Neuron-like bionic structure nanofiber electrode material and preparation method and application thereof
By introducing nanofiber electrode materials with bionic structures like neurons into lithium-ion batteries, the problems of insufficient rigidity and energy density of traditional electrode materials are solved, the development of high-performance flexible batteries is achieved, and electron/ion transmission efficiency and cycle stability are improved. sex.
Patent Information
- Application Number
- CN202411199978.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-06
AI Technical Summary
The mechanical rigidity of traditional lithium-ion battery electrode materials cannot meet the needs of flexible products, and the energy density of carbon nanofibers is insufficient, which limits the improvement of the energy density and power density of lithium-ion batteries.
By introducing two-dimensional metal organic frame materials into polymer nanofibers, nanofiber electrode materials with bionic structures with neurons are prepared by electrospinning technology, combining high-temperature carbonization and low-temperature oxidation treatment to form nanosegments with one-dimensional and two-dimensional structures connected to each other. Fiber electrode material.
Significantly improves electron/ion transmission efficiency and volumetric strain capability, provides high capacity and cycling stability, suitable for applications of flexible energy storage devices, surpassing the performance of commercial graphite anodes.
Smart Images

Figure CN119082937A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of nanomaterials, and in particular relates to a nanofiber electrode material with a neuron-like bionic structure, a preparation method and an application thereof. Background Art
[0002] Lithium-ion batteries have the advantages of high output voltage, high energy density, long cycle life, safety and pollution-free. As the mainstream electrochemical energy storage product in the current market, they are still the core devices for the development of energy storage technology in the future. Further promote the safe service of lithium-ion batteries and steadily improve their energy density and power density in use. It is crucial to accelerate the transformation of my country's energy structure, develop and utilize renewable clean energy, and achieve the dual carbon goals. Electrode materials are one of the key components of lithium-ion batteries. Commercial graphite negative electrodes that have reached their theoretical limits are difficult to meet the requirements of the new era. Traditional energy storage devices generally have mechanical rigidity and cannot meet the practical needs of social development for wearable flexible products. Therefore, the development and utilization of lightweight carbon-based fiber electrode materials is a research field with great potential.
[0003] The one-dimensional nanofiber nonwoven membrane produced based on electrospinning technology is very important for promoting the development of the field of flexible self-supporting electrode materials. At present, it is urgent to break the current situation of insufficient intrinsic energy density of carbon nanofibers. The electrochemical performance of the material can be significantly improved through component compounding and structural design. Thanks to the unique structure and surface state of graphene, the two-dimensional structure exhibits structural advantages such as rich reactive active sites, fast ion diffusion kinetics, excellent electron transport characteristics and unique anisotropic mechanical properties in energy storage applications, making it an ideal functional unit for constructing composite materials. Therefore, it is very important to effectively construct a two-dimensional morphology in nanofibers in order to develop a structurally integrated fiber electrode with both one-dimensional and two-dimensional morphologies to promote the development of flexible energy storage devices. Summary of the invention
[0004] The purpose of the present invention is to provide a nanofiber electrode material with a neuron-like bionic structure and a preparation method thereof. Through the radial expansion behavior of the two-dimensional material in the polymer nanofiber, a lithium-ion battery anode self-supporting electrode material with interconnected one-dimensional and two-dimensional structures is prepared, which can meet the application and development needs in the field of energy storage batteries.
[0005] For the above purpose, the neuron-like bionic structure nanofiber electrode material of the present invention is prepared by the following method:
[0006] Step 1: adding dimethylformamide to polyacrylonitrile powder to form a polyacrylonitrile solution; adding a two-dimensional metal organic framework material to the polyacrylonitrile solution, stirring and dispersing the mixture evenly to obtain an electrospinning precursor solution;
[0007] Step 2: electrospinning the electrospinning precursor solution obtained in step 1 to obtain neuron-like bionic structure polymer nanofibers;
[0008] Step 3: The polymer nanofibers obtained in step 2 are subjected to high-temperature carbonization and low-temperature oxidation treatments in sequence to obtain a neuron-like bionic structure nanofiber electrode material.
[0009] In the above step 1, the two-dimensional metal organic framework material is prepared by the following method: adding transition metal salt and terephthalic acid to a mixed solvent of dimethylformamide, anhydrous ethanol and deionized water, and dissolving by ultrasonication to obtain a clear mixed solution; rapidly injecting triethylamine into the mixed solution, and ultrasonically reacting at 0 to 20°C for 5 to 10 hours under sealed conditions to obtain a two-dimensional metal organic framework material. Preferably, the concentration of the transition metal salt in the mixed solution is 0.015 to 0.025 mol L -1 The molar ratio of the transition metal salt to terephthalic acid is 1:0.5-2, the volume ratio of dimethylformamide, anhydrous ethanol and deionized water in the mixed solvent is 16:1:1, and the volume ratio of triethylamine to the mixed solution is 1:40-50. It is further preferred that the transition metal salt is one or both of cobalt chloride and nickel chloride.
[0010] In the above step 1, the concentration of the polyacrylonitrile solution is preferably 0.05 to 0.1 g mL -1 The mass ratio of the two-dimensional metal organic framework material to polyacrylonitrile is 1:1 to 4.
[0011] In the above step 2, the electrospinning parameters are preferably set as follows: voltage of 10-20 kV, propulsion speed of 0.1-1 mL h -1 , the receiving distance is 10 to 20 cm.
[0012] In the above step 3, the conditions for the high temperature carbonization are preferably: in an argon atmosphere or a nitrogen atmosphere, keeping warm at 260-290° C. for 1-4 hours, and then keeping warm at 600-800° C. for 1-4 hours.
[0013] In the above step 3, the conditions of the low-temperature oxidation treatment are preferably: keeping warm at 280-330° C. for 1-3 hours in an air atmosphere.
[0014] The present invention also provides the application of the above-mentioned neuron-like bionic structure nanofiber electrode material directly as a self-supporting electrode anode material in a lithium ion battery.
[0015] Compared with the prior art, the present invention has the following beneficial effects:
[0016] 1. The present invention uses transition metal salts and terephthalic acid organic ligands as raw materials, and uses the method of ultrasonic reaction growth to obtain a two-dimensional metal organic framework material; the obtained two-dimensional metal organic framework material is dispersed in a spinning solution (polyacrylonitrile solution) as a morphological initiator, and in the process of electrospinning to prepare polymer nanofibers, the two-dimensional metal organic framework material is radially expanded in the one-dimensional polymer nanofiber, thereby preparing a neuron-like bionic structure polymer nanofiber material with a one-dimensional and two-dimensional structure interconnected. The above-mentioned fiber material is subjected to high-temperature carbonization and low-temperature oxidation treatment, and finally a nanofiber electrode material with a neuron-like bionic structure is prepared. The preparation method is simple and economical, and the raw materials used are cheap and easy to obtain, which is suitable for industrial-scale mass production.
[0017] 2. The nanofiber electrode material of the present invention has a neuron-like bionic structure, which is formed by interconnecting one-dimensional and two-dimensional structures. The one-dimensional structure in the electrode material serves as the basic skeleton and transmission path, and the two-dimensional structure provides metal active centers. This material structure effectively improves the electron / ion transmission efficiency and volume strain capacity during the material energy storage process. Compared with the graphite anode used in commercial lithium-ion batteries, the neuron-like bionic structure nanofiber electrode material of the present invention has the advantage of being directly used as a self-supporting electrode, and exhibits good capacity and cycle stability, which is of reference significance for the development of a new generation of high-performance flexible batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 These are low-magnification and high-magnification SEM images of the two-dimensional metal-organic framework material prepared in Example 1.
[0019] Figure 2 This is the XRD pattern of the two-dimensional metal organic framework material prepared in Example 1.
[0020] Figure 3 This is a low-magnification SEM image of the neuron-like bionic structure polymer nanofiber prepared in Example 1.
[0021] Figure 4 This is a low-magnification SEM image of the neuron-like bionic structure carbon nanofiber prepared in Example 1.
[0022] Figure 5 These are low-magnification and high-magnification SEM images of the neuron-like bionic structure nanofiber electrode material prepared in Example 1.
[0023] Figure 6 These are the TEM and SADE images of the neuron-like bionic structure nanofiber electrode material prepared in Example 1.
[0024] Figure 7 This is the XRD diagram of the neuron-like bionic structure nanofiber electrode material prepared in Example 1.
[0025] Figure 8 This is a low-magnification SEM image of the neuron-like bionic structure nanofiber electrode material prepared in Example 2.
[0026] Fig. 9 This is a low-magnification SEM image of the neuron-like bionic structure nanofiber electrode material prepared in Example 3.
[0027] Fig.10 These are optical photographs of the self-supporting electrode slices of the neuron-like bionic structure nanofiber electrode material prepared in Example 1 and its different bending states.
[0028] Fig.11 The neuron-like bionic structure nanofiber electrode material prepared in Example 1 is directly used as a self-supporting electrode anode and a button battery half-cell assembled with a counter electrode metal lithium at 100 mA g -1 Cycling performance diagram at different current densities. DETAILED DESCRIPTION
[0029] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments, but the protection scope of the present invention is not limited to these embodiments.
[0030] Example 1
[0031] Step 1: Measure 32 mL of dimethylformamide, 2 mL of anhydrous ethanol and 2 mL of deionized water, stir and mix to obtain a mixed solvent, add 0.0892 g (0.375 mmol) of CoCl2·6H2O, 0.0891 g (0.375 mmol) of NiCl2·6H2O and 0.1246 g (0.75 mmol) of terephthalic acid to the mixed solvent, ultrasonically treat to fully dissolve, add 0.8 mL of triethylamine, and ultrasonically react at 0°C for 8 h under sealed conditions. After the reaction is complete, centrifuge and dry to obtain a light pink solid powder, i.e., a two-dimensional metal organic framework material. Figure 1 It can be seen that the obtained material is a two-dimensional ultra-thin sheet, and the edges of the nanosheets curl spontaneously during drying. Figure 2 It can be seen that the XRD results of the material are consistent with the crystal simulation diffraction results, indicating the successful preparation of the two-dimensional metal organic framework material. 0.4g of polyacrylonitrile powder was added to 5mL of dimethylformamide and stirred evenly to form a polyacrylonitrile solution; 0.2g of the two-dimensional metal organic framework material was added to the obtained polyacrylonitrile solution, stirred and dispersed evenly, and an electrospinning precursor solution was obtained.
[0032] Step 2: The electrospinning precursor solution obtained in step 1 was electrospun. The electrospinning parameters were: voltage of 15 kV, propulsion speed of 0.5 mL h -1 , the receiving distance is 15cm, and the neuron-like bionic structure polymer nanofiber is obtained. Figure 3 It can be seen that the obtained polymer nanofibers have a morphology in which one-dimensional and two-dimensional structures are interconnected, indicating the successful synthesis of neuron-like bionic structure polymer nanofibers.
[0033] Step 3: In an argon atmosphere, the neuron-like bionic structure polymer nanofibers obtained in step 2 are kept at 280°C for 2 hours, and then heated to 600°C for 2 hours to obtain neuron-like bionic structure carbon nanofibers. Figure 4 It can be seen that after high-temperature carbonization treatment, the size of the polymer nanofibers shrinks radially, while the radially expanded two-dimensional units shrink to a lesser extent, so that the obtained carbon nanofibers maintain the neuron-like bionic structure of the initial polymer. Subsequently, oxidation at 330°C in an air atmosphere for 2h obtained a neuron-like bionic structure nanofiber electrode material. Figure 5 The medium and low magnification SEM images show that the neuron-like structured nanofibers interweave with each other to form a three-dimensional network structure, and the high magnification SEM images show that the ultrafine active metal species derived from the metal organic framework in the two-dimensional unit are dispersed in the derived carbon material. Figure 6 It can be seen from the TEM that the low-temperature oxidation treatment causes the metal nanoparticles to produce the Kirkendall effect and form hollow nanoparticles. Figure 6 The SADE shows the diffraction rings of metal oxides and Figure 7 The presence of characteristic peaks corresponding to metal oxides in the XRD indicates that neuron-like bionic structure nanofiber electrode materials with active metal species were successfully prepared after low-temperature oxidation treatment.
[0034] Example 2
[0035] Step 1: Add 0.4 g of polyacrylonitrile powder to 5 mL of dimethylformamide and stir evenly to form a polyacrylonitrile solution; add 0.1 g of two-dimensional metal organic framework material to the obtained polyacrylonitrile solution, stir and disperse evenly to obtain an electrospinning precursor solution.
[0036] Step 2: The electrospinning precursor solution obtained in step 1 was electrospun. The electrospinning parameters were: voltage of 15 kV, propulsion speed of 0.5 mL h -1 , the receiving distance is 15cm, and neuron-like bionic structure polymer nanofibers are obtained.
[0037] Step 3: In an argon atmosphere, the neuron-like bionic structure polymer nanofiber obtained in step 2 is kept at 280° C. for 2 h, then heated to 600° C. for 2 h, and then oxidized at 330° C. for 2 h in an air atmosphere to obtain a neuron-like bionic structure nanofiber electrode material, such as Figure 8 shown.
[0038] Example 3
[0039] Step 1: Add 0.4 g of polyacrylonitrile powder to 5 mL of dimethylformamide and stir evenly to form a polyacrylonitrile solution; add 0.4 g of two-dimensional metal organic framework material to the obtained polyacrylonitrile solution, stir and disperse evenly to obtain an electrospinning precursor solution.
[0040] Step 2: The electrospinning precursor solution obtained in step 1 was electrospun. The electrospinning parameters were: voltage of 15 kV, propulsion speed of 0.5 mL h -1 , the receiving distance is 15cm, and neuron-like bionic structure polymer nanofibers are obtained.
[0041] Step 3: In an argon atmosphere, the neuron-like bionic structure polymer nanofiber obtained in step 2 is kept at 280° C. for 2 h, then heated to 600° C. for 2 h, and then oxidized at 330° C. for 2 h in an air atmosphere to obtain a neuron-like bionic structure nanofiber electrode material, such as Fig. 9 shown.
[0042] Application Example 1
[0043] In order to demonstrate the beneficial effects of the present invention, the neuron-like bionic structure nanofiber electrode material prepared in Example 1 was used as the anode directly as a self-supporting electrode (with a loading mass of 2 mg). Fig.10 The following are optical photographs of the self-supporting electrode slice of the neuron-like bionic structure nanofiber electrode material prepared in Example 1 and its different bending states. The self-supporting electrode slice and the counter electrode metal lithium sheet were assembled into a button battery in a glove box to construct a two-electrode sealed half-cell system (bionic structure nanofiber electrode material||metal lithium). The assembled button battery was tested for charge and discharge performance on the Xinwei battery test system: In the battery cycle test, the current density was controlled at 100mA g -1 , the results are shown in Fig.11 .Depend on Fig.11 It can be seen that after 120 cycles of charge and discharge, the reversible capacity of the battery can still be maintained at 794.5 mAh g -1 , which is much better than the capacity of commercial graphite anode (372.0 mAh g -1 ), which can well meet the new demands of the current society for flexible energy storage devices.
Claims
1. A method for preparing a neuron-like bionic structure nanofiber electrode material, characterized in that: The preparation method comprises the following steps: Step 1: adding dimethylformamide to polyacrylonitrile powder to form a polyacrylonitrile solution; adding a two-dimensional metal organic framework material to the polyacrylonitrile solution, stirring and dispersing the mixture evenly to obtain an electrospinning precursor solution; Step 2: electrospinning the electrospinning precursor solution obtained in step 1 to obtain neuron-like bionic structure polymer nanofibers; Step 3: The polymer nanofibers obtained in step 2 are subjected to high-temperature carbonization and low-temperature oxidation treatments in sequence to obtain a neuron-like bionic structure nanofiber electrode material.
2. The method for preparing the neuron-like bionic structure nanofiber electrode material according to claim 1, characterized in that: In step 1, the two-dimensional metal organic framework material is prepared by the following method: adding transition metal salt and terephthalic acid to a mixed solvent of dimethylformamide, anhydrous ethanol and deionized water, and obtaining a clear mixed solution after ultrasonic dissolution; quickly injecting triethylamine into the mixed solution, and ultrasonically reacting at 0-20°C for 5-10 hours under sealed conditions to obtain a two-dimensional metal organic framework material.
3. The method for preparing the neuron-like bionic structure nanofiber electrode material according to claim 2, characterized in that: The concentration of the transition metal salt in the mixed solution is 0.015 to 0.025 mol L -1 The molar ratio of the transition metal salt to terephthalic acid is 1:0.5-2, and the transition metal salt is one or both of cobalt chloride and nickel chloride.
4. The method for preparing the neuron-like bionic structure nanofiber electrode material according to claim 2, characterized in that: The volume ratio of dimethylformamide, anhydrous ethanol and deionized water in the mixed solvent is 16:1:1, and the volume ratio of triethylamine to the mixed solution is 1:40-50.
5. The method for preparing the neuron-like bionic structure nanofiber electrode material according to claim 1, characterized in that: In step 1, the concentration of the polyacrylonitrile solution is 0.05-0.1 g mL -1 The mass ratio of the two-dimensional metal organic framework material to polyacrylonitrile is 1:1 to 4.
6. The method for preparing the neuron-like bionic structure nanofiber electrode material according to claim 1, characterized in that: In step 2, the electrospinning parameters are: voltage of 10-20 kV, propulsion speed of 0.1-1 mL h -1 , the receiving distance is 10 to 20 cm.
7. The method for preparing the neuron-like bionic structure nanofiber electrode material according to claim 1, characterized in that: In step 3, the high temperature carbonization conditions are: in an argon atmosphere or a nitrogen atmosphere, keeping warm at 260-290° C. for 1-4 hours, and then keeping warm at 600-800° C. for 1-4 hours.
8. The method for preparing the neuron-like bionic structure nanofiber electrode material according to claim 1, characterized in that: In step 3, the conditions for the low-temperature oxidation treatment are: keeping warm at 280-330° C. for 1-3 hours in an air atmosphere.
9. The neuron-like bionic structure nanofiber electrode material prepared by any one of the preparation methods of claims 1 to 8.
10. The neuron-like bionic structure nanofiber electrode material according to claim 9 is directly used as a self-supporting electrode anode material in a lithium-ion battery.