO(NH2)2 were dissolved in 60mL deionized water, stirred thoroughly and transferred to a 100mL reactor, and the prepared Co3O4 / NF composite electrode material was immersed therein, reacted at 120°C for 6h, cooled to room temperature, and washed the electrode with ethanol and deionized water several times to remove the residual solution, and then vacuum dried at 60°C overnight to obtain Ni(OH)2 / Co3O4 / NF heterostructure electrode material;

[0073] d. Preparation of Ni5P4 / Co3O4 / NF heterostructure electrode material: 1.5 g NaPO2H2 was placed upstream of the air flow of the tube furnace, and 10 g Ni(OH)2 / Co3O4 / NF heterostructure material electrode was placed downstream of the tube furnace. The temperature was raised from room temperature to 350°C in an Ar atmosphere at a heating rate of 2°C / min and annealed for 1 h to obtain Ni5P4 / Co3O4 / NF heterostructure electrode material.

[0074] Example 2

[0075] This embodiment prepares a self-supporting hierarchical Ni5P4 / Co3O4 / NF heterostructure electrode material, and the preparation process and steps are as follows:

[0076] a. Preparation of Co(OH)2 / NF composite electrode material: ultrasonically clean nickel foam with acetone, ethanol, hydrochloric acid and water in sequence to remove surface stains and oxides, dissolve 1.0g Co(NO3)2·6H2O, 0.42g NH4F and 1.71g CO(NH2)2 in 60mL deionized water, stir thoroughly and transfer together with the clean nickel foam to a 100mL reactor, react at 100℃ for 3h, cool to room temperature and wash the electrode with ethanol and deionized water several times to remove residual solution, then vacuum dry at 60℃ overnight to obtain Co(OH)2 / NF composite electrode material;

[0077] b. Preparation of Co3O4 / NF composite electrode material: calcining the Co(OH)2 / NF composite electrode material at 200°C in air for 1.5h at a calcination heating rate of 5°C / min to obtain the Co3O4 / NF composite electrode material;

[0078] c. Preparation of Ni(OH)2 / Co3O4 / NF heterostructure electrode material: 0.3mmol Ni(NO3)2·6H2O, 3.2mmol NH4F and 4.75mmol CO(NH2)2 were dissolved in 60mL deionized water, stirred thoroughly and transferred to a 100mL reactor, and the prepared Co3O4 / NF composite electrode material was immersed therein, reacted at 100℃ for 3h, cooled to room temperature, and washed the electrode with ethanol and deionized water several times to remove the residual solution, and then vacuum dried at 60℃ overnight to obtain Ni(OH)2 / Co3O4 / NF heterostructure electrode material;

[0079] d. Preparation of Ni5P4 / Co3O4 / NF heterostructure electrode material: 1.0 g NaPO2H2 was placed upstream of the air flow of the tube furnace, and 10 g of the prepared Ni(OH)2 / Co3O4 / NF heterostructure electrode material was placed downstream of the tube furnace. The temperature was raised from room temperature to 300°C in an Ar atmosphere at a heating rate of 2°C / min and annealed for 2 h to obtain the Ni5P4 / Co3O4 / NF heterostructure electrode material.

[0080] Example 3

[0081] This embodiment prepares a self-supporting hierarchical Ni5P4 / Co3O4 / NF heterostructure electrode material, and the preparation process and steps are as follows:

[0082] a. Preparation of Co(OH)2 / NF composite electrode material: ultrasonically clean the nickel foam with acetone, ethanol, hydrochloric acid and water in sequence to remove stains and oxides on the surface, dissolve 2.0g Co(NO3)2·6H2O, 0.42g NH4F and 1.71g CO(NH2)2 in 60ml deionized water, stir thoroughly and transfer them together with the clean nickel foam to a 100mL reactor, react at 150℃ for 9h, cool to room temperature and wash the electrode with ethanol and deionized water several times to remove residual solution, then vacuum dry at 60℃ overnight to obtain Co(OH)2 / NF composite electrode material;

[0083] b. Preparation of Co3O4 / NF composite electrode material: calcining the Co(OH)2 / NF composite electrode material at 400°C in air for 3h at a calcination heating rate of 5°C / min to obtain the Co3O4 / NF composite electrode material;

[0084] c. Preparation of Ni(OH)2 / Co3O4 / NF heterostructure electrode material: 0.6mmol Ni(NO3)2·6H2O, 3.2mmol NH4F and 4.75mmol CO(NH2)2 were dissolved in 60mL deionized water, stirred thoroughly and transferred to a 100mL reactor, and the prepared Co3O4 / NF composite electrode material was immersed therein, reacted at 150°C for 9h, cooled to room temperature, and washed the electrode with ethanol and deionized water several times to remove the residual solution, and then vacuum dried at 60°C overnight to obtain Ni(OH)2 / Co3O4 / NF heterostructure electrode material;

[0085] d. Preparation of Ni5P4 / Co3O4 / NF heterostructure electrode material: 3.0 g of NaPO2H2 was placed upstream of the air flow of the tube furnace, and 10 g of the prepared Ni(OH)2 / Co3O4 / NF heterostructure electrode material was placed downstream of the tube furnace. The temperature was raised from room temperature to 400°C in an Ar atmosphere at a heating rate of 2°C / min and annealed for 3 h to obtain the Ni5P4 / Co3O4 / NF heterostructure electrode material.

[0086] Comparative Example

[0087] In order to explore the influence of different parameters in the preparation process of the present invention on the performance of the product of the present invention, the following comparative test was carried out. Different hydrogen evolution catalytic electrode materials were prepared in the following comparative examples, as follows:

[0088] Comparative Example 1

[0089] The nickel foam is ultrasonically cleaned with acetone, ethanol, hydrochloric acid and water in sequence to remove surface stains and oxides, and a clean nickel foam is prepared to be directly used as a hydrogen evolution catalytic electrode material (NF electrode material).

[0090] Comparative Example 2

[0091] An electrode material similar to that of Example 1 was prepared, except that steps c and d were not performed, that is, the Co3O4 / NF composite electrode material prepared by steps a and b was directly used as a hydrogen evolution catalytic electrode material (Co3O4 / NF electrode material).

[0092] Comparative Example 3

[0093] An electrode material similar to that in Example 1 is prepared, except that steps a and b are not performed, that is, Ni(OH)2 nanosheets are directly grown on clean nickel foam by hydrothermal reaction, and the preparation method is the same as step c. The Ni2P / NF composite electrode material obtained after phosphating treatment in step d is directly used as a hydrogen evolution electrode material (Ni2P / NF electrode material).

[0094] Performance Testing

[0095] The electrochemical performance of the electrode materials prepared in Example 1 and the comparative example was tested, and the test process was carried out in the following steps:

[0096] a. Preparation of working electrode: Ni5P4 / Co3O4 / NF, Co3O4 / NF, Ni2P / NF and NF electrode materials were cut into 1×1 cm size and directly used as catalysts for hydrogen evolution reaction;

[0097] b. Test system construction: The test system is a classic three-electrode system. The prepared electrode is directly used as the working electrode, the carbon rod and saturated calomel electrode are used as the counter electrode and reference electrode respectively, and the electrolyte is 1M KOH solution;

[0098] c. Electrochemical test was performed using CHI660E workstation. The linear sweep voltammetry curve voltage range was -1.0 to -1.8 V, and the scan rate was 10 mV s -1 ;

[0099] d. The electrochemical impedance test conditions were carried out at room temperature and the frequency range was 100kHz to 10mHz;

[0100] e. The non-Faraday potential window is selected within a range of 100 mV. Cyclic voltammetry curves are collected at different scan rates. The current density difference between the positive and negative electrodes is plotted relative to the scan rate. The slope of the fitted line is the double-layer capacitance (C dl );

[0101] f. According to C dl The value can be used to estimate the electrochemical specific surface area (ECSA) of the electrode and further evaluate the intrinsic activity of the catalyst;

[0102] g. Test the stability of the electrode by chronoamperometry, and select a voltage of -1.57V;

[0103] h. Structural characterization of the electrode: The dried electrode was directly characterized by ex situ X-ray diffraction (XRD), X-ray photoelectron spectroscopy (XPS), scanning electron microscopy (SEM) and transmission electron microscopy (TEM).

[0104] The results after the test are as follows:

[0105] (I) Morphology and structural characterization of self-supported hierarchical Ni5P4 / Co3O4 / NF heterostructure electrodes:

[0106] In Example 1, after step a, Co(OH)2 nanowires are in situ grown on the surface of nickel foam by hydrothermal reaction, and the morphology thereof is as follows: Figure 3 As shown; after step b, calcination in air forms Co3O4 nanowires of uniform size as a template precursor, Figure 4This is a scanning electron microscope (SEM) image of the Co3O4 / NF composite electrode material. In the image, it can be seen that the diameter of the Co3O4 nanowire is about 50nm and the length is about 2μm; Figure 5 This is the X-ray diffraction (XRD) diagram of the Co3O4 / NF composite electrode material. It can be seen from the figure that in addition to the characteristic peak of Ni, additional diffraction peaks appear at 2θ=31.3°, 36.8°, 59.4° and 65.2°, corresponding to Co3O4. The tiny Co3O4 nanowires as a substrate limit the subsequent growth of Ni(OH)2, thereby forming ultra-thin nanosheets, which are more easily fully phosphated into Ni5P4 instead of the common Ni2P. Figure 6 This is the microscopic morphology of the Ni5P4 / Co3O4 / NF heterostructure electrode material finally prepared. It can be seen from the figure that the product is a nanorod array formed by combining ultra-thin Ni5P4 nanosheets and Co3O4 nanowires integrated on the nickel foam current collector, where the thickness of the Ni5P4 nanosheets is only a few nanometers; Figure 7 The XRD diagram of the Ni5P4 / Co3O4 / NF heterostructure electrode material shows that the diffraction peaks at 2θ=44.5°, 51.8° and 76.4° correspond to the (111), (200) and (220) planes of nickel foam (JCPDS 04-0850), and the other diffraction peaks correspond to Ni5P4 (JCPDS 89-2588). The diffraction peak of Co3O4 is not obvious because it is completely covered by Ni5P4 nanosheets and the X-rays excited by the Cu target are not sensitive to Co-based materials. As a comparative example 3 of the comparative experiment, Ni(OH)2 nanosheets are directly grown on the surface of the nickel foam substrate by hydrothermal reaction, and the Ni2P / NF composite electrode material is prepared after phosphating. The test results of the product are shown in FIG. Figure 8 and Fig. 9 As shown, Figure 8 This is the SEM image of the Ni2P / NF composite electrode. It can be seen from the figure that due to the absence of Co3O4 nanowires as a precursor to limit the growth of Ni(OH)2, the size of the formed Ni(OH)2 nanosheets is significantly increased. Fig. 9 This is the XRD diagram of the Ni2P / NF composite electrode material, which confirms the existence of Ni2P on the surface of the Ni skeleton.

[0107] Fig.10 This is the full X-ray photoelectron spectroscopy (XPS) spectrum of Ni2P / NF, Co3O4 / NF and Ni5P4 / Co3O4 / NF electrode materials, which confirms the presence of Ni, Co, P and O elements in the Ni5P4 / Co3O4 / NF heterostructure electrode. Fig.11This is a high-resolution transmission electron microscopy (HRTEM) image of the Ni5P4 / Co3O4 interface. An obvious two-phase interface can be observed in the image, and Ni5P4 is seamlessly integrated on the Co3O4 surface. This unique combination can effectively reduce contact resistance and charge transfer resistance, which is conducive to rapid reaction. The stable interface structure also ensures the service life of the electrode.

[0108] Ex situ XPS spectroscopy was used to characterize the valence states of elements in Co3O4 / NF, Ni2P / NF and Ni5P4 / Co3O4 / NF electrode materials. Fig.12 High-resolution Ni 2p XPS spectra of Ni2P / NF, Co3O4 / NF and Ni5P4 / Co3O4 / NF electrode materials. It can be seen from the figure that in addition to the metallic Ni from the nickel foam, the Co3O4 / NF and Ni2P / NF electrode materials also contain Ni due to calcination in air and the formation of Ni2P. 2+ However, the Ni 2pXPS spectrum of the Ni5P4 / Co3O4 / NF heterostructure electrode material only shows the characteristic peaks of the Ni oxidation state, because the thickness of the Ni5P4 nanosheets coated on the surface exceeds the detection depth of the device.

[0109] Fig.13 High-resolution Co 2p XPS spectra of Ni2P / NF, Co3O4 / NF and Ni5P4 / Co3O4 / NF heterostructure electrode materials. Comparing the Co3O4 / NF and Ni5P4 / Co3O4 / NF electrode materials, after the Ni5P4 nanosheets were constructed on the surface of the Ni5P4 / Co3O4 / NF prepared in Example 1, the peak position of the Co atoms moved toward the high binding energy direction, which indicated that the charge was transferred directionally from the Co3O4 nanowires to the Ni5P4 nanosheets.

[0110] Fig.14 Figure 2 is the P 2p XPS spectra of Co3O4 / NF, Ni2P / NF and Ni5P4 / Co3O4 / NF heterogeneous electrode materials. It can be seen from the figure that the double peaks at 129.6eV and 134.5eV correspond to metal phosphide (MP) and oxidized metal phosphide (MPO), respectively. From the P 2p XPS spectrum of Ni5P4 / Co3O4 / NF heterostructure electrode material, it is found that the characteristic peak of MP is almost imperceptible, indicating that Ni5P4 is very easy to oxidize due to exposure to air, which is related to the strong oxygen absorption of Ni5P4. This conclusion can be Fig.15 The O1s XPS spectrum in Fig.15It can be seen that at a binding energy of 533.0 eV, compared with Co3O4 / NF and Ni2P / NF electrode materials, the Ni5P4 / Co3O4 / NF heterostructure electrode material has a significantly enhanced oxygen adsorption characteristic peak, which can promote the adsorption and dissociation of water molecules, which may be one of the reasons for its excellent catalytic performance in alkaline hydrogen evolution reaction; in addition, compared with the Ni2P / NF electrode material, the P 2p XPS spectrum of the Ni5P4 / Co3O4 / NF heterostructure electrode material shifts toward the low binding energy direction by about 0.24 eV, indicating that the P atoms in Ni5P4 receive electrons from the Co3O4 nanowires. This redistribution of charge between the heterostructure interfaces can effectively regulate the electronic structure of the active sites and improve the intrinsic catalytic activity.

[0111] To evaluate the electrocatalytic performance, electrochemical measurements were performed in a typical three-electrode system using Ni5P4 / Co3O4 / NF, Co3O4 / NF, Ni2P / NF, and pure NF electrode materials directly as working electrodes, and saturated calomel electrode (SCE) and carbon rod as reference and counter electrodes, respectively. Figure 1 The linear sweep voltammetry (LSV) curves of Ni5P4 / Co3O4 / NF, Co3O4 / NF, Ni2P / NF and pure NF electrode materials in 0.1M KOH electrolyte are shown, where the potential is iR corrected relative to the reversible hydrogen electrode (RHE) and the current density is normalized by the geometric area. The results show that the current density of the Ni5P4 / Co3O4 / NF heterostructure electrode material is significantly higher than that of Co3O4 / NF, Ni2P / NF and pure NF electrode materials, indicating that the Ni5P4 / Co3O4 / NF heterostructure electrode material has the best HER catalytic performance at the same potential, and only 265mV overpotential is required to achieve -1500mA cm -2 The ultra-large current density; In addition, Figure 1 The inset is the enlarged LSV curve. It can be seen that the starting potential of the Ni5P4 / Co3O4 / NF heterostructure electrode material is close to 0V, indicating that the Ni5P4 / Co3O4 catalyst effectively reduces the reaction energy barrier of HER.

[0112] Fig.16 The results of comparing the performance of Ni5P4 / Co3O4 / NF, Co3O4 / NF, Ni2P / NF and pure NF electrode materials to achieve 200 mA cm -2 The overpotential required for the current density and the current density achieved at an overpotential of 250 mV. The Ni5P4 / Co3O4 / NF heterostructure electrode material only requires an overpotential of 152.2 mV to achieve 200 mA cm -2The current density of the hierarchical Ni5P4 / Co3O4 / NF heterostructure electrode material can reach 1282.0 mA cm at 0.25 V. -2 Industrial current density, respectively Ni2P / NF (118.3mA·cm -2 )、Co3O4 / NF(21.7mA·cm -2 ) and NF (16.3 mA cm -2 ) are 10.8 times, 59.0 times and 78.7 times.

[0113] Fig.17 The Tafel slope diagram of Ni5P4 / Co3O4 / NF, Co3O4 / NF, Ni2P / NF and pure NF electrode materials, among which the Tafel slope of Ni5P4 / Co3O4 / NF heterostructure electrode material is as low as 76.6mV·dec -1 , which is much smaller than other electrodes, indicating that the reaction kinetics of the Ni5P4 / Co3O4 / NF heterostructure electrode material catalyst is the fastest; the Tafel slope is between 40 and 120 mV·dec -1 In the range of , it indicates the Volmer-Heyrovsky mechanism, in which the Volmer step (i.e., the dissociation of water into OH - and *H) is the rate-determining step (RDS).

[0114] The fast reaction kinetics of Ni5P4 / Co3O4 / NF heterostructure electrode materials can also be Fig.18 The Nyquist plot of electrochemical impedance spectroscopy (EIS) in Figure 2 shows that the equivalent circuit model for fitting EIS is composed of the intrinsic electrode and electrolyte resistances (R s ), constant phase element (C PE ) and charge transfer resistance (R ct ) composition, the semicircular area of ​​the Ni5P4 / Co3O4 / NF heterostructure electrode material is smaller, indicating that its charge transfer resistance (R ct ) is lower; the composite nonlinear least squares fitting results show that the charge transfer resistance of Ni5P4 / Co3O4 / NF heterostructure electrode material is as low as 1.7Ω, which is much smaller than Ni2P / NF (5.7Ω), Co3O4 / NF (13.7Ω) and pure NF (29.0Ω) electrode materials.

[0115] In order to evaluate the intrinsic activity of Ni5P4, Ni2P, Co3O4 and Ni, the double layer capacitance (C dl) method to estimate the electrochemical surface area (ECSA) of Ni5P4 / Co3O4 / NF, Co3O4 / NF, Ni2P / NF and pure NF electrode materials, where cyclic voltammetry was performed at different scan rates in the non-Faraday voltage window, as Fig.19 , 20 , 21 and 22; C is measured by plotting the relationship between ΔJ and the scan rate dl Value, where ΔJ=(J a -J c ) / 2,J a is the anode current density, J c is the cathode current density, and the slope of the fitting line is C dl Values, such as Fig.23 As shown in the figure, the C of Ni5P4 / Co3O4 / NF heterostructure electrode material dl Value (139.9mF·cm -2 ) is much higher than Co3O4 / NF (97.5mF·cm -2 )、Ni2P / NF(78.9mF·cm -2 ) and pure NF electrode material (21.9mF·cm -2 ), according to the measured C dl Value and average roughness coefficient (R f )40μF·cm -2 According to the formula ECSA=C dl / R f Estimate the ECSA value of each electrode, such as Fig.24 As shown in Figure 2, the ECSA value of the Ni5P4 / Co3O4 / NF heterostructure electrode material is as high as 3497.5 cm 2 cm -2 geo , which is significantly higher than the other three electrode materials, indicating that the Ni5P4 / Co3O4 / NF heterostructure electrode material can expose more active sites, which is another reason for its excellent catalytic performance.

[0116] In order to exclude the influence of ECSA, the specific activity of the electrode is intuitively displayed, such as Fig.25 As shown, the polarization curves of four electrode materials, NF, Ni2P / NF, Co3O4 / NF and Ni5P4 / Co3O4 / NF, are plotted with ECSA-normalized current density and iR-corrected potential as the y-axis and x-axis. Compared with the other three electrode materials, the Ni5P4 / Co3O4 / NF heterostructure electrode material still shows quite obvious advantages; Fig.26 The bar graph in Figure 2 shows that the specific activity of Ni5P4 is as high as 374.1 μA·cm at an overpotential of 250 mV. -2, compared with Ni2P (67μA·cm -2 )、Co3O4(13μA·cm -2 ) and NF (23 μA·cm -2 ) were 5.5 times, 28.7 times and 16.2 times higher respectively.

[0117] In order to detect the service performance of the electrode, a chronoamperometric test was performed at a potential of -1.54 V. Fig. 27 The stability test results of Ni5P4 / Co3O4 / NF heterostructure electrode show that the Ni5P4 / Co3O4 / NF heterostructure electrode material is close to -1000mA·cm -2 When working under high current density for 50h, the current density does not change significantly; Fig.28 This is the LSV curve of the Ni5P4 / Co3O4 / NF heterostructure electrode material before and after the stability test, which can further prove that the current density has almost no attenuation before and after the electrode stability test; Fig.29 This is the SEM image of the Ni5P4 / Co3O4 / NF heterostructure electrode material after stability test. It can be seen that the morphology of the electrode has not changed, indicating that the electrode has good stability.

[0118] Fig.30 , 31 The SEM images of a self-supporting graded Ni5P4 / Co3O4 / NF heterostructure electrode material prepared in Examples 2 and 3 respectively show that the Ni5P4 / Co3O4 / NF heterostructure electrode materials prepared in Examples 2 and 3 have similar morphologies to the Ni5P4 / Co3O4 / NF heterostructure electrode material prepared in Example 1, showing a heterostructure composite of nanosheets and nanowires.

[0119] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein with equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the scope of protection of the claims of the present invention.

Claims

1. A self-supporting graded Ni 5 P 4 / Co 3 O 4 / NF heterostructure electrode material preparation method, It is characterized in that Follow the steps below in order: a. Preparation of Co(OH) 2 / NF composite electrode material: The nickel foam was ultrasonically cleaned with acetone, ethanol, hydrochloric acid and water in sequence to remove surface stains and oxides. 3 ) 2 6H 2 O、NH 4 F and CO(NH 2 ) 2 Dissolve in deionized water, stir thoroughly and transfer to a reactor together with clean nickel foam, react at 100-150°C for 3-9h, cool to room temperature and wash the electrode with ethanol and deionized water several times to remove residual solution, then vacuum dry at 60°C overnight to obtain Co(OH) 2 / NF composite electrode materials; b. Preparation of Co 3 O 4 / NF composite electrode material: Co(OH) 2 / NF composite electrode material was calcined in air to obtain Co 3 O 4 / NF composite electrode materials; c. Preparation of Ni(OH) 2 / Co 3 O 4 / NF heterostructure electrode materials: Ni(NO 3 ) 2 6H 2 O、NH 4 F and CO(NH 2 ) 2 Dissolve in deionized water, stir thoroughly and transfer to the reactor. 3 O 4 / NF composite electrode material was immersed in it, reacted at 100-150℃ for 3-9h, cooled to room temperature, and washed the electrode with ethanol and deionized water several times to remove the residual solution, and then vacuum dried at 60℃ overnight to obtain Ni(OH) 2 / Co 3 O 4 / NF heterostructure electrode materials; d. Preparation of Ni 5 P 4 / Co 3 O 4 / NF heterostructure electrode materials: NaPO 2 H 2 Placed upstream of the tube furnace gas flow, Ni(OH) 2 / Co 3 O 4 The / NF heterostructure electrode material was placed downstream of a tube furnace and annealed in an Ar atmosphere to obtain Ni 5 P 4 / Co 3 O 4 / NF heterostructure electrode materials.

2. A self-supporting graded Ni according to claim 1 5 P 4 / Co 3 O 4 / NF heterostructure electrode material preparation method, It is characterized in that In step a, the Co(NO 3 ) 2 6H 2 O、NH 4 F and CO(NH 2 ) 2 The mass ratio is (100~200):42:

171.

3. A self-supporting graded Ni according to claim 1 5 P 4 / Co 3 O 4 / NF heterostructure electrode material preparation method, It is characterized in that In step b, the calcination temperature is 200-400° C. and the time is 1-3 hours.

4. A self-supporting graded Ni according to claim 3 5 P 4 / Co 3 O 4 / NF heterostructure electrode material preparation method, It is characterized in that In step b, the heating rate during calcination is 5°C / min.

5. A self-supporting graded Ni according to claim 1 5 P 4 / Co 3 O 4 / NF heterostructure electrode material preparation method, It is characterized in that In step c, the Ni(NO 3 ) 2 6H 2 O、NH 4 F and CO(NH 2 ) 2 The molar ratio is (3-6):32:47.

5.

6. A self-supporting graded Ni according to claim 1 5 P 4 / Co 3 O 4 / NF heterostructure electrode material preparation method, It is characterized in that In step d, the NaPO 2 H 2 with Ni 5 P 4 / Co 3 O 4 The mass ratio of / NF heterostructure electrode materials is (1~3):

10.

7. A self-supporting graded Ni according to claim 1 5 P 4 / Co 3 O 4 / NF heterostructure electrode material preparation method, It is characterized in that In step d, the annealing temperature is 300-400° C. and the time is 1-3 hours.

8. A self-supporting graded Ni according to claim 7 5 P 4 / Co 3 O 4 / NF heterostructure electrode material preparation method, It is characterized in that In step d, the heating rate of the annealing process is 2°C / min.

9. A self-supporting graded Ni according to any one of claims 1 to 8. 5 P 4 / Co 3 O 4 / NF heterostructure electrode material preparation method, It is characterized in that The Ni 5 P 4 / Co 3 O 4 / NF heterostructure electrode material structure is ultra-thin Ni 5 P 4 Nanosheets and Co 3 O 4 The nanorod arrays formed by the combination of nanowires are integrated on the nickel foam current collector.