Heat-resistant and flame-retardant polylactic acid fiber cloth and preparation method thereof

By introducing coated nanomagnesium hydroxide into polylactic fibers and using cross-network and hydrotunneling entanglement processes, a thermally resistant and flame-resistant polylactic fiber cloth was prepared, which solved the problem of insufficient heat resistance of polylactic fiber cloth. It has achieved widespread application in the field of high temperature and the maintenance of environmental protection performance.

CN119083030APending Publication Date: 2024-12-06HANGZHOU GAOJIAN EXHIBITION DECORATION ENGINEERING CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411414976.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-11
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing polylactic fiber cloth has poor heat resistance, which limits its application in the field of high temperature.

Method used

The modified polylactic fiber is used to pass the cross-meshing and hydrotunneling entanglement process, and the coated nanomagnesium hydroxide is introduced into the fibers, and a heat-resistant and flame-resistant polylactic fiber cloth is prepared by drying and spinning technology.

Benefits of technology

It significantly improves the heat resistance and flame retardant properties of polylactic fiber cloth, broadens its application range in the high temperature field, while maintaining its degradable and environmentally friendly properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention relates to the technical field of fibers, in particular to heat-resistant and flame-retardant polylactic acid fiber cloth and a preparation method thereof.The heat-resistant and flame-retardant polylactic acid fiber cloth is obtained by conducting cross netting and spunlace entanglement on modified polylactic acid fibers and finally conducting drying; the thickness of the heat-resistant and flame-retardant polylactic acid fiber cloth is 0.4 to 1.0 mm; the unit mass of the heat-resistant flame-retardant polylactic acid is 60-70g / m < 2 >; the prepared polylactic acid fiber cloth has excellent heat resistance and flame retardance, and the application range of the polylactic acid fiber cloth in the high-temperature field can be widened. The polylactic acid fiber cloth disclosed by the invention can be decomposed into carbon dioxide and water in soil or seawater under the action of microorganisms due to the degradability of the polylactic acid fiber, does not emit toxic gas or cause pollution during combustion, conforms to the current sustainable development strategy, and is green and environment-friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fibers, in particular to a heat-resistant and flame-retardant polylactic acid fiber cloth and a preparation method thereof. Background Art

[0002] Polylactic acid fiber is made from starch-containing agricultural products such as corn, wheat, and beets. After fermentation to generate lactic acid, it is then polycondensed and melt-spun. Polylactic acid fiber is a synthetic fiber that is easy to grow and can be naturally degraded in nature. It can be decomposed into carbon dioxide and water by microorganisms in soil or seawater. When burned, it does not emit toxic gases or cause pollution. It is a sustainable ecological fiber.

[0003] Polylactic acid fiber cloth, as an emerging environmentally friendly material, has attracted much attention in the textile industry in recent years. Polylactic acid fiber cloth can be widely used in many fields:

[0004] Garment industry: used to make underwear, outerwear, sportswear, shirts and other types of clothing. In particular, its softness, wrinkle resistance and antibacterial properties make polylactic acid fiber very suitable for the production of high-end clothing fabrics and sports and leisure clothing.

[0005] Household items: such as carpets, sofa covers, curtains, towels and other decorative textiles, as well as bedding, etc. The natural and clean appearance and elegant texture of polylactic acid fiber make it very popular in the home furnishing market.

[0006] Medical field: Due to its good biocompatibility and degradability, polylactic acid fiber is widely used in the production of medical devices such as surgical sutures, dressings and tissue engineering scaffolds.

[0007] Other areas: including construction materials (such as ground cover reinforcement materials), agricultural products (such as nets and non-woven fabrics for planting), fishery products (such as fish nets and kelp farming nets) and materials for the paper industry.

[0008] However, the heat resistance of the polylactic acid fiber cloth prepared by the prior art is relatively poor, which limits its further application.

[0009] Based on this, the present invention provides a heat-resistant and flame-retardant polylactic acid fiber cloth to solve the corresponding problem. Summary of the invention

[0010] In view of the problems in the prior art, the present invention provides a heat-resistant and flame-retardant polylactic acid fiber cloth and a preparation method thereof.

[0011] The technical solution adopted by the present invention to solve the technical problem is: a method for preparing heat-resistant and flame-retardant polylactic acid fiber cloth, wherein the modified polylactic acid fibers are cross-webbed, hydroentangled and finally dried to obtain the heat-resistant and flame-retardant polylactic acid fiber cloth;

[0012] The thickness of the heat-resistant and flame-retardant polylactic acid fiber cloth is 0.4-1.0 mm;

[0013] The unit mass of the heat-resistant flame-retardant polylactic acid is 60-70 g / m 2 .

[0014] As a further technical solution: the modified polylactic acid fiber preparation method is:

[0015] S1. Weigh by weight: 80-85 parts of polylactic acid resin, 1-2 parts of stearic acid, 10-12 parts of calcium carbonate, and 6-10 parts of coated nano magnesium hydroxide;

[0016] S2, adding polylactic acid resin, stearic acid, calcium carbonate, and coated nano magnesium hydroxide into a blender in order, and mixing them evenly to obtain a mixture;

[0017] S3, adding the mixed material into a drying oven, and subjecting it to drying treatment to obtain a dry mixed material;

[0018] S4, adding the dry mixed material into a twin-screw extruder, subjecting it to melt extrusion, and then spinning it through a spinneret to obtain polylactic acid fibers.

[0019] As a further technical solution: the preparation method of the coated nano magnesium hydroxide is:

[0020] First, magnesium chloride is added to deionized water, and stirred to mix evenly to obtain a magnesium chloride solution;

[0021] Add anhydrous ethanol to the magnesium chloride solution, continue stirring and mixing to obtain a magnesium chloride ethanol solution;

[0022] Acrylic acid was added to the magnesium chloride ethanol solution, the temperature was adjusted to 15°C, stirred for 30 minutes, then ammonia water was added dropwise, stirring was continued for 2 hours, sodium hydroxide solution was added dropwise, stirring was continued for 2 hours, the temperature was adjusted to 55°C, kept warm for 4 hours, filtered and dried to obtain coated nano magnesium hydroxide.

[0023] As a further technical solution: the mass fraction of the magnesium chloride solution is 3-4%;

[0024] The volume ratio of the anhydrous ethanol to deionized water is 1:1.

[0025] As a further technical solution: the volume ratio of the acrylic acid to the magnesium chloride ethanol solution is 1:20-22;

[0026] The mass fraction of ammonia water is 5%, and the volume ratio of ammonia water to deionized water is 1.2-1.4:1;

[0027] The mass fraction of sodium hydroxide solution is 2%;

[0028] The volume ratio of sodium hydroxide solution to ammonia water is 2.5-2.8:1;

[0029] The drying temperature was 80°C and the drying time was 10 hours.

[0030] As a further technical solution: the hydroentanglement is formed by using water needles, through which a fine water flow with a pressure of 6-8 MPa passes through a water spray plate with a micropore diameter of 0.2-0.5 mm.

[0031] As a further technical solution: the drying is carried out at a temperature of 75-80°C.

[0032] As a further technical solution: the drying time is 20-22 hours.

[0033] A method for preparing heat-resistant and flame-retardant polylactic acid fiber cloth obtains the heat-resistant and flame-retardant polylactic acid fiber cloth.

[0034] Beneficial effects of the present invention:

[0035] The polylactic acid fiber cloth prepared by the present invention has excellent heat resistance and flame retardancy, and can broaden the application of the polylactic acid fiber cloth in high temperature fields.

[0036] The polylactic acid fiber cloth of the present invention is degradable and can be decomposed into carbon dioxide and water by microorganisms in soil or seawater. It does not emit toxic gas or cause pollution when burned, and is in line with the contemporary sustainable development strategy and is green and environmentally friendly.

[0037] The present invention introduces the prepared coated nano magnesium hydroxide, which can undergo a decomposition reaction when heated, usually within the range of 340-490° C. This process absorbs a large amount of latent heat, and the absorbed heat helps to reduce the temperature of the surface of the polylactic acid fiber cloth, thereby slowing down or preventing further combustion of the polylactic acid fiber cloth material, thereby greatly improving the heat resistance and flame retardancy of the prepared polylactic acid fiber cloth.

[0038] At the same time, compared with conventional magnesium hydroxide flame retardants, the present invention adopts a specially coated nano magnesium hydroxide, which will produce water vapor during the decomposition process under heat. Due to the coating effect, the slow and continuous release of water vapor not only helps to reduce the oxygen concentration around the polylactic acid fiber cloth, but also can form a barrier through the diffusion effect of the continuously generated steam, hindering the direct contact between oxygen and the polylactic acid fiber cloth, thereby inhibiting the combustion.

[0039] The coated magnesium oxide produced after high-temperature decomposition will adhere to the polylactic acid fiber cloth. This layer attached to the surface of the polylactic acid fiber cloth can isolate the transfer of air and heat, and can prevent the occurrence of smoldering. At the same time, the produced magnesium oxide can also continuously absorb incompletely burned molten residues, which helps to eliminate smoke and prevent the formation of molten droplets. DETAILED DESCRIPTION

[0040] In order to enable those skilled in the art to better understand the present application, the technical solutions in the embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without creative work should fall within the scope of protection of the present application.

[0041] Example 1

[0042] A method for preparing a heat-resistant and flame-retardant polylactic acid fiber cloth, wherein modified polylactic acid fibers are cross-webbed, hydroentangled, and finally dried to obtain the heat-resistant and flame-retardant polylactic acid fiber cloth;

[0043] The thickness of the heat-resistant and flame-retardant polylactic acid fiber cloth is 0.5 mm;

[0044] The unit mass of the heat-resistant flame-retardant polylactic acid is 62 g / m 2 The hydroentanglement is formed by using water needles, where a fine water flow with a pressure of 6.5 MPa passes through a water jet plate with a micropore diameter of 0.5 mm.

[0045] The drying is carried out at a temperature of 75°C; the drying time is 20 hours; the preparation method of the modified polylactic acid fiber is:

[0046] S1. Weigh by weight: 80 parts of polylactic acid resin, 1 part of stearic acid, 10 parts of calcium carbonate, and 6 parts of coated nano magnesium hydroxide;

[0047] S2, adding polylactic acid resin, stearic acid, calcium carbonate, and coated nano magnesium hydroxide into a blender in order, and mixing them evenly to obtain a mixture;

[0048] S3, adding the mixed material into a drying oven, and subjecting it to drying treatment to obtain a dry mixed material;

[0049] S4, adding the dry mixed material into a twin-screw extruder, subjecting it to melt extrusion, and then spinning it through a spinneret to obtain polylactic acid fibers.

[0050] The preparation method of coated nano magnesium hydroxide is as follows:

[0051] First, magnesium chloride is added to deionized water, and stirred to mix evenly to obtain a magnesium chloride solution;

[0052] Add anhydrous ethanol to the magnesium chloride solution, continue stirring and mixing to obtain a magnesium chloride ethanol solution;

[0053] Acrylic acid was added to the magnesium chloride ethanol solution, the temperature was adjusted to 15°C, stirred for 30 minutes, then ammonia water was added dropwise, stirring was continued for 2 hours, sodium hydroxide solution was added dropwise, stirring was continued for 2 hours, the temperature was adjusted to 55°C, kept warm for 4 hours, filtered and dried to obtain coated nano magnesium hydroxide.

[0054] The mass fraction of magnesium chloride solution is 3%;

[0055] The volume ratio of the anhydrous ethanol to deionized water is 1:1.

[0056] The volume ratio of the acrylic acid to the magnesium chloride ethanol solution is 1:20;

[0057] The mass fraction of ammonia water is 5%, and the volume ratio of ammonia water to deionized water is 1.2:1;

[0058] The mass fraction of sodium hydroxide solution is 2%;

[0059] The volume ratio of sodium hydroxide solution to ammonia water is 2.5:1;

[0060] The drying temperature was 80°C and the drying time was 10 hours.

[0061] Example 2

[0062] A method for preparing a heat-resistant and flame-retardant polylactic acid fiber cloth, wherein modified polylactic acid fibers are cross-webbed, hydroentangled, and finally dried to obtain the heat-resistant and flame-retardant polylactic acid fiber cloth;

[0063] The thickness of the heat-resistant and flame-retardant polylactic acid fiber cloth is 0.5 mm;

[0064] The unit mass of the heat-resistant flame-retardant polylactic acid is 66 g / m 2 The hydroentanglement is formed by using water needles, where a fine water flow with a pressure of 6.5 MPa passes through a water jet plate with a micropore diameter of 0.5 mm.

[0065] The drying is carried out at a temperature of 78°C; the drying time is 21 hours; the preparation method of the modified polylactic acid fiber is:

[0066] S1. Weigh by weight: 82 parts of polylactic acid resin, 1.5 parts of stearic acid, 11 parts of calcium carbonate, and 7 parts of coated nano magnesium hydroxide;

[0067] S2, adding polylactic acid resin, stearic acid, calcium carbonate, and coated nano magnesium hydroxide into a blender in order, and mixing them evenly to obtain a mixture;

[0068] S3, adding the mixed material into a drying oven, and subjecting it to drying treatment to obtain a dry mixed material;

[0069] S4, adding the dry mixed material into a twin-screw extruder, subjecting it to melt extrusion, and then spinning it through a spinneret to obtain polylactic acid fibers.

[0070] The preparation method of coated nano magnesium hydroxide is as follows:

[0071] First, magnesium chloride is added to deionized water, and stirred to mix evenly to obtain a magnesium chloride solution;

[0072] Add anhydrous ethanol to the magnesium chloride solution, continue stirring and mixing to obtain a magnesium chloride ethanol solution;

[0073] Acrylic acid was added to the magnesium chloride ethanol solution, the temperature was adjusted to 15°C, stirred for 30 minutes, then ammonia water was added dropwise, stirring was continued for 2 hours, sodium hydroxide solution was added dropwise, stirring was continued for 2 hours, the temperature was adjusted to 55°C, kept warm for 4 hours, filtered and dried to obtain coated nano magnesium hydroxide.

[0074] The mass fraction of magnesium chloride solution is 3.2%;

[0075] The volume ratio of the anhydrous ethanol to deionized water is 1:1.

[0076] The volume ratio of the acrylic acid to the magnesium chloride ethanol solution is 1:21;

[0077] The mass fraction of ammonia water is 5%, and the volume ratio of ammonia water to deionized water is 1.25:1;

[0078] The mass fraction of sodium hydroxide solution is 2%;

[0079] The volume ratio of sodium hydroxide solution to ammonia water is 2.7:1;

[0080] The drying temperature was 80°C and the drying time was 10 hours.

[0081] Example 3

[0082] A method for preparing a heat-resistant and flame-retardant polylactic acid fiber cloth, wherein modified polylactic acid fibers are cross-webbed, hydroentangled, and finally dried to obtain the heat-resistant and flame-retardant polylactic acid fiber cloth;

[0083] The thickness of the heat-resistant and flame-retardant polylactic acid fiber cloth is 0.5 mm;

[0084] The unit mass of the heat-resistant flame-retardant polylactic acid is 68 g / m 2The hydroentanglement is formed by using water needles, where a fine water flow with a pressure of 7 MPa passes through a water jet plate with a micropore size of 0.5 mm.

[0085] The drying is carried out at a temperature of 78°C; the drying time is 21 hours; the preparation method of the modified polylactic acid fiber is:

[0086] S1. Weigh by weight: 84 parts of polylactic acid resin, 1.6 parts of stearic acid, 11 parts of calcium carbonate, and 8 parts of coated nano magnesium hydroxide;

[0087] S2, adding polylactic acid resin, stearic acid, calcium carbonate, and coated nano magnesium hydroxide into a blender in order, and mixing them evenly to obtain a mixture;

[0088] S3, adding the mixed material into a drying oven, and subjecting it to drying treatment to obtain a dry mixed material;

[0089] S4, adding the dry mixed material into a twin-screw extruder, subjecting it to melt extrusion, and then spinning it through a spinneret to obtain polylactic acid fibers.

[0090] The preparation method of coated nano magnesium hydroxide is as follows:

[0091] First, magnesium chloride is added to deionized water, and stirred to mix evenly to obtain a magnesium chloride solution;

[0092] Add anhydrous ethanol to the magnesium chloride solution, continue stirring and mixing to obtain a magnesium chloride ethanol solution;

[0093] Acrylic acid was added to the magnesium chloride ethanol solution, the temperature was adjusted to 15°C, stirred for 30 minutes, then ammonia water was added dropwise, stirring was continued for 2 hours, sodium hydroxide solution was added dropwise, stirring was continued for 2 hours, the temperature was adjusted to 55°C, kept warm for 4 hours, filtered and dried to obtain coated nano magnesium hydroxide.

[0094] The mass fraction of magnesium chloride solution is 3.8%;

[0095] The volume ratio of the anhydrous ethanol to deionized water is 1:1.

[0096] The volume ratio of the acrylic acid to the magnesium chloride ethanol solution is 1:21;

[0097] The mass fraction of ammonia water is 5%, and the volume ratio of ammonia water to deionized water is 1.3:1;

[0098] The mass fraction of sodium hydroxide solution is 2%;

[0099] The volume ratio of sodium hydroxide solution to ammonia water is 2.7:1;

[0100] The drying temperature was 80°C and the drying time was 10 hours.

[0101] Example 4

[0102] A method for preparing a heat-resistant and flame-retardant polylactic acid fiber cloth, wherein modified polylactic acid fibers are cross-webbed, hydroentangled, and finally dried to obtain the heat-resistant and flame-retardant polylactic acid fiber cloth;

[0103] The thickness of the heat-resistant and flame-retardant polylactic acid fiber cloth is 0.5 mm;

[0104] The unit mass of the heat-resistant flame-retardant polylactic acid is 69 g / m 2 The hydroentanglement is formed by using water needles, where a fine water flow with a pressure of 7.5 MPa passes through a water jet plate with a micropore diameter of 0.5 mm.

[0105] The drying is carried out at a temperature of 76°C; the drying time is 21 hours; the preparation method of the modified polylactic acid fiber is:

[0106] S1. Weigh by weight: 83 parts of polylactic acid resin, 1.5 parts of stearic acid, 11 parts of calcium carbonate, and 9 parts of coated nano magnesium hydroxide;

[0107] S2, adding polylactic acid resin, stearic acid, calcium carbonate, and coated nano magnesium hydroxide into a blender in order, and mixing them evenly to obtain a mixture;

[0108] S3, adding the mixed material into a drying oven, and subjecting it to drying treatment to obtain a dry mixed material;

[0109] S4, adding the dry mixed material into a twin-screw extruder, subjecting it to melt extrusion, and then spinning it through a spinneret to obtain polylactic acid fibers.

[0110] The preparation method of coated nano magnesium hydroxide is as follows:

[0111] First, magnesium chloride is added to deionized water, and stirred to mix evenly to obtain a magnesium chloride solution;

[0112] Add anhydrous ethanol to the magnesium chloride solution, continue stirring and mixing to obtain a magnesium chloride ethanol solution;

[0113] Acrylic acid was added to the magnesium chloride ethanol solution, the temperature was adjusted to 15°C, stirred for 30 minutes, then ammonia water was added dropwise, stirring was continued for 2 hours, sodium hydroxide solution was added dropwise, stirring was continued for 2 hours, the temperature was adjusted to 55°C, kept warm for 4 hours, filtered and dried to obtain coated nano magnesium hydroxide.

[0114] The mass fraction of magnesium chloride solution is 3.8%;

[0115] The volume ratio of the anhydrous ethanol to deionized water is 1:1.

[0116] The volume ratio of the acrylic acid to the magnesium chloride ethanol solution is 1:21;

[0117] The mass fraction of ammonia water is 5%, and the volume ratio of ammonia water to deionized water is 1.3:1;

[0118] The mass fraction of sodium hydroxide solution is 2%;

[0119] The volume ratio of sodium hydroxide solution to ammonia water is 2.7:1;

[0120] The drying temperature was 80°C and the drying time was 10 hours.

[0121] Example 5

[0122] A method for preparing a heat-resistant and flame-retardant polylactic acid fiber cloth, wherein modified polylactic acid fibers are cross-webbed, hydroentangled, and finally dried to obtain the heat-resistant and flame-retardant polylactic acid fiber cloth;

[0123] The thickness of the heat-resistant and flame-retardant polylactic acid fiber cloth is 0.5 mm;

[0124] The unit mass of the heat-resistant flame-retardant polylactic acid is 70 g / m 2 The hydroentanglement is formed by using water needles, where a fine water flow with a pressure of 8 MPa passes through a water jet plate with a micropore diameter of 0.5 mm.

[0125] The drying is carried out at a temperature of 80°C; the drying time is 22 hours; the preparation method of the modified polylactic acid fiber is:

[0126] S1. Weigh by weight: 85 parts of polylactic acid resin, 2 parts of stearic acid, 12 parts of calcium carbonate, and 10 parts of coated nano magnesium hydroxide;

[0127] S2, adding polylactic acid resin, stearic acid, calcium carbonate, and coated nano magnesium hydroxide into a blender in order, and mixing them evenly to obtain a mixture;

[0128] S3, adding the mixed material into a drying oven, and subjecting it to drying treatment to obtain a dry mixed material;

[0129] S4, adding the dry mixed material into a twin-screw extruder, subjecting it to melt extrusion, and then spinning it through a spinneret to obtain polylactic acid fibers.

[0130] The preparation method of coated nano magnesium hydroxide is as follows:

[0131] First, magnesium chloride is added to deionized water, and stirred to mix evenly to obtain a magnesium chloride solution;

[0132] Add anhydrous ethanol to the magnesium chloride solution, continue stirring and mixing to obtain a magnesium chloride ethanol solution;

[0133] Acrylic acid was added to the magnesium chloride ethanol solution, the temperature was adjusted to 15°C, stirred for 30 minutes, then ammonia water was added dropwise, stirring was continued for 2 hours, sodium hydroxide solution was added dropwise, stirring was continued for 2 hours, the temperature was adjusted to 55°C, kept warm for 4 hours, filtered and dried to obtain coated nano magnesium hydroxide.

[0134] The mass fraction of magnesium chloride solution is 4%;

[0135] The volume ratio of the anhydrous ethanol to deionized water is 1:1.

[0136] The volume ratio of the acrylic acid to the magnesium chloride ethanol solution is 1:22;

[0137] The mass fraction of ammonia water is 5%, and the volume ratio of ammonia water to deionized water is 1.4:1;

[0138] The mass fraction of sodium hydroxide solution is 2%;

[0139] The volume ratio of sodium hydroxide solution to ammonia water is 2.8:1;

[0140] The drying temperature was 80°C and the drying time was 10 hours.

[0141] Comparative Example 1:

[0142] Based on Example 1, no coated nano magnesium hydroxide is added to the polylactic acid fiber, and the rest of the technical solutions remain unchanged.

[0143] Comparative Example 2:

[0144] Based on Example 1, the coated nano magnesium hydroxide is replaced by conventional magnesium hydroxide, and the rest of the technical solutions remain unchanged.

[0145] Thermal stability test

[0146] In a nitrogen atmosphere, a thermogravimetric analyzer was used to test the thermal stability of the samples of the embodiment and the comparative example. The test temperature was 400° C., the nitrogen gas flow rate was 20 mL / min, the heating rate was 10° C. / min, and the time was 30 min.

[0147] Table 1

[0148] Quality retention rate % Example 1 75.3 Example 2 75.8 Example 3 76.1 Example 4 75.0 Example 5 75.4 Comparative Example 1 43.7 Comparative Example 2 60.5

[0149] It can be seen from Table 1 that the polylactic acid fiber cloth prepared by the present invention has excellent heat resistance and stability.

[0150] Flame retardant performance test

[0151] Vertical combustion index: refer to GB / T5455-2014 "Determination of vertical direction damage length and smoldering of textile combustion performance", use the vertical method fabric combustion performance tester to test the damage length and smoldering time of the original sample and the flame retardant treated sample, as shown in Table 2:

[0152] Table 2

[0153]

[0154]

[0155] It can be seen from Table 2 that the polylactic acid fiber cloth prepared by the present invention has excellent flame retardancy.

[0156] Limiting oxygen index: According to GB / T5454-1997 "Textile Combustion Performance Test Oxygen Index Method", the limiting oxygen index (LOI) of the original sample and the flame retardant treated sample is tested using an oxygen index tester;

[0157] Table 3

[0158] LOI% Example 1 35.5 Example 2 34.2 Example 3 35.8 Example 4 34.7 Example 5 35.6 Comparative Example 1 18.1 Comparative Example 2 26.4

[0159] It can be seen from Table 3 that the polylactic acid fiber cloth obtained by the present invention has a higher limiting oxygen index and a better flame retardant effect.

[0160] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing heat-resistant and flame-retardant polylactic acid fiber cloth, characterized in that: The modified polylactic acid fibers are cross-webbed, hydroentangled and finally dried to obtain heat-resistant and flame-retardant polylactic acid fiber cloth; The thickness of the heat-resistant and flame-retardant polylactic acid fiber cloth is 0.4-1.0 mm; The unit mass of the heat-resistant flame-retardant polylactic acid is 60-70 g / m 2 .

2. The method for preparing a heat-resistant and flame-retardant polylactic acid fiber cloth according to claim 1, characterized in that: The modified polylactic acid fiber preparation method is: S1. Weigh by weight: 80-85 parts of polylactic acid resin, 1-2 parts of stearic acid, 10-12 parts of calcium carbonate, and 6-10 parts of coated nano magnesium hydroxide; S2, adding polylactic acid resin, stearic acid, calcium carbonate, and coated nano magnesium hydroxide into a blender in order, and mixing them evenly to obtain a mixture; S3, adding the mixed material into a drying oven, and subjecting it to drying treatment to obtain a dry mixed material; S4, adding the dry mixed material into a twin-screw extruder, subjecting it to melt extrusion, and then spinning it through a spinneret to obtain polylactic acid fibers.

3. The method for preparing a heat-resistant and flame-retardant polylactic acid fiber cloth according to claim 2, characterized in that: The method for preparing the coated nano magnesium hydroxide is as follows: First, magnesium chloride is added to deionized water, and stirred to mix evenly to obtain a magnesium chloride solution; Add anhydrous ethanol to the magnesium chloride solution, continue stirring and mixing to obtain a magnesium chloride ethanol solution; Acrylic acid was added to the magnesium chloride ethanol solution, the temperature was adjusted to 15°C, stirred for 30 minutes, then ammonia water was added dropwise, stirring was continued for 2 hours, sodium hydroxide solution was added dropwise, stirring was continued for 2 hours, the temperature was adjusted to 55°C, kept warm for 4 hours, filtered and dried to obtain coated nano magnesium hydroxide.

4. The method for preparing a heat-resistant and flame-retardant polylactic acid fiber cloth according to claim 3, characterized in that: The mass fraction of the magnesium chloride solution is 3-4%; The volume ratio of the anhydrous ethanol to deionized water is 1:

1.

5. The method for preparing a heat-resistant and flame-retardant polylactic acid fiber cloth according to claim 4, characterized in that: The volume ratio of the acrylic acid to the magnesium chloride ethanol solution is 1:20-22; The mass fraction of ammonia water is 5%, and the volume ratio of ammonia water to deionized water is 1.2-1.4:1; The mass fraction of sodium hydroxide solution is 2%; The volume ratio of sodium hydroxide solution to ammonia water is 2.5-2.8:1; The drying temperature was 80°C and the drying time was 10 hours.

6. The method for preparing a heat-resistant and flame-retardant polylactic acid fiber cloth according to claim 1, characterized in that: The hydroentanglement is formed by using water needles, where a fine water flow with a pressure of 6-8 MPa passes through a water spray plate with a micropore size of 0.2-0.5 mm.

7. The method for preparing a heat-resistant and flame-retardant polylactic acid fiber cloth according to claim 6, characterized in that: The drying is carried out at a temperature of 75-80°C.

8. The method for preparing a heat-resistant and flame-retardant polylactic acid fiber cloth according to claim 7, characterized in that: The drying time is 20-22 hours.

9. A heat-resistant and flame-retardant polylactic acid fiber cloth obtained according to the method for preparing the heat-resistant and flame-retardant polylactic acid fiber cloth according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Method for preparing halogen-free flame-proof polylactic acid

    CN101260227A

  • Fully degradable polylactic acid fiber spunlace fabric and preparation method thereof

    CN101649528A

  • Preparation method of nanotubular magnesium hydroxide

    CN102344153A

  • Flame-retardant fire-resistance-enhanced-type polylactic-acid fiber composite material for automotive interior trim parts and preparation method therefor

    CN105504709A

  • Polylactic acid fiber fabric for automobile seat cushion

    CN106012085A