Method for reducing dosage of alkaline agent in polyester alkali decrement process
By using a non-aqueous medium system in the alkali reduction process, the alkali agent molecules are dispersed at a high concentration in the silicon-based non-aqueous medium, the problems of low NaOH utilization rate and safety hazards in the traditional alkali reduction process are solved, and the low alkali consumption is achieved , high-efficiency alkali reduction treatment improves the performance and environmental protection of polyester fabrics.
Patent Information
- Application Number
- CN202411215730.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-12-06
AI Technical Summary
The utilization rate of NaOH in the traditional alkali reduction process is low, resulting in a large amount of free alkali in the wastewater, which is difficult to deal with, and poses a safety hazard to the working workers.
The non-aqueous medium system is used to disperse alkaline molecules in silicon-based non-aqueous medium with high concentrations, improve the affinity of alkaline agents for fibers, reduce the amount of alkaline agents, and at the same time explore the optimal NaOH concentration and moisture content, and use the Decamethylcyclopentasiloxane or liquid paraffin serves as a heat transfer medium, instead of water bath heat transfer.
It significantly reduces the amount of alkali, improves the efficiency of alkali reduction, reduces the generation and emission of sewage, improves the dyeing effect and physical properties of polyester fabrics, and the non-aqueous medium can be recycled, making the process safe and environmentally friendly.
Smart Images

Figure CN119083152A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of alkali weight reduction process, and in particular relates to a method for reducing the amount of alkali agent used in the process of alkali weight reduction of polyester. Background Art
[0002] Polyester fabrics have high strength, good elastic recovery, and are easy to blend with natural fibers, occupying an important position in textiles. However, they have problems such as poor hygroscopicity and easy static electricity, which restrict their market prospects as high-end textile materials. After alkali reduction treatment, the defects of polyester fibers themselves can be improved, giving them advantages such as good drape and water retention. Generally, the traditional alkali reduction process uses high temperature and concentrated caustic soda solution to treat polyester fabrics, but the utilization rate of NaOH in traditional alkali reduction is low, resulting in a large amount of free alkali in the wastewater of the alkali reduction process, which has the characteristics of high pH value and high chemical oxygen demand (COD), and is difficult to handle. At the same time, since liquid alkali is a hazardous chemical, high-concentration liquid alkali poses a great safety hazard to workers in the actual production process. Summary of the invention
[0003] Technical issues
[0004] At present, the alkali reduction process of polyester fabric is carried out under water bath conditions. Since the hydroxyl groups in the alkali agent are distributed throughout the treatment bath, the probability of attacking the molecular structure of polyester is low, resulting in the need to add a high concentration of alkali agent to obtain the desired alkali reduction effect. However, the utilization rate of NaOH in traditional alkali reduction is low, resulting in a large amount of free alkali in the wastewater of the alkali reduction process, which has the characteristics of high pH value and high chemical oxygen demand (COD), and is difficult to handle. At the same time, since liquid alkali is a hazardous chemical, high concentration of liquid alkali poses a great safety hazard to workers in the actual production process. Therefore, it is necessary to provide a process method that reduces the amount of alkali while not reducing the alkali reduction effect.
[0005] Technical Solution
[0006] To solve the above problems, the present invention utilizes the characteristic that the alkali agent in the non-aqueous medium system is only soluble in a small amount of water but insoluble in the non-aqueous medium, so that the alkali agent molecules are dispersed in the silicon-based non-aqueous medium in the form of small droplets with high concentration. At the same alkali agent dosage, the affinity of the alkali agent for the fiber is increased, thereby improving the alkali reduction efficiency and achieving the purpose of reducing the amount of alkali agent used.
[0007] There are many types of non-aqueous media on the market, the most representative of which are liquid paraffin (LP) and decamethylcyclopentasiloxane (D5). Liquid paraffin (LP) is a normal alkane with 8 to 24 carbon atoms. It is a colorless, odorless, non-toxic, and non-volatile oily liquid. LP is cheap and has a very broad industrial prospect. D5 is an organic silicon compound with a silicon-oxygen bond as the main chain. It is colorless, non-toxic, recyclable, and has good compatibility with some organic solvents. It is an eco-friendly organic solvent. Using non-aqueous media as a heat transfer medium to treat polyester fabrics with alkali reduction, instead of water bath heat transfer in traditional processes, can increase the reduction rate in the non-aqueous medium system without a high amount of alkali agent, and achieve the effect of energy saving and emission reduction. Moreover, alkali reduction is a key process to improve the wearing performance of polyester fabrics. In the context of the increasing awareness of environmental protection, it is of great significance to use non-aqueous media to reduce the amount of alkali used in the alkali reduction process.
[0008] The present invention explores the optimal NaOH concentration and moisture content of the treatment solution in the alkali reduction process of the non-aqueous medium, explores the reusability of the non-aqueous medium, and tests the physical properties of polyester fabrics under different treatment conditions, exploring the influence of the alkali reduction process of the non-aqueous medium on the whiteness and hair effect of the polyester fabric. In addition, the present invention performs traditional water bath dyeing on polyester fabrics under different treatment conditions and compares the dyeing effects.
[0009] The present invention is different from the low-salt and low-alkali technology of non-aqueous medium mentioned in other studies. The existing studies describe that when dyeing cotton fabric with reactive dyes in non-aqueous medium system, adding alkali can provide color fixation pH value and act as inorganic salt to promote dyeing. In this case, the alkali can only be reduced by about 15%. If it is reduced too low, the dyeing effect cannot be achieved. The present invention utilizes the characteristics of non-aqueous medium system alkali molecules dispersed in silicon-based non-aqueous medium in small droplets with high concentration. When the alkali concentration is 5g / L, the polyester fabric reduction rate has reached 20%, which is twice the reduction rate (only 9%) when the traditional water bath sodium hydroxide concentration is 36g / L. At this time, the amount of alkali has been reduced by 86.11%.
[0010] The invention provides an alkali reduction treatment liquid with low alkali dosage, which consists of a non-aqueous medium, water and an alkali agent. Calculated by mass fraction, the non-aqueous medium accounts for 90-95% of the alkali reduction treatment liquid, and the water accounts for 5-10%. The concentration of the alkali agent in the alkali reduction treatment liquid is 1.0-10.0 g / L.
[0011] Furthermore, the non-aqueous medium includes one or more of decamethylcyclopentasiloxane, liquid paraffin, and anhydrous ethanol.
[0012] Preferably, the non-aqueous medium is decamethylcyclopentasiloxane or liquid paraffin.
[0013] Furthermore, the alkaline agent includes one or more of sodium hydroxide, potassium hydroxide, and calcium hydroxide.
[0014] Preferably, the concentration of the alkali agent in the alkali reduction treatment solution is 5.0 to 10.0 g / L.
[0015] Preferably, by mass fraction, the non-aqueous medium accounts for 92.5-95% of the alkali weight reduction treatment liquid, and water accounts for 5-7.5%.
[0016] The alkali weight reduction treatment liquid with low alkali dosage provided by the present invention is applied in the textile field.
[0017] Furthermore, the application is alkali weight reduction treatment of polyester.
[0018] The present invention also provides a method for treating fabric with alkali reduction using low alkali dosage, the method comprising the following steps:
[0019] (1) preparing an alkali reduction treatment solution using a non-aqueous medium, an alkali agent and water;
[0020] (2) The fabric is placed in an alkali weight reduction treatment solution at a certain temperature and heated for a period of time before being taken out, and then washed and dried to obtain the fabric after alkali weight reduction treatment.
[0021] In one embodiment of the present invention, the non-aqueous medium in step (1) comprises one or more of decamethylcyclopentasiloxane, liquid paraffin, and anhydrous ethanol.
[0022] Preferably, the non-aqueous medium in step (1) is decamethylcyclopentasiloxane or liquid paraffin.
[0023] Specifically, optionally, the non-aqueous medium in step (1) is decamethylcyclopentasiloxane.
[0024] In one embodiment of the present invention, the alkaline agent in step (1) includes one or more of sodium hydroxide, potassium hydroxide, and calcium hydroxide.
[0025] In one embodiment of the present invention, the concentration of the alkali agent in step (1) is 1.0 to 10.0 g / L.
[0026] Preferably, the concentration of the alkali agent in step (1) is 5.0 to 10.0 g / L.
[0027] Specifically, optionally, the concentration of the alkali agent in step (1) is 7.0 g / L.
[0028] In one embodiment of the present invention, in the treatment liquid in step (1), the non-aqueous medium accounts for 90-95% of the alkali weight reduction treatment liquid, and water accounts for 5-10% by mass.
[0029] Preferably, in the treatment liquid in step (1), by mass fraction, the non-aqueous medium accounts for 92.5-95% of the alkali weight reduction treatment liquid, and water accounts for 5-7.5%.
[0030] In one embodiment of the present invention, the fabric in step (2) is polyester fabric.
[0031] In one embodiment of the present invention, the polyester fabric comprises 100% knitted or woven polyester fabric.
[0032] In one embodiment of the present invention, the bath ratio in step (2) is 1:10-30.
[0033] In one embodiment of the present invention, the certain temperature in step (2) is 40.0-50.0°C.
[0034] In one embodiment of the present invention, the heating in step (2) refers to heating to 90-95° C. at a rate of 4-6° C. / min.
[0035] In one embodiment of the present invention, the insulation time in step (2) is 50 to 70 minutes.
[0036] The invention provides fabric treated with alkali weight reduction and prepared according to the method.
[0037] The invention provides an application of the alkali-reduced fabric in the field of textiles and clothing.
[0038] Beneficial Effects
[0039] (1) Reduction and efficiency: The method of the present invention can significantly reduce the amount of alkali used in the alkali reduction treatment of polyester, and at the same time can ensure that the alkali reduction rate is improved. The polyester fabric obtained by the alkali reduction treatment can achieve excellent dyeing effect and physical properties, and also has the characteristics of imitation silk and a softer feel. For example, when the alkali reduction process under the non-aqueous medium system of the present invention is used to treat the polyester fabric, when the NaOH concentration is 7g / L, the reduction rate is as high as 25%, and the K / S value after dyeing is 19.24. Compared with the polyester fabric treated by the traditional water bath alkali reduction process, when the NaOH concentration is as high as the industrial concentration of 36g / L, the reduction rate is only 8.03%, and the K / S value after dyeing is 18.20. In addition, after the alkali reduction process of the present invention, the wicking height of the polyester fabric is higher than that of the untreated fabric in both the warp and weft directions, and the hair effect is increased by more than 50%, which is better than the effect of the traditional treated fabric.
[0040] (2) Green and safe: The alkali reduction process under the non-aqueous medium system of the present invention can reduce the alkali consumption by 70-85%, avoiding the use of concentrated alkali. At the same time, the non-aqueous medium in the alkali reduction treatment liquid can be recycled many times. The consumption in the entire alkali reduction process is extremely small, and the amount of sewage generated and discharged is extremely small. It is a green, environmentally friendly, safe, efficient and resource-saving production process. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 The effect of different alkali agent concentrations and different water contents on alkali reduction of polyester in non-aqueous medium system;
[0042] Figure 2 The effect of the number of cycles of non-aqueous media on the alkali reduction of polyester;
[0043] Figure 3 The effect of 7g / L alkali agent concentration in non-aqueous medium system and 36g / L alkali agent concentration in traditional water bath on alkali reduction of polyester;
[0044] Figure 4 The effect of D5 and liquid paraffin on alkali reduction of polyester at 7g / L alkali concentration;
[0045] Figure 5 The effect of different treatment conditions on the K / S value of polyester dyed fabric; treatment condition 1 is no treatment; treatment condition 2 is 36g / L NaOH+H 2 O; treatment condition 3 is 7g / L NaOH+H 2 O; treatment condition 4 is 7g / L NaOH + non-aqueous medium that has not been circulated; treatment condition 5 is 7g / L NaOH + non-aqueous medium after 5 cycles. DETAILED DESCRIPTION
[0046] Test Method
[0047] K / S value test: Datacolor 800 colorimeter was used to measure three different positions of the sample in the spectral range of 380-700nm under light source D65 and with a 10° standard observer to obtain the average value of K / S value. This was used to evaluate the color parameter differences of polyester fabrics after dyeing under different treatment conditions.
[0048] Determination of weight reduction rate: In order to determine the alkali weight reduction efficiency of polyester fabric, the fabric before and after alkali weight reduction was dried in an oven at 60°C for 60 minutes and then quickly weighed. The weight reduction rate of the fabric was calculated according to formula I.
[0049]
[0050] Where: m 0 is the absolute dry weight of the fabric before alkali reduction, m 1It is the absolute dry weight of the fabric after alkali reduction.
[0051] Determination of whiteness: The fabric used at the end of the experiment was tested using a Datacolor 800 colorimeter. The measurements were made three times and the average value was taken.
[0052] Determination of capillary effect: The capillary effect is determined using a capillary effect tester. The main steps are: cut the sample into 30cm×5cm along the warp and weft directions, and record the wicking height of water climbing along the fabric within 30 minutes to indicate the wettability of the fabric after alkali reduction.
[0053] Source of raw materials
[0054] Polyester fabric: 100% polyester woven fabric, specification: 3.5D×65mm, purchased from Zhejiang Lvyu Textile Co., Ltd.;
[0055] Disperse Red 73: It is a reactive dye (filter cake), purchased from Zhejiang Longsheng Dye Chemical Co., Ltd., and its structural formula is as follows:
[0056]
[0057] Example 1
[0058] (1) Alkali weight reduction treatment liquid was prepared by using non-aqueous medium D5 and water, the percentage of water to fabric weight was expressed by moisture content, which was 100%, 130%, 150%, 175%, and 200%, respectively. The alkali used was NaOH, and the concentration of the alkali agent in the treatment liquid was 1 g / L, 2 g / L, 5 g / L, 7 g / L, and 10 g / L, respectively, where L represents the total volume of the alkali weight reduction treatment liquid;
[0059] (2) After heating the prepared treatment solution to 40°C, 1.0 g of polyester fabric was added, with a bath ratio of 1:20;
[0060] (3) Then the temperature was raised to 95°C at 5.6°C / min, kept at this temperature for 50 min, then lowered to 70°C at 5°C / min, and the fabric was taken out and washed for 15 min (bath ratio was 1:30);
[0061] (4) After washing, the fabric was placed in a 60°C oven and dried for 60 min. The weight of the fabric after drying was measured and the weight loss rate of the polyester fabric was calculated.
[0062] Table 1 Effect of different alkali concentrations and different water contents on alkali reduction of polyester in non-aqueous medium system
[0063] 1g / L 2g / L 5g / L 7g / L 10g / L 100% 3.985% 7.12% 19.54% 26.39% 33.95% 130% 3.355% 6.28% 18.24% 25.84% 33.89% 150% 3.17% 5.04% 17.86% 24.765% 31.75% 175% 2.545% 4.19% 13.58% 20.12% 26.81% 200% 2.3% 3.53% 12.36% 18.47% 25.9%
[0064] The results are as follows Figure 1As shown in Table 1, it can be found that the alkali reduction is not high at a lower alkali concentration, but when the alkali concentration is above 5g / L, the alkali reduction increases to more than 12.36%. At the same time, the higher the alkali concentration, the greater the alkali reduction. However, the higher the water content, the lower the alkali reduction. Therefore, considering the reuse of non-aqueous media and the treatment of wastewater, the optimal treatment conditions are finally selected as 7g / L alkali concentration and 130% water content.
[0065] Example 2
[0066] (1) using non-aqueous medium D5 and water to prepare alkali weight reduction treatment liquid, the percentage of water to fabric weight is expressed by moisture content, the moisture content is: 130%, the alkali used is NaOH, the alkali dosage is 7g / L, where L represents the total volume of the alkali weight reduction treatment liquid;
[0067] (2) After heating the prepared treatment solution to 40°C, 1.0 g of polyester fabric was added, with a bath ratio of 1:20;
[0068] (3) Then the temperature was raised to 95°C at 5.6°C / min, kept at this temperature for 50 min, then lowered to 70°C at 5°C / min, and the fabric was taken out and washed for 15 min (bath ratio was 1:30);
[0069] (4) After washing, the fabric was placed in a 60°C oven and dried for 60 min. The weight of the fabric after drying was measured and the weight loss rate of the polyester fabric was calculated.
[0070] (5) Repeat the above steps 5 times, measure the weight of the fabric after each drying treatment, and calculate the weight loss rate of the polyester fabric.
[0071] The results are as follows Figure 2 As shown, the reduction rate of the non-aqueous medium after 5 cycles is only 0.99% different from the first reduction rate, and the non-aqueous medium itself has no obvious change and can be used many times, which means that in this process, not only the amount of alkali can be greatly reduced, but also the consumption of the raw material itself is extremely low.
[0072] Example 3
[0073] This example is to explore the difference in effect between a non-aqueous medium system and a traditional water bath alkali weight reduction treatment.
[0074] (1) using deionized water to prepare an alkali weight reduction treatment solution, the alkali used is NaOH, and the alkali dosage is 36 g / L, where L represents the total volume of the alkali weight reduction treatment solution;
[0075] (2) After heating the prepared treatment solution to 40°C, 1.0 g of polyester fabric was added, with a bath ratio of 1:20;
[0076] (3) Then the temperature was raised to 95°C at 5.6°C / min, kept at this temperature for 50 min, then lowered to 70°C at 5°C / min, and the fabric was taken out and washed for 15 min (bath ratio was 1:30);
[0077] (4) After washing, the fabric was placed in a 60°C oven and dried for 60 min. The weight of the fabric after drying was measured and the weight loss rate of the polyester fabric was calculated.
[0078] The results are as follows Figure 3 As shown, it can be clearly seen that in the non-aqueous medium system, when the alkali dosage is only 7g / L, the alkali reduction of polyester fabric reaches 25.84%, while in the traditional alkali reduction process, even if the alkali dosage is 36g / L, the alkali reduction is only 9%. This fully demonstrates that the use of non-aqueous medium polyester alkali reduction treatment can significantly reduce the amount of alkali, while also improving the alkali reduction and increasing the utilization rate of the alkali.
[0079] Example 4
[0080] (1) using non-aqueous medium liquid paraffin and water to prepare alkali weight reduction treatment liquid, the percentage of water to fabric weight is expressed by moisture content, the moisture content is: 130%, the alkali used is NaOH, the alkali dosage is 7g / L, where L represents the total volume of the alkali weight reduction treatment liquid;
[0081] (2) After heating the prepared treatment solution to 40°C, 1.0 g of polyester fabric was added, with a bath ratio of 1:20;
[0082] (3) Then the temperature was raised to 95°C at 5.6°C / min, kept at this temperature for 50 min, then lowered to 70°C at 5°C / min, and the fabric was taken out and washed for 15 min (bath ratio was 1:30);
[0083] (4) After washing, the fabric was placed in a 60°C oven and dried for 60 min. The weight of the fabric after drying was measured and the weight loss rate of the polyester fabric was calculated.
[0084] The results are as follows Figure 4 As shown in Figure 2, at the same NaOH dosage of 7 g / L, the alkali reduction of D5 (25.84%) is better than that of liquid paraffin (12.85%), but at the same time Figure 3 Compared with the data in , it can be found that the use of non-aqueous media in the alkali weight reduction treatment of polyester can reduce the amount of alkali used, but in the comparison of different non-aqueous media, the effect of D5 is better than that of liquid paraffin.
[0085] Comparative Example 1
[0086] (1) Weigh the disperse dye into a dye cup at a dye concentration of 0.5% (owf), add 20 mL of deionized water into the dye cup at a bath ratio of 1:20, and the pH value of the dye solution is between 4.0 and 5.0;
[0087] (2) Polyester fabrics were selected under different treatment conditions: no treatment; 36 g / L NaOH + H 2 O; 7g / L NaOH+H 2 O; 7g / L NaOH + non-aqueous medium that has not been circulated (D5, moisture content: 130%); 7g / L NaOH + non-aqueous medium after 5 cycles (D5, moisture content: 130%); The treated fabric is directly rinsed with clean water several times.
[0088] (3) The polyester fabrics under different treatment conditions were immersed in dye solution at room temperature, and dyeing experiments were carried out using a DYE-24 adjustable dyeing machine. The temperature was raised to 80°C at 6°C / min, then raised to 140°C at 3°C / min, and dyed at 140°C for 60 min, and then cooled to 60°C.
[0089] (4) After dyeing, the dyed fabric was washed at 80°C for 15 min (bath ratio 1:20), repeated twice and dried for 60 min, and its K / S value was tested.
[0090] The results are as follows Figure 5 As shown, the polyester fabrics treated by the present invention and the traditional alkali reduction process were subjected to traditional water-bath dyeing. By comparison, it was found that the dyed fabric treated with a small amount of alkali agent in the non-aqueous medium system can achieve the dyeing effect after the high-concentration alkali agent treatment under the traditional alkali reduction process, and the non-aqueous medium treatment after the cycle does not affect its dyeing effect. Specifically, when the NaOH concentration is 7g / L, the K / S value of the fabric treated with the non-aqueous medium after dyeing is 19.24, and the K / S value of the fabric treated with the non-aqueous medium after 5 cycles is 18.99. The K / S value of the fabric treated with the traditional alkali reduction process after dyeing is 19.10. When the NaOH concentration is 36g / L, the K / S value of the fabric treated with the traditional alkali reduction process after dyeing is 18.20.
[0091] Comparative Example 2
[0092] (1) Polyester fabrics were selected under different treatment conditions: no treatment; 36 g / L NaOH + H 2 O; 7g / L NaOH+H 2 O; 7g / L NaOH + non-aqueous medium that has not been circulated (D5, moisture content: 130%); 7g / L NaOH + non-aqueous medium after 5 cycles (D5, moisture content: 130%); All the treated fabrics were directly rinsed with clean water several times.
[0093] (2) To explore the effects of different treatments on the physical properties of polyester fabrics, the Datacolor 800 colorimeter was used to test the whiteness of the fabrics used at the end of the experiment. The results were measured three times and the average value was taken.
[0094] (3) The samples treated in different ways were cut into 30 cm × 5 cm pieces along the warp and weft directions. The capillary effect was measured using a capillary effect meter, and the wicking height of water climbing along the fabric within 30 min was recorded.
[0095] Table 2 Test results of physical properties of polyester fabrics under different treatment conditions
[0096]
[0097] The results are shown in Table 2. For the polyester fabric treated by the method of the present invention, its physical properties are improved, which is specifically manifested in the changes in the wool effect and whiteness of the fabric. After the polyester fabric is treated by reducing the amount of alkali agent used in the non-aqueous medium system, the wicking height of the polyester fabric is higher than that of the untreated fabric in both the warp and weft directions, and the wool effect is increased by more than 50%. Compared with the untreated fabric, the whiteness of the polyester fabric treated with different alkali reduction prescriptions is increased by 1.43%, with no significant difference.
[0098] The embodiments provided above are not intended to limit the scope of the present invention, and the steps described are not intended to limit the execution order thereof. Those skilled in the art may make obvious improvements to the present invention in combination with existing common knowledge, which also fall within the scope of protection defined by the claims of the present invention.
Claims
1. An alkali reduction treatment solution with low alkali dosage, characterized in that: The alkali weight reduction treatment liquid is composed of non-aqueous medium, water and alkali agent; by mass fraction, the non-aqueous medium accounts for 90-95% of the alkali weight reduction treatment liquid, and the water accounts for 5-10%; the concentration of the alkali agent in the alkali weight reduction treatment liquid is 1.0-10.0g / L.
2. The low alkali dosage alkali reduction treatment liquid according to claim 1, characterized in that: The non-aqueous medium includes one or more of decamethylcyclopentasiloxane, liquid paraffin, and anhydrous ethanol.
3. The low alkali dosage alkali reduction treatment liquid according to claim 1, characterized in that: The alkaline agent includes one or more of sodium hydroxide, potassium hydroxide and calcium hydroxide.
4. Use of the alkali weight reduction treatment liquid according to any one of claims 1 to 3 in the textile field.
5. A method for treating fabric with alkali weight reduction using the alkali weight reduction treatment liquid according to any one of claims 1 to 3, characterized in that: The processing method comprises the following steps: (1) using a non-aqueous medium alkali agent and water to prepare an alkali reduction treatment solution; (2) The fabric is placed in an alkali weight reduction treatment solution at a certain temperature and heated for a period of time before being taken out, and then washed and dried to obtain the fabric after alkali weight reduction treatment.
6. The method for fabric alkali weight reduction treatment according to claim 5, characterized in that: In step (1), the non-aqueous medium includes one or more of decamethylcyclopentasiloxane, liquid paraffin, and anhydrous ethanol; the alkali agent includes one or more of sodium hydroxide, potassium hydroxide, and calcium hydroxide; the concentration of the alkali agent is 1.0 to 10.0 g / L; in the treatment liquid, by mass fraction, the non-aqueous medium accounts for 90 to 95% of the alkali reduction treatment liquid, and water accounts for 5 to 10%.
7. The method for fabric alkali weight reduction treatment according to claim 5, characterized in that: The fabric in step (2) is polyester fabric.
8. The method for treating fabric with alkali weight reduction according to claim 5, characterized in that: In step (2), the bath ratio is 1:10-30; the certain temperature is 40.0-50.0° C.; the heating refers to heating to 90-95° C. at 4-6° C. / min; and the heat preservation time is 50-70 min.
9. A fabric treated with alkali weight reduction prepared according to the method for treating fabric with alkali weight reduction according to any one of claims 5 to 8.
10. Use of the alkali-reduced fabric according to claim 9 in the field of textiles and clothing.