Preparation process of ultra-high molecular weight body armor heat-resistant flame-retardant fiber

By adding catalyst and compatibilizer to ultra-high molecular weight polyethylene fibers and mixing them with other flame retardant materials to form a composite 2UD structure, the problem of insufficient heat resistance and flame retardancy of fibers is solved, and the bulletproof vest is significantly improved Heat resistance and flame retardant properties.

CN119082909APending Publication Date: 2024-12-06JIANGSU XINGDUN NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411481496.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-23
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Ultra-high molecular weight polyethylene fibers have problems with insufficient heat resistance and flame retardancy in the body armor, especially when the temperature rises, which can easily cause creep, affecting performance.

Method used

Using a process, it is modified by adding a catalyst and a compatibilizer to the ultra-high molecular weight polyethylene fiber stock solution, and it is also modified with carbon nanoatoms, phosphorus-based flame retardants, inorganic nanofire retardants, nitrogen-based flame retardants and other materials. Mixed to form an additive slurry, which is melt-spinned, cooling and stretching, relaxation treatment and water-based polyurethane soaking, and finally forms a composite 2UD structure of ultra-high molecular weight body armor heat-resistant flame retardant fiber.

Benefits of technology

It significantly improves the flame retardancy and heat resistance of the fiber, improves its resistance to heat and ballistic invasion, extends the melting point and heat resistance of the fiber, and enhances physical resistance and bulletproof performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082909A_ABST
    Figure CN119082909A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation process of ultra-high molecular weight body armor heat-resistant flame-retardant fibers, which comprises the following main steps: raw material treatment, melt spinning, cooling and stretching, post-treatment, material compounding, product detection and delivery, firstly, a spinning solution is prepared, then four editions of UHMWPE fibers are sequentially obtained, and the ultra-high molecular weight body armor heat-resistant flame-retardant fibers are obtained. And finally tiling and compounding to obtain the ultra-high molecular weight body armor heat-resistant flame-retardant fiber. According to the invention, the catalyst and the compatilizer are added into the fiber stock solution, and the interfacial force is enhanced through the combination of chemical bonds, so that the modified stock solution with better compatibility is obtained, and subsequent addition of auxiliaries is facilitated; related auxiliaries are added, so that clustered CNPs are formed on the surface of the subsequently obtained fiber, the clustered CNPs serve as a sporadic first ignition point, a combustion spreading route is broken, the overall flame retardance is improved, and the isolation performance of the fiber can be effectively improved through in-situ modification of the CNPs; the fiber is soaked in a water-based polyurethane WUP material liquid, a compact protective film is formed on the surface of the fiber, and physical resistance including but not limited to heat resistance is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of protective fibers, and more specifically, to a preparation process of ultra-high molecular weight bulletproof vest heat-resistant and flame-retardant fibers. Background Art

[0002] The core material of bulletproof vests is high-strength and high-toughness fiber materials, among which the most commonly used is ultra-high molecular weight polyethylene fiber, which is a linear unbranched polyethylene with a molecular weight greater than 1.5 million. It is known for its high modulus, low density, good wear resistance, low temperature resistance, UV resistance, shielding resistance, good acid and alkali resistance, and strong impact resistance. However, it also has disadvantages such as low surface hardness and low heat deformation temperature, which generally need to be overcome with the help of modification methods. For example, the hydrophilicity of UHMWPE can be effectively enhanced through plasma modification, the biocompatibility of UHMWPE can be optimized through radiation modification, and the composite interface performance of UHMWPE can be significantly improved through grafting modification.

[0003] At present, there is room for improvement in the heat resistance and flame retardancy of ultra-high molecular weight polyethylene fibers used in bulletproof vests. Ultra-high molecular weight polyethylene fibers have a maximum heat resistance of 130°C, and rising temperatures will accelerate creep, which will inevitably affect the performance of bulletproof vests. Summary of the invention

[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a process for preparing ultra-high molecular weight heat-resistant and flame-retardant fibers for bulletproof vests to solve one or more of the above-mentioned problems.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] A process for preparing ultra-high molecular weight heat-resistant and flame-retardant fibers for bulletproof vests comprises the following steps:

[0007] S1. Raw material processing: under anaerobic conditions, adding a catalyst and a compatibilizer to the ultra-high molecular weight polyethylene UHMWPE fiber stock solution, heating and mixing in an internal mixer for modification, and obtaining a modified UHMWPE stock solution;

[0008] The carbon nano-atom CNPs material, phosphorus flame retardant, inorganic nano flame retardant particles, nitrogen flame retardant, polycarbonate and nano boron particles are mixed and ground, added into quaternary ammonium salt ionic liquid and mixed evenly to obtain an additive slurry;

[0009] The modified UHMWPE stock solution and the auxiliary agent slurry are mixed in a ratio of 24 to 30:1 and allowed to stand to obtain a spinning stock solution;

[0010] S2, melt spinning: the spinning solution is heated to a molten state, enters the spinning machine through a screw extruder, and is extruded from a metering pump spinneret to form continuous molten fibers;

[0011] S3, cooling and stretching: the extruded molten fiber is rapidly cooled and solidified in a water bath, and stretched by a stretching machine to obtain modified UHMWPE fiber I;

[0012] S4, post-treatment: performing relaxation treatment on the stretched modified UHMWPE fiber to obtain modified UHMWPE fiber II;

[0013] S5. Material compounding: immersing the treated modified UHMWPE fiber II in a sedimentation tank filled with aqueous polyurethane WUP liquid to obtain modified UHMWPE fiber III;

[0014] The modified UHMWPE fiber III is evenly laid on the support film by a fiber winding machine to form a parallel and straightly arranged single UD structure UHMWPE fiber IV;

[0015] The UHMWPE fiber IV is compounded into a 2UD structured ultra-high molecular weight bulletproof heat-resistant and flame-retardant fiber by an equipment in an orthogonal stacking manner;

[0016] S6. Product testing and delivery.

[0017] Furthermore, in step S1, the catalyst is prepared by mixing polyethylene oxide, xylene, triethylamine and acyl bromide in a ratio of 1:4.9:2:0.7 in a water bath at 80°C.

[0018] Furthermore, in step S1, the compatibilizer is prepared by reacting copper sulfate, potassium bromide, sodium tripolyphosphate and anisole in a ratio of 1:1:0.2:17 at a temperature not lower than 75° C. for 8 to 10 hours under a vacuum environment.

[0019] Furthermore, in step S1, the internal mixer is mixed for 2 to 3 hours at a speed of 50 to 215 r / min, an effective internal mixer volume of not less than 150 L, and a pressure of 0.6 to 0.8 MPa.

[0020] Furthermore, in step S1, the carbon nanoatom CNPs material is nanocarbon spheres;

[0021] The phosphorus-based flame retardant is one or more of phosphate, phosphite, and phosphonate;

[0022] The inorganic nano flame retardant particles are fumed silica inorganic nano particles;

[0023] The nitrogen flame retardant is one or more of melamine MA, polynitrogen flame retardant melamine phosphate MPP, and melamine cyanurate MCA;

[0024] The quaternary ammonium salt ionic liquid is one or more of 1-ethylpyridinium bromide solution, 1-butyl-3-methylimidazole solution, and 1-butylpyridinium chloride solution.

[0025] Furthermore, the formula of the additive slurry is calculated by weight: 10 to 13 parts of carbon nanoatom CNPs material, 5 to 8 parts of phosphorus flame retardant, 2 to 5 parts of inorganic nano flame retardant particles, 3 to 6 parts of nitrogen flame retardant, 1 to 2 parts of polycarbonate, 0.4 to 1.5 parts of nano boron particles, and 22 to 36 parts of quaternary ammonium salt ionic liquid.

[0026] Furthermore, the molecular weight of the ultra-high molecular weight polyethylene UHMWPE fiber stock solution in step S1 is not less than 3.5 million.

[0027] Furthermore, in step S4, a relaxation treatment is performed by heat setting.

[0028] Furthermore, in step S5, the modified UHMWPE fiber III is firstly passed through an extractor to remove excess chemical reagents on the surface and then wound and laid flat.

[0029] Furthermore, in order to facilitate the wetting of the modified UHMWPE fiber II in step S5, the aqueous polyurethane WUP stock solution is diluted with deionized water in a mass ratio of 1:1 to 1.2 in advance to obtain an aqueous polyurethane WUP stock solution.

[0030] In summary, the present invention has the following beneficial effects:

[0031] 1. Add catalyst and compatibilizer to the ultra-high molecular weight polyethylene UHMWPE fiber stock solution, combine through chemical bonds, strengthen the interfacial force, and obtain a modified UHMWPE stock solution with better compatibility, which is convenient for subsequent mixing of additives;

[0032] 2. Add additives such as carbon nano-atoms (CNPs) to make the surface of the fiber obtained later have clusters of CNPs, which are used as sporadic first ignition points to destroy the combustion propagation route and improve the overall flame retardancy. The in-situ modification of CNPs can effectively improve the insulation performance of the fiber, such as resistance to external influences such as heat and ballistic penetration;

[0033] 3. Soaking the fiber in water-based polyurethane WUP liquid can form a dense protective film on its surface, improving physical resistance including but not limited to heat resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 A flow chart of a preparation process according to an embodiment of the present invention;

[0035] Figure 2 A process equipment roadmap for an embodiment of the present invention;

[0036] Figure 3 A microscopic image of the surface of a finished fiber according to an embodiment of the present invention. DETAILED DESCRIPTION

[0037] The following is combined with Figure 1-3 The present invention is described in further detail.

[0038] Example 1

[0039] The preparation process of ultra-high molecular weight bulletproof heat-resistant flame-retardant fiber comprises the following steps:

[0040] S1. Raw material processing:

[0041] S1.1, under anaerobic conditions, adding a catalyst and a compatibilizer to an ultra-high molecular weight polyethylene UHMWPE fiber stock solution, heating and mixing in an internal mixer for modification, and obtaining a modified UHMWPE stock solution;

[0042] Among them, the molecular weight of ultra-high molecular weight polyethylene UHMWPE fiber stock solution is not less than 3.5 million;

[0043] The catalyst is prepared by mixing polyethylene oxide, xylene, triethylamine and acyl bromide in a ratio of 1:4.9:2:0.7 in a water bath at 80°C.

[0044] The compatibilizer is prepared by reacting copper sulfate, potassium bromide, sodium tripolyphosphate and anisole in a ratio of 1:1:0.2:17 at an environment not lower than 75°C for 8 hours under vacuum;

[0045] Mixing in an internal mixer at a speed of 50 r / min, an effective mixing volume of not less than 150 L, and a pressure of 0.6 MPa for 2 h;

[0046] S1.2, mixing carbon nano-atom CNPs material, phosphorus flame retardant, inorganic nano flame retardant particles, nitrogen flame retardant, polycarbonate, and nano-boron particles, grinding them, adding them into quaternary ammonium salt ionic liquid and mixing them evenly to obtain an additive slurry;

[0047] Among them, the carbon nanoatom CNPs material is nanocarbon spheres;

[0048] The phosphorus-based flame retardant is one or more of phosphate, phosphite, and phosphonate;

[0049] The inorganic nano flame retardant particles are fumed silica inorganic nano particles;

[0050] The nitrogen flame retardant is one or more of melamine MA, polynitrogen flame retardant melamine phosphate MPP, and melamine cyanurate MCA;

[0051] The quaternary ammonium salt ionic liquid is one or more of 1-ethylpyridinium bromide solution, 1-butyl-3-methylimidazole solution, and 1-butylpyridinium chloride solution;

[0052] The formula of the additive slurry is calculated by weight: 10 parts of carbon nano-atom CNPs material, 5 parts of phosphorus flame retardant, 2 parts of inorganic nano flame retardant particles, 3 parts of nitrogen flame retardant, 1 part of polycarbonate, 0.4 parts of nano boron particles, and 22 parts of quaternary ammonium salt ionic liquid;

[0053] S1.3, mixing the modified UHMWPE stock solution and the additive slurry in a ratio of 24:1 and letting it stand to obtain a spinning stock solution;

[0054] S2, melt spinning: the spinning solution is heated to a molten state, enters the spinning machine through a screw extruder, and is extruded from a metering pump spinneret to form continuous molten fibers;

[0055] S3, cooling and stretching: the extruded molten fiber is rapidly cooled and solidified in a water bath, and stretched by a stretching machine to obtain modified UHMWPE fiber I;

[0056] S4, post-treatment: performing a relaxation treatment on the stretched modified UHMWPE fiber by heat setting to obtain modified UHMWPE fiber II;

[0057] S5. Material Composite:

[0058] S5.1, immersing the treated modified UHMWPE fiber II in a sedimentation tank filled with aqueous polyurethane WUP liquid to obtain modified UHMWPE fiber III;

[0059] S5.2, firstly, the modified UHMWPE fiber III is passed through an extractor to remove excess chemical reagents on the surface, and then is evenly spread on the support film through a fiber winding machine to form a parallel and straightly arranged single UD structure UHMWPE fiber IV;

[0060] S5.3, compounding UHMWPE fiber IV into a 2UD structured ultra-high molecular weight bulletproof heat-resistant flame-retardant fiber through equipment in an orthogonal stacking manner;

[0061] S6. Product testing and delivery.

[0062] Example 2

[0063] The preparation process of ultra-high molecular weight bulletproof heat-resistant flame-retardant fiber comprises the following steps:

[0064] S1. Raw material processing:

[0065] S1.1, under anaerobic conditions, adding a catalyst and a compatibilizer to an ultra-high molecular weight polyethylene UHMWPE fiber stock solution, heating and mixing in an internal mixer for modification, and obtaining a modified UHMWPE stock solution;

[0066] Among them, the molecular weight of ultra-high molecular weight polyethylene UHMWPE fiber stock solution is not less than 3.5 million;

[0067] The catalyst is prepared by mixing polyethylene oxide, xylene, triethylamine and acyl bromide in a ratio of 1:4.9:2:0.7 in a water bath at 80°C.

[0068] The compatibilizer is prepared by reacting copper sulfate, potassium bromide, sodium tripolyphosphate and anisole in a ratio of 1:1:0.2:17 at an environment not lower than 75°C for 10 hours under a vacuum environment;

[0069] Mixing in an internal mixer at a speed of 215 r / min, an effective mixing volume of not less than 150 L, and a pressure of 0.8 MPa for 3 h;

[0070] S1.2, mixing carbon nano-atom CNPs material, phosphorus flame retardant, inorganic nano flame retardant particles, nitrogen flame retardant, polycarbonate, and nano-boron particles, grinding them, adding them into quaternary ammonium salt ionic liquid and mixing them evenly to obtain an additive slurry;

[0071] Among them, the carbon nanoatom CNPs material is nanocarbon spheres;

[0072] The phosphorus-based flame retardant is one or more of phosphate, phosphite, and phosphonate;

[0073] The inorganic nano flame retardant particles are fumed silica inorganic nano particles;

[0074] The nitrogen flame retardant is one or more of melamine MA, polynitrogen flame retardant melamine phosphate MPP, and melamine cyanurate MCA;

[0075] The quaternary ammonium salt ionic liquid is one or more of 1-ethylpyridinium bromide solution, 1-butyl-3-methylimidazole solution, and 1-butylpyridinium chloride solution;

[0076] The formula of the additive slurry is calculated by weight, including 13 parts of carbon nano-atom CNPs material, 8 parts of phosphorus flame retardant, 5 parts of inorganic nano flame retardant particles, 6 parts of nitrogen flame retardant, 2 parts of polycarbonate, 1.5 parts of nano boron particles, and 36 parts of quaternary ammonium salt ionic liquid;

[0077] S1.3, mixing the modified UHMWPE stock solution and the additive slurry in a ratio of 30:1 and letting it stand to obtain a spinning stock solution;

[0078] S2, melt spinning: the spinning solution is heated to a molten state, enters the spinning machine through a screw extruder, and is extruded from a metering pump spinneret to form continuous molten fibers;

[0079] S3, cooling and stretching: the extruded molten fiber is rapidly cooled and solidified in a water bath, and stretched by a stretching machine to obtain modified UHMWPE fiber I;

[0080] S4, post-treatment: performing a relaxation treatment on the stretched modified UHMWPE fiber by heat setting to obtain modified UHMWPE fiber II;

[0081] S5. Material Composite:

[0082] S5.1, immersing the treated modified UHMWPE fiber II in a sedimentation tank filled with aqueous polyurethane WUP liquid to obtain modified UHMWPE fiber III;

[0083] S5.2, firstly, the modified UHMWPE fiber III is passed through an extractor to remove excess chemical reagents on the surface, and then is evenly spread on the support film through a fiber winding machine to form a parallel and straightly arranged single UD structure UHMWPE fiber IV;

[0084] S5.3, compounding UHMWPE fiber IV into a 2UD structured ultra-high molecular weight bulletproof heat-resistant flame-retardant fiber through equipment in an orthogonal stacking manner;

[0085] S6. Product testing and delivery.

[0086] Example 3

[0087] The preparation process of ultra-high molecular weight bulletproof heat-resistant flame-retardant fiber comprises the following steps:

[0088] S1. Raw material processing:

[0089] S1.1, under anaerobic conditions, adding a catalyst and a compatibilizer to an ultra-high molecular weight polyethylene UHMWPE fiber stock solution, heating and mixing in an internal mixer for modification, and obtaining a modified UHMWPE stock solution;

[0090] Among them, the molecular weight of ultra-high molecular weight polyethylene UHMWPE fiber stock solution is not less than 3.5 million;

[0091] The catalyst is prepared by mixing polyethylene oxide, xylene, triethylamine and acyl bromide in a ratio of 1:4.9:2:0.7 in a water bath at 80°C.

[0092] The compatibilizer is prepared by reacting copper sulfate, potassium bromide, sodium tripolyphosphate and anisole in a ratio of 1:1:0.2:17 at an environment not lower than 75°C for 9 hours under vacuum;

[0093] Mixing in an internal mixer at a speed of 135 r / min, an effective mixing volume of not less than 150 L, and a pressure of 0.7 MPa for 2.5 h;

[0094] S1.2, mixing carbon nano-atom CNPs material, phosphorus flame retardant, inorganic nano flame retardant particles, nitrogen flame retardant, polycarbonate, and nano-boron particles, grinding them, adding them into quaternary ammonium salt ionic liquid and mixing them evenly to obtain an additive slurry;

[0095] Among them, the carbon nanoatom CNPs material is nanocarbon spheres;

[0096] The phosphorus-based flame retardant is one or more of phosphate, phosphite, and phosphonate;

[0097] The inorganic nano flame retardant particles are fumed silica inorganic nano particles;

[0098] The nitrogen flame retardant is one or more of melamine MA, polynitrogen flame retardant melamine phosphate MPP, and melamine cyanurate MCA;

[0099] The quaternary ammonium salt ionic liquid is one or more of 1-ethylpyridinium bromide solution, 1-butyl-3-methylimidazole solution, and 1-butylpyridinium chloride solution;

[0100] The formula of the additive slurry is calculated by weight, including 12 parts of carbon nano-atom CNPs material, 7 parts of phosphorus flame retardant, 3 parts of inorganic nano flame retardant particles, 5 parts of nitrogen flame retardant, 1.5 parts of polycarbonate, 1 part of nano boron particles, and 29 parts of quaternary ammonium salt ionic liquid;

[0101] S1.3, mixing the modified UHMWPE stock solution and the additive slurry in a ratio of 27:1 and letting it stand to obtain a spinning stock solution;

[0102] S2, melt spinning: the spinning solution is heated to a molten state, enters the spinning machine through a screw extruder, and is extruded from a metering pump spinneret to form continuous molten fibers;

[0103] S3, cooling and stretching: the extruded molten fiber is rapidly cooled and solidified in a water bath, and stretched by a stretching machine to obtain modified UHMWPE fiber I;

[0104] S4, post-treatment: performing a relaxation treatment on the stretched modified UHMWPE fiber by heat setting to obtain modified UHMWPE fiber II;

[0105] S5. Material Composite:

[0106] S5.1, immersing the treated modified UHMWPE fiber II in a sedimentation tank filled with aqueous polyurethane WUP liquid to obtain modified UHMWPE fiber III;

[0107] S5.2, firstly, the modified UHMWPE fiber III is passed through an extractor to remove excess chemical reagents on the surface, and then is evenly spread on the support film through a fiber winding machine to form a parallel and straightly arranged single UD structure UHMWPE fiber IV;

[0108] S5.3, compounding UHMWPE fiber IV into a 2UD structured ultra-high molecular weight bulletproof heat-resistant flame-retardant fiber through equipment in an orthogonal stacking manner;

[0109] S6. Product testing and delivery.

[0110] The anaerobic condition in step S1 can be achieved by filling with nitrogen, and nitrogen deoxygenation is performed at least three times; the catalyst and the compatibilizer are preferably prepared by mixing in a four-mouth beaker, and the four raw materials are ensured to be added and mixed at the same time; there is no special grinding requirement for the material grinding because the spinning solution will be melted later, and it is sufficient to ensure that the material can be smoothly mixed with the quaternary ammonium salt ionic liquid after grinding; the modified UHMWPE solution and the auxiliary agent slurry can be accelerated by ultrasonic treatment; the spinning parameters in step S2 are directly determined by the spinneret and are replaced according to customer needs; the water bath cooling, curing and stretching in step S3 and the heat setting in step S4 are all conventional operations without special requirements; in the material compounding stage in step S5, the solid particle mass fractionation of the waterborne polyurethane WPU is 50wt%, and the volume density is 1.2g / cm 3 Step S6 product testing mainly focuses on tensile strength, friction coefficient, wear rate, elongation at break, volume resistivity, etc., and tests are carried out on demand. Products that pass the test can be shipped directly or stored in the warehouse.

[0111] Figure 2 The production direction of the upper and middle parts is from right to left, and the lower part transports and processes the fiber products from left to right.

[0112] In summary, Examples 1 to 3 are experiments conducted under different conditions. The obtained ultra-high molecular weight bulletproof heat-resistant flame-retardant fibers are mainly tested in terms of heat resistance and flame retardancy. In order to more intuitively reflect the product advantages, the homologous ultra-high molecular weight polyethylene UHMWPE fiber stock solution is directly used to skip steps S1 and S5, and directly perform the process steps of steps S2, S3, and S4, and obtain the 2UD structure by conventional composite means to obtain the conventional bulletproof raw material initial fiber as a comparative example. The four groups of fibers must ensure that the basic parameters such as thickness and UD structure are the same.

[0113] First, four groups of fibers were subjected to FESEM (Hitachi-S4800, Japan) characterization experiments, and observed under the magnification environment of 20 μm, 2 μm, and 500 nm. The fibers of the comparative example and Example 3 were compared as examples. The image above is the surface feature of the comparative target fiber, and the image below is the surface feature of the target fiber of Example 3 obtained by the process of this application. It can be clearly observed that the latter has clustered CNPs distributed on the surface. This is because the raw materials were processed in advance, and catalysts and compatibilizers were added to the ultra-high molecular weight polyethylene UHMWPE fiber stock solution. The component materials of the compatibilizer have good compatibility with ultra-high molecular weight polyethylene, and can also improve various properties after modification. The compatibilizer and catalyst act, combined by chemical bond action, strengthen the interface action, and have a positive effect on the combination of subsequent other substances and the film formation of waterborne polyurethane WUP liquid, which is an important prerequisite for CNPs clustering. In addition, it can also reduce the surface friction coefficient and improve wear resistance and strength. Subsequent addition of additives such as carbon nano-atom CNPs materials can more conveniently cluster on the fiber surface. Clustering has two benefits. One is the flame-breaking effect. The landing points of clustered CNPs are irregular. When the bulletproof vest comes into contact with a fire source or spark, the cluster points will be ignited in advance, which can effectively block the spread route, thereby improving flame retardancy. At the same time, it also helps to block the heat exchange between the fiber cluster points and the outside world, playing a role in heat insulation.

[0114] Secondly, the fiber is subjected to the GB / T 13767-92 textile heat resistance test, and the fiber is observed at high temperature to see if there are signs of damage such as melting, yellowing, sticking or shrinking, and the melting point of the fiber is determined. In the process of the present application, the fiber is immersed in the aqueous polyurethane WUP liquid after forming, and a dense protective film can be formed on the surface of the fiber together with the surface of the clustered CNPs. The direct protection of the fiber and the protection of the cluster points can improve the overall physical resistance of the bulletproof clothing, including but not limited to heat resistance, toughness, impact resistance, etc. The test results are summarized as the melting point of the three groups of fibers in the present application is 215~260℃, and the melting point of the comparative example is about 145~160℃. It is not difficult to conclude that the fiber product treated by the process of the present application has a better melting point, a higher heat resistance limit, and better overall heat resistance.

[0115] Then, the combustion of ultra-high molecular weight UHMWPE fiber is divided into five stages: heating, degradation, ignition, combustion and cyclic combustion. The limiting oxygen index of the fiber is mainly tested, and the experiment is carried out according to GB / T5454-1997 "Oxygen Index Method for Determination of Combustion Performance of Textile Fabrics": Test device inspection: Open the valve of the gas supply part, and arbitrarily select the concentration of the mixed gas, the flow rate is about 10L / min, close the outlet and inlet valves, and record the pressure and flow rate of oxygen, nitrogen and mixed gas. Leave it for 30 minutes, then observe the values ​​shown by each pressure gauge and flow meter, and check with the previous recorded value. If there is no change, it means that the device has no leakage. The test temperature and humidity test is carried out in an atmosphere with a temperature of 10-30℃ and a relative humidity of 30% to 80%.

[0116] Initial selection of sample oxygen concentration: When the oxygen index value of the sample to be tested is completely unknown, the sample can be ignited in the air. If the sample burns quickly, the oxygen concentration can start from about 18%. If the sample burns slowly or burns unsteadily, select an initial oxygen concentration of about 21%. If the sample cannot continue to burn in the air, select an initial concentration of not less than 25%. Based on the estimated oxygen concentration, find out the corresponding oxygen flow and ammonia flow. When changing the concentration, it should be noted that the total flow rate of the mixed gas is between 10 and 11.4 L / min; install the sample in the middle of the sample clamp and fix it, then vertically insert the sample clamp together with the sample on the sample support in the burning glass cylinder, the upper end of the sample is not less than 100 mm from the cylinder mouth, and the lowest end of the exposed part of the sample is not less than 100 mm from the top surface of the gas distribution device at the bottom of the cylinder; open the nitrogen valve, adjust the corresponding oxygen and nitrogen flow rates found in Appendix B, and let the adjusted air flow flow and flush the combustion cylinder for at least 30 seconds before the sample is ignited, and keep this flow rate unchanged during the ignition and combustion process; ignite the igniter: point the igniter nozzle upwards, adjust the flame height to 15-20 mm, ignite at the upper end of the sample, and after the upper end of the sample is completely ignited (the ignition time should be controlled within 10-15 seconds), remove the igniter, and immediately start measuring the afterburning and smoldering time, and then measure the damaged length; Determination of initial concentration: take any interval as a variable, and conduct the test according to the "up-down method"; the sample is ignited If the sample extinguishes itself immediately after ignition, continues to burn, smolders, or continues to burn and smolder for less than 2 minutes, or the damaged length is less than 40 mm, the oxygen concentration is too low, and the reaction symbol is recorded as "○", then the oxygen concentration must be increased; if the sample continues to burn, smolders, or continues to burn and smolder for more than 2 minutes, or the damaged length exceeds 40 mm, the oxygen concentration is too high, and the reaction symbol is recorded as "x", then the oxygen concentration must be reduced; until the difference between the two oxygen concentrations obtained is ≤1.0, one of which has a reaction symbol "○" and the other has a reaction symbol "x", and the reaction symbol of this pair of oxygen concentrations is the initial oxygen concentration (co); for the determination of the limiting oxygen concentration, use the initial oxygen concentration co, while keeping the oxygen concentration interval of d=0.2%, and measure a series of oxygen concentration values ​​and corresponding symbols, among which the last reaction symbol "○" or "x" is the exponential determination N, and continue to repeat the measurement of four more samples at an oxygen concentration interval of d=0.2%, and record the oxygen concentration of each time and its corresponding reaction number, and use the formula LOI=c F +Kd was used to calculate the limiting oxygen index of the four groups of fibers.

[0117] The limiting oxygen index of Examples 1 to 3 is between 24.1 and 25.5%, which is quite close to the 28% limiting oxygen index flame retardancy index of fiber products; the comparative example is around 17.3%. Since the higher the limiting oxygen index, the better the flame retardancy of the material, it can be determined that the flame retardancy of the fiber object treated by the process of this application is significantly improved.

[0118] In summary, it can be considered that the ultra-high molecular weight bulletproof heat-resistant flame-retardant fiber obtained by the preparation process of the present application has greatly improved flame retardancy and heat resistance, which meets the expected goals.

[0119] It should be noted that this specific embodiment is only an explanation of the present invention, and it is not a limitation of the present invention. After reading this specification, those skilled in the art can make non-creative modifications to this embodiment as needed, but as long as it is within the scope of the claims of the present invention, it is protected by the patent law.

Claims

1. A process for preparing ultra-high molecular weight heat-resistant flame-retardant fiber for bulletproof vests, characterized in that: The following steps are included: S1. Raw material processing: under anaerobic conditions, adding a catalyst and a compatibilizer to an ultra-high molecular weight polyethylene UHMWPE fiber stock solution, heating and mixing in an internal mixer for modification, and obtaining a modified UHMWPE stock solution; The carbon nano-atom CNPs material, phosphorus flame retardant, inorganic nano flame retardant particles, nitrogen flame retardant, polycarbonate and nano boron particles are mixed and ground, added into quaternary ammonium salt ionic liquid and mixed evenly to obtain an additive slurry; The modified UHMWPE stock solution and the auxiliary agent slurry are mixed in a ratio of 24 to 30:1 and allowed to stand to obtain a spinning stock solution; S2, melt spinning: the spinning solution is heated to a molten state, enters the spinning machine through a screw extruder, and is extruded from a metering pump spinneret to form continuous molten fibers; S3, cooling and stretching: the extruded molten fiber is rapidly cooled and solidified in a water bath, and stretched by a stretching machine to obtain modified UHMWPE fiber I; S4, post-treatment: performing relaxation treatment on the stretched modified UHMWPE fiber to obtain modified UHMWPE fiber II; S5. Material compounding: immersing the treated modified UHMWPE fiber II in a sedimentation tank filled with aqueous polyurethane WUP liquid to obtain modified UHMWPE fiber III; The modified UHMWPE fiber III is evenly laid on the support film by a fiber winding machine to form a parallel and straightly arranged single UD structure UHMWPE fiber IV; The UHMWPE fiber IV is compounded into a 2UD structured ultra-high molecular weight bulletproof heat-resistant and flame-retardant fiber by an equipment in an orthogonal stacking manner; S6. Product testing and delivery.

2. The process for preparing the ultra-high molecular weight heat-resistant and flame-retardant fiber for bulletproof vests according to claim 1, characterized in that: In step S1, the catalyst is prepared by mixing polyethylene oxide, xylene, triethylamine and acyl bromide in a ratio of 1:4.9:2:0.7 in a water bath at 80°C.

3. The process for preparing the ultra-high molecular weight heat-resistant and flame-retardant fiber for bulletproof vests according to claim 1, characterized in that: In step S1, the compatibilizer is prepared by reacting copper sulfate, potassium bromide, sodium tripolyphosphate and anisole in a ratio of 1:1:0.2:17 at a temperature not lower than 75° C. for 8 to 10 hours under a vacuum environment.

4. The process for preparing the ultra-high molecular weight heat-resistant and flame-retardant fiber for bulletproof vests according to claim 1, characterized in that: In step S1, the internal mixer is mixed for 2 to 3 hours at a speed of 50 to 215 r / min, an effective internal mixing volume of not less than 150 L, and a pressure of 0.6 to 0.8 MPa.

5. The process for preparing the ultra-high molecular weight heat-resistant and flame-retardant fiber for bulletproof vests according to claim 1, characterized in that: In step S1, the carbon nanoatom CNPs material is nanocarbon spheres; The phosphorus-based flame retardant is one or more of phosphate, phosphite, and phosphonate; The inorganic nano flame retardant particles are fumed silica inorganic nano particles; The nitrogen flame retardant is one or more of melamine MA, polynitrogen flame retardant melamine phosphate MPP, and melamine cyanurate MCA; The quaternary ammonium salt ionic liquid is one or more of 1-ethylpyridinium bromide solution, 1-butyl-3-methylimidazole solution, and 1-butylpyridinium chloride solution.

6. The process for preparing the ultra-high molecular weight heat-resistant and flame-retardant fiber for bulletproof vests according to claim 5, characterized in that: The formula of the additive slurry is calculated by weight: 10-13 parts of carbon nano-atom CNPs material, 5-8 parts of phosphorus flame retardant, 2-5 parts of inorganic nano flame retardant particles, 3-6 parts of nitrogen flame retardant, 1-2 parts of polycarbonate, 0.4-1.5 parts of nano boron particles, and 22-36 parts of quaternary ammonium salt ionic liquid.

7. The process for preparing the ultra-high molecular weight heat-resistant and flame-retardant fiber for bulletproof vests according to claim 1, characterized in that: The molecular weight of the ultra-high molecular weight polyethylene UHMWPE fiber stock solution in step S1 is not less than 3.5 million.

8. The process for preparing the ultra-high molecular weight heat-resistant and flame-retardant fiber for bulletproof vests according to claim 1, characterized in that: In step S4, a relaxation treatment is performed by heat setting.

9. The process for preparing the ultra-high molecular weight heat-resistant and flame-retardant fiber for bulletproof vests according to claim 1, characterized in that: In step S5, the modified UHMWPE fiber III is firstly passed through an extractor to remove excess chemical reagents on the surface and then wound and laid flat.

10. The process for preparing the ultra-high molecular weight heat-resistant and flame-retardant fiber for bulletproof vests according to claim 1, characterized in that: In step S5, in order to facilitate the wetting of the modified UHMWPE fiber II, the aqueous polyurethane WUP stock solution is diluted with deionized water in a mass ratio of 1:1 to 1.2 in advance to obtain an aqueous polyurethane WUP stock solution.