Electrochromic covalent organic framework fiber membrane and preparation method thereof
Through the preparation of covalent organic frame fiber membranes, the problem of limited electrolyte penetration in flexible electrochromic materials is solved, and the electrochromic performance is improved, which is suitable for military camouflage stealth clothing.
Patent Information
- Application Number
- CN202411203651.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-30
AI Technical Summary
The linear conductive polymers of existing flexible electrochromic materials have large inter-chain forces, resulting in limited penetration and ion deintercalation processes of electrolytes, affecting the transmission efficiency of carriers and electrolyte ions, and limiting their electrochromic properties. promote.
The preparation method of covalent organic frame fiber membrane is adopted, and the covalent organic frame fiber membrane with a whole gradient porous covalent organic frame fiber membrane is formed through electrospinning and in-situ thermal synthesis reaction, which optimizes the permeability concentration and speed of the electrolyte, so that the electrolyte and the redox unit are fully in contact. , improve electrochromic performance.
The electrochromic performance has been improved. The material has a large specific surface area, stable structure, π-electron conjugation system and multi-stage pore structure, short color change time, high color efficiency, and excellent optical contrast. It is suitable for military camouflage stealth clothing.
Smart Images

Figure CN119083041A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of fiber materials, and in particular to an electrochromic covalent organic framework fiber membrane and a preparation method thereof. Background Art
[0002] With the continuous development of high-tech reconnaissance systems, the visibility of weapons and equipment and individual soldiers on the battlefield has been greatly improved, which seriously threatens soldiers and national security. Flexible electrochromic materials are a kind of material that urgently needs to be vigorously developed in the field of intelligent camouflage protection such as stealth, shielding, and false indication, and have great application prospects in the field of military security. However, the current flexible electrochromic materials are mainly linear conductive polymers (such as polyaniline and polypyrrole), which have the advantages of rich color change and short response time. However, due to the large interaction force between the molecular chains of linear conductive polymers and the tight entanglement, it is not conducive to the penetration of electrolytes and the ion deintercalation process in practical applications, which affects the transmission efficiency of carriers and electrolyte ions, resulting in its electrochromic performance still being limited in application.
[0003] Covalent organic frameworks (COFs) are a type of porous powder materials with low density, large specific surface area, adjustable size and structure. The porosity, high crystallinity, π-electron conjugation system and ordered π-π stacking of COFs can effectively promote electron conduction and ion transport. In addition, by screening multifunctional compounds with redox properties as building blocks, COFs can be endowed with electrochromic functions; due to the unique porous structure and rich redox units of COFs, the new electrochromic materials prepared with COFs can effectively improve the transmission efficiency of electrons and ions, making their color-changing properties have the advantages of short color change time, high coloring efficiency and high optical contrast compared with traditional linear polymer-based electrochromic materials. However, the intrinsic nanopore (<5nm) structure of COFs leads to large resistance to the insertion and removal of electrolyte ions, which to a certain extent limits the further improvement of its electrochromic performance. Summary of the invention
[0004] In view of this, the purpose of the present invention is to provide an electrochromic covalent organic framework fiber membrane and a preparation method thereof. The preparation method provided by the present invention can obtain a covalent organic framework electrochromic fiber membrane material with gradient porosity throughout the body, which has micron-level pores formed by fiber entanglement, submicron pores of porous fibers and intrinsic mesopores of the covalent organic framework. Such a gradient pore structure is conducive to the simultaneous optimization of the penetration concentration and speed of the electrolyte in the electrochromic material, so that the electrolyte is fully in contact with the redox unit of the material, thereby improving the electrochromic performance.
[0005] In order to achieve the above object, the present invention provides the following technical solutions:
[0006] One of the technical solutions of the present invention is a method for preparing an electrochromic covalent organic framework fiber membrane, comprising the following steps:
[0007] Dissolving polyvinylidene fluoride, polyamino compounds and polyethylene glycol in a mixed solvent to obtain a spinning solution, and then electrospinning the spinning solution to obtain a precursor fiber membrane;
[0008] The precursor fiber membrane is subjected to an in-situ thermal synthesis reaction in a solution containing a polyaldehyde compound and a catalyst to obtain an electrochromic covalent organic framework fiber membrane.
[0009] The second technical solution of the present invention is an electrochromic covalent organic framework fiber membrane prepared by the above preparation method.
[0010] The present invention discloses the following technical effects:
[0011] The present invention provides a method for preparing an electrochromic covalent organic framework fiber membrane. The material prepared by the method not only has the characteristics of large specific surface area, stable structure, π electron conjugated system, and multiple reaction sites of the covalent organic framework, but also has a multi-level pore structure of micron pores / submicron pores / micro-mesopores, so that the electrolyte and the reaction units in the electrochromic COFs can contact quickly and fully, effectively improving the electrochromic performance of the material.
[0012] The electrochromic covalent organic framework fiber membrane provided by the present invention is a fiber-based electrochromic material, which can be better applied to military camouflage stealth clothing and maintain excellent flexibility, air permeability and macroscopic continuity. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0014] Figure 1 The nitrogen adsorption-desorption isotherm and specific surface area diagram of the electrochromic covalent organic framework fiber membrane in Example 1;
[0015] Figure 2 This is a pore size distribution diagram of the electrochromic covalent organic framework fiber membrane in Example 1;
[0016] Figure 3 This is a scanning electron microscope (SEM) image of the electrochromic covalent organic framework fiber membrane in Example 1;
[0017] Figure 4 1 is a cyclic voltammetry curve of the electrochromic covalent organic framework fiber membrane in Example 1;
[0018] Figure 5This is a color-changing optical photograph of the electrochromic covalent organic framework fiber membrane in Example 1. DETAILED DESCRIPTION
[0019] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0020] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0021] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0022] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.
[0023] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0024] The present invention provides a method for preparing an electrochromic covalent organic framework fiber membrane, comprising the following steps:
[0025] Dissolving polyvinylidene fluoride, polyamino compounds and polyethylene glycol in a mixed solvent to obtain a spinning solution, and then electrospinning the spinning solution to obtain a porous electrochromic covalent organic framework precursor fiber membrane (referred to as a precursor fiber membrane);
[0026] The precursor fiber membrane is subjected to an in-situ thermal synthesis reaction in a solution containing a polyaldehyde compound and a catalyst to obtain an electrochromic covalent organic framework fiber membrane.
[0027] In some embodiments of the present invention, the molecular weight of the polyvinylidene fluoride is 400,000 to 900,000; and the molecular weight of the polyethylene glycol is 2,000 to 2,000,000.
[0028] The reason why the molecular weights of polyvinylidene fluoride and polyethylene glycol in the present invention are selected to be within the above parameter range is that the molecular weight of polyvinylidene fluoride will affect the fiber morphology and performance of electrospinning. If it is not within this range, it will lead to poor fiber uniformity and beading phenomenon. The molecular weight of polyethylene glycol will affect the size and density of the pores on the fiber, and will also affect the viscosity of the spinning solution. If it is not within this range, it will cause fiber pore formation failure.
[0029] In some embodiments of the present invention, in the spinning solution, the concentration of the polyvinylidene fluoride is 4-15wt%.
[0030] In some embodiments of the present invention, the polyamino compound is at least one of tris(4-aminophenyl)amine, 1,3,6,8-tetrakis-(p-aminophenyl)-pyrene and 1,3,5-tris(4-aminophenyl)benzene; and the mass ratio of the polyvinylidene fluoride, the polyamino compound and the polyethylene glycol is 1:(0.1-1):(0.01-0.1).
[0031] In the present invention, if the mass ratio of polyvinylidene fluoride, polyamino compound and polyethylene glycol is not within the above range, it will result in: (1) the fiber morphology with uniform diameter cannot be formed after electrospinning; (2) the spinning solution is not fully phase-separated during the jet process, and the fiber has no pores. Both of the above situations will affect the microscopic morphology of the final electrochromic covalent organic framework fiber membrane, thereby affecting its electrochromic performance.
[0032] In some embodiments of the present invention, the mixed solvent is a mixture of N,N-dimethylformamide and water in a volume ratio of 1:(0-0.1).
[0033] In the present invention, if the volume ratio of N,N-dimethylformamide to water is not within the above range, it will affect the pore size of the precursor fiber membrane, causing it to deviate from the optimal pore size, thereby affecting the transmission rate of electrolyte ions.
[0034] In some embodiments of the present invention, the parameters of the electrospinning are: voltage 15-30 kV, liquid supply rate 0.2-5.0 mL / min, receiving distance 10-40 cm, drum speed 30-80 r / min, spinning temperature 20-28 ° C, spinning humidity 50-80%, and the material for receiving the fiber membrane is tin foil, aluminum foil or conductive carbon cloth.
[0035] In the present invention, if the electrospinning parameters are not within the above range, the spinning solution will not be able to break through the surface tension of the spinning solution under the action of charging, and will not be able to form a Taylor cone and continuously spray out into filaments, so that the material cannot form a nanofiber morphology with uniform diameter; or reasonable moisture-induced phase separation cannot occur, so that the fibers obtained by electrospinning do not have a suitable porous structure.
[0036] In some embodiments of the present invention, the polyaldehyde compound is at least one of thieno[3,2-b]thiophene-2,5-dicarboxaldehyde, benzo[C][1,2,5]thiadiazole-4,7-dicarboxaldehyde, 2,6-naphthalene dicarboxaldehyde, tris(4-formylphenyl)amine and trialdehyde pyrogallol; and the concentration of the polyaldehyde compound in the solution is 1.0 to 5.0 mM.
[0037] In some embodiments of the present invention, the catalyst is formic acid, acetic acid or toluenesulfonic acid; the concentration of the catalyst in the solution is 20-40 mM.
[0038] In some embodiments of the present invention, the solvent used to dissolve the polyaldehyde compound and the catalyst is at least one of methanol, ethanol, 1,4-dioxane, mesitylene, benzyl alcohol and chloroform.
[0039] In some embodiments of the present invention, the reaction temperature of the in-situ thermal synthesis reaction is 25 to 120° C., and the reaction time is 3 to 72 hours.
[0040] In some embodiments of the present invention, after the in-situ thermal synthesis reaction is completed, it also includes washing and drying steps; the solvent used for washing is at least one of methanol, ethanol, 1,4-dioxane, mesitylene, benzyl alcohol, chloroform and water; the drying temperature is 80°C and the time is 12 hours.
[0041] The present invention also provides an electrochromic covalent organic framework fiber membrane prepared by the preparation method described in the above technical solution.
[0042] The electrochromic covalent organic framework fiber membrane provided by the present invention has a gradient porous structure of micron pores, submicron pores, and mesopores. Such a gradient pore structure is conducive to the simultaneous optimization of the penetration concentration and speed of the electrolyte in the electrochromic material, so that the electrolyte is fully in contact with the redox unit of the material, and the electrochromic performance is improved. Compared with the electrochromic film prepared by the prior art, the material of the present invention has the characteristics of high specific surface area, large gradient porosity, stable structure, multiple reaction sites, high ion deintercalation efficiency, etc., and can achieve excellent electrochromic performance.
[0043] The mechanism of the present invention is as follows:
[0044] The electrochromic covalent organic framework fiber membrane provided by the present invention has gradient porosity throughout the body, which needs to meet two conditions: First, the electrochromic covalent organic framework precursor fiber membrane with porosity throughout the body is stably and uniformly prepared. By adding polyethylene glycol of a certain molecular weight and water to induce the electrospinning solution to undergo controllable phase separation during the charged jet and stretching orientation process, a precursor fiber membrane with a submicron pore structure throughout the body is obtained. The average diameter of the fiber is 1.8μm, the average surface pore size is 350±200nm, and the fiber surface pore number density is 9±3 pores / μm 2 . The chemical composition of the spinning solution determines the critical conditions for phase separation in the system. The final fiber morphology is highly dependent on the electrospinning parameters, and the porous morphology of the fiber has a significant impact on the electrochromic properties of the final material. The second is the sufficient and uniform in-situ synthesis of the electrochromic covalent organic framework on the porous precursor fiber membrane. It requires that the polyamine compounds in the precursor fiber and the polyaldehyde compounds in the solution have a comparable diffusion rate in the reaction liquid system, so as to synthesize a sufficient amount of electrochromic covalent organic framework in situ inside the submicron porous precursor fiber. A non-ideal solvent system will cause the covalent organic framework particles to be synthesized in the reaction liquid, physically adhere to the fiber surface, or an insufficient amount of covalent organic framework film to adhere to the fiber surface. All of the above situations will affect the electrochromic properties of the final fiber membrane.
[0045] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with the embodiments, but the content of the present invention is not limited to the following embodiments.
[0046] Unless otherwise specified, the raw materials and reagents used in the examples can be obtained through commercial channels.
[0047] Example 1
[0048] This embodiment provides an electrochromic covalent organic framework fiber membrane, and the preparation method steps are as follows:
[0049] Step 1: Mix polyvinylidene fluoride (molecular weight: 400,000, 1.2 g), polyethylene glycol (molecular weight: 2,000,000, 0.08 g), and tri(4-aminophenyl)amine (0.36 g) in a mixed solvent (10 mL) of DMF and deionized water, wherein the volume ratio of DMF to deionized water is 1:0.06; stir the mixed system at 90°C for 8 hours to obtain a spinning solution; use the spinning solution to prepare an electrochromic covalent organic framework precursor fiber membrane (referred to as a precursor fiber membrane) by electrospinning; the electrospinning parameters are: voltage 22.5 kV, liquid supply rate 1.5 mL / h, receiving distance 15 cm, drum speed 30 r / min, the material of the receiving fiber membrane is aluminum foil, the spinning temperature is 25±1°C, and the spinning humidity is 56±2%.
[0050] Step 2: Mix and dissolve tri(4-formylphenyl)amine (5.2 mg) and acetic acid (3M, 0.3 mL) in mesitylene / ethanol (1:1 v / v, 30 ml) to obtain a polyaldehyde compound reaction solution; soak the precursor fiber membrane (20 mg) prepared in step 1 in the polyaldehyde compound reaction solution and react at 120°C for 24 hours; the fiber membrane after the reaction is washed with DMF, water, and ethanol in turn, and then dried at 80°C for 12 hours to obtain an electrochromic covalent organic framework fiber membrane, which has a gradient porous structure throughout the body and exhibits a reversible color change from reddish brown to dark green in the voltage range of -2.5 to 2.5 V, with a color change response time of 4.8 s.
[0051] The specific surface area of the obtained electrochromic covalent organic framework fiber membrane is 289.90 m 2 / g( Figure 1 ), the pore size distribution is as follows Figure 2 shown. Figure 3 The scanning electron microscope (SEM) images of electrochromic covalent organic framework fiber membranes at different magnifications are shown ((a) is 10 μm, (b) is 3 μm), and the fibers exhibit a gradient porous structure throughout the body; Figure 4 The cyclic voltammetry curves of electrochromic covalent organic framework fiber membranes are shown; Figure 5 The color-changing optical photographs of the electrochromic covalent organic framework fiber membrane are shown.
[0052] Comparative Example 1
[0053] This comparative example provides an electrochromic covalent organic framework fiber membrane, and the preparation method steps are as follows:
[0054] Step 1: Mix polyvinylidene fluoride (molecular weight: 400,000, 1.2 g) and tri(4-aminophenyl)amine (0.36 g) in DMF (10 mL), and stir at 90°C for 8 h to obtain a spinning solution; use the spinning solution to prepare an electrochromic covalent organic framework precursor fiber membrane (referred to as a precursor fiber membrane) by electrospinning; the electrospinning parameters are: voltage 22.5 kV, liquid supply rate 2.5 mL / h, receiving distance 15 cm, drum speed 30 r / min, the material of the receiving fiber membrane is aluminum foil, the spinning temperature is 25±1°C, and the humidity is 56±2%.
[0055] Step 2: Mix and dissolve tri(4-formylphenyl)amine (5.2 mg) and acetic acid (concentration 3M, volume 0.3 mL) in mesitylene / ethanol (1:1 v / v, 30 ml) to obtain a polyaldehyde compound reaction solution; soak the precursor fiber membrane (20 mg) prepared in step 1 in the polyaldehyde compound reaction solution and react at 120°C for 24 hours; the fiber membrane after the reaction is washed with DMF, water, and ethanol in turn, and then dried at 80°C for 12 hours to obtain an electrochromic covalent organic framework fiber membrane. The material has only a mesoporous structure and exhibits a reversible color change from reddish brown to dark brown in the voltage range of -2.5 to 2.5 V, and the color change response time is 19.1 s.
[0056] The specific surface area of the obtained electrochromic covalent organic framework fiber membrane is 50.6 m 2 / g.
[0057] Example 2
[0058] This embodiment provides an electrochromic covalent organic framework fiber membrane, and the preparation method steps are as follows:
[0059] Step 1: polyvinylidene fluoride (molecular weight: 400,000, 1.2 g), polyethylene glycol (molecular weight: 2,000,000, 0.08 g), and 1,3,5-tris(4-aminophenyl)benzene (0.36 g) were mixed in a mixed solvent (10 mL) of DMF and deionized water, wherein the volume ratio of DMF to deionized water was 50:3; the mixed system was stirred at 90°C for 8 h to obtain a spinning solution; the spinning solution was electrospinned to prepare an electrochromic covalent organic framework precursor fiber membrane (referred to as a precursor fiber membrane); the electrospinning parameters were: voltage 22.5 kV, liquid supply rate 1.5 mL / h, receiving distance 15 cm, drum speed 30 r / min, the material for receiving the fiber membrane was aluminum foil, the spinning temperature was 25±1°C, and the humidity was 56±2%.
[0060] S2: Mix and dissolve trialdehyde pyrogallol (5.2 mg) and acetic acid (concentration 3M, volume 0.3 mL) in mesitylene / ethanol (1:1 v / v, 30 ml) to obtain a polyaldehyde compound reaction solution; soak the precursor fiber membrane (20 mg) prepared in step 1 in the polyaldehyde compound reaction solution and react at 120°C for 24 hours; the fiber membrane after the reaction is washed with DMF, water and ethanol in sequence, and then dried at 80°C for 12 hours to obtain an electrochromic covalent organic framework fiber membrane, which has a gradient porous structure throughout and exhibits a reversible color change from orange to brick red in the voltage range of -3 to 3V, with a color change response time of 12.3s.
[0061] The specific surface area of the obtained electrochromic covalent organic framework fiber membrane is 260.1 m2 / g.
[0062] Comparative Example 2
[0063] This comparative example provides an electrochromic covalent organic framework fiber membrane, and the preparation method steps are as follows:
[0064] Step 1: Mix polyvinylidene fluoride (molecular weight: 400,000, 1.2 g) and 1,3,5-tri(4-aminophenyl)benzene (0.36 g) in DMF (10 mL), and stir the mixed system at 90°C for 8 h to obtain a spinning solution; prepare an electrochromic covalent organic framework precursor fiber membrane (referred to as a precursor fiber membrane) from the spinning solution by electrospinning; the electrospinning parameters are: voltage 22.5 kV, liquid supply rate 1.5 mL / h, receiving distance 15 cm, drum speed 30 r / min, the material of the receiving fiber membrane is aluminum foil, the spinning temperature is 25±1°C, and the humidity is 56±2%.
[0065] Step 2: Mix and dissolve trialdehyde pyrogallol (5.2 mg) and acetic acid (concentration 3M, volume 0.3 mL) in mesitylene / ethanol (1:1 v / v, 30 ml) to obtain a polyaldehyde compound reaction solution; soak the precursor fiber membrane (20 mg) prepared in step 1 in the polyaldehyde compound reaction solution and react at 120°C for 24 hours; the fiber membrane after the reaction is washed with DMF, water, and ethanol in turn, and then dried at 80°C for 12 hours to obtain an electrochromic covalent organic framework fiber membrane, which has only a mesoporous structure and exhibits a reversible color change from orange to brick red in the voltage range of -3 to 3V, and the color change response time is 28.9s.
[0066] The specific surface area of the obtained electrochromic covalent organic framework fiber membrane is 79.8 m 2 / g.
[0067] The electrochromic properties of the electrochromic covalent organic framework fiber membranes of Examples 1-2 and Comparative Examples 1-2 are summarized (Table 1).
[0068] Table 1
[0069] Color Change Driving voltage Response time Example 1 Reddish brown-dark green -2.5~2.5V 4.8s Comparative Example 1 Reddish brown-dark brown -2.5~2.5V 19.1s Example 2 Orange-Brick Red -3~3V 12.3s Comparative Example 2 Orange-Brick Red -3~3V 28.9s
[0070] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing an electrochromic covalent organic framework fiber membrane, characterized in that: The following steps are involved: Dissolving polyvinylidene fluoride, polyamino compounds and polyethylene glycol in a mixed solvent to obtain a spinning solution, and then electrospinning the spinning solution to obtain a precursor fiber membrane; The precursor fiber membrane is subjected to an in-situ thermal synthesis reaction in a solution containing a polyaldehyde compound and a catalyst to obtain an electrochromic covalent organic framework fiber membrane.
2. The method for preparing the electrochromic covalent organic framework fiber membrane according to claim 1, characterized in that: The molecular weight of the polyvinylidene fluoride is 400,000 to 900,000; the molecular weight of the polyethylene glycol is 2,000 to 2,000,000.
3. The method for preparing the electrochromic covalent organic framework fiber membrane according to claim 1, characterized in that: The polyamino compound is at least one of tris(4-aminophenyl)amine, 1,3,6,8-tetrakis-(p-aminophenyl)-pyrene and 1,3,5-tris(4-aminophenyl)benzene; the mass ratio of the polyvinylidene fluoride, the polyamino compound and the polyethylene glycol is 1:(0.1-1):(0.01-0.1).
4. The method for preparing the electrochromic covalent organic framework fiber membrane according to claim 1, characterized in that: The mixed solvent is a mixture of N,N-dimethylformamide and water in a volume ratio of 1:(0-0.1).
5. The method for preparing the electrochromic covalent organic framework fiber membrane according to claim 1, characterized in that: The electrostatic spinning parameters are: voltage 15-30 kV, liquid supply rate 0.2-5.0 mL / min, receiving distance 10-40 cm, drum speed 30-80 r / min, spinning temperature 20-28° C., and spinning humidity 50-80%.
6. The method for preparing the electrochromic covalent organic framework fiber membrane according to claim 1, characterized in that: The polyaldehyde compound is at least one of thieno[3,2-b]thiophene-2,5-dicarboxaldehyde, benzo[C][1,2,5]thiadiazole-4,7-dicarboxaldehyde, 2,6-naphthalene dicarboxaldehyde, tris(4-formylphenyl)amine and trialdehyde phloroglucinol; and the concentration of the polyaldehyde compound in the solution is 1.0 to 5.0 mM.
7. The method for preparing the electrochromic covalent organic framework fiber membrane according to claim 1, characterized in that: The catalyst is formic acid, acetic acid or toluenesulfonic acid; the concentration of the catalyst in the solution is 20-40 mM.
8. The method for preparing the electrochromic covalent organic framework fiber membrane according to claim 1, characterized in that: The solvent used to dissolve the polyaldehyde compound and the catalyst is at least one of methanol, ethanol, 1,4-dioxane, mesitylene, benzyl alcohol and chloroform.
9. The method for preparing the electrochromic covalent organic framework fiber membrane according to claim 1, characterized in that: The reaction temperature of the in-situ thermal synthesis reaction is 25 to 120° C., and the reaction time is 3 to 72 hours.
10. An electrochromic covalent organic framework fiber membrane prepared by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Solid electrolyte and preparation method and application thereof
CN110165291A
Preparation method of shape-controllable covalent organic framework material
CN114106276A
Flexible covalent organic framework nanofiber membrane, electrochromic device and preparation method
CN116466528A
Covalent organic framework composite nanofiber electrochromic film and preparation and application thereof
CN116479583A
Porous covalent organic framework nanofiber membrane and preparation method thereof
CN118497980A