Micro-channel heat exchanger and preparation method and application thereof

Through alloy powder layering and prepressing technology, the problems of high processing cost of microchannel heat exchanger flow path plates and insufficient material selectivity are solved, and microchannel heat exchange with high strength, high corrosion resistance and high welding reliability are achieved It is suitable for a variety of corrosive media and high temperature and high pressure environments.

CN119085370AActive Publication Date: 2024-12-06SHAANXI ZHITUO SOLID PHASE ADDITIVE MFG TECH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202311515729.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-11-14
Publication Date
2024-12-06
Estimated Expiration
2043-11-14

AI Technical Summary

Technical Problem

In the existing micro-channel heat exchanger manufacturing process, the runner plate processing cost is high, the machining range is narrow, the diffusion welding process damages the material, and the processing materials are single, which limits the scale promotion of micro-channel heat exchangers.

Method used

The microchannel heat exchanger is prepared by layered laying and layered pre-pressing of alloy powder. Through the gradient arrangement of alloy powders of different compositions, the welding material system of diffusion welding technology is expanded, providing high strength, high corrosion resistance and high welding. Reliable micro-channel heat exchanger, suitable for corrosive media such as lead and bismuth and high-temperature and high-pressure fields such as supercritical carbon dioxide.

Benefits of technology

It reduces the cost of runner plate processing, expands the material category of microchannel heat exchangers, achieves high strength, high corrosion resistance, and high welding reliability, and is suitable for a variety of corrosive media and high temperature and high pressure environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119085370A_ABST
    Figure CN119085370A_ABST
Patent Text Reader

Abstract

The invention discloses a micro-channel heat exchanger and a preparation method and application thereof, and belongs to the technical field of micro-channel heat exchangers, the micro-channel heat exchanger is composed of a plurality of cold side plates, a plurality of hot side plates and a cover plate, the cold side plates and the hot side plates are sequentially stacked, and the cold side plates or the hot side plates comprise a plurality of parallel array micro-channels arranged at equal intervals; and the cold side plate or the hot side plate is formed by pressing a welding layer, a corrosion-resistant functional layer and a strength supporting layer. According to the technology for preparing the prefabricated runner plate through the alloy powder and the pre-pressing process, the assembly of microchannel heat exchanger material design is increased, and the heat exchanger design requirements of high strength, corrosion resistance, high heat conductivity and the like which cannot be completely achieved through conventional materials have the possibility of being integrated in the same heat exchanger to be achieved. And through gradient arrangement of the alloy powder, a weldable material system of the diffusion welding technology is expanded, and the material category of the micro-channel heat exchanger is expanded.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of microchannel heat exchangers, and in particular to a microchannel heat exchanger and a preparation method and application thereof. Background Art

[0002] A microchannel heat exchanger is an efficient and compact heat exchange device that achieves excellent heat transfer performance by transferring fluid in tiny channels. Microchannel heat exchangers have many advantages over traditional heat exchangers. Efficient heat exchange: The small size of the microchannel shortens the heat transfer distance between the fluid and the solid, thereby improving the heat transfer efficiency. Fast response: Due to its small size and low heat capacity, the microchannel heat exchanger can respond to temperature changes more quickly. Energy saving and environmental protection: Due to its efficient heat exchange characteristics, the microchannel heat exchanger can reduce the energy consumption of equipment operation and achieve energy conservation and emission reduction. Compact structure: The compact design of the microchannel heat exchanger makes it suitable for scenarios with limited space, such as automobiles, aerospace and other fields.

[0003] As a typical representative of microchannel heat exchangers, printed circuit board heat exchangers have higher reliability and broad application prospects in the fields of petroleum and chemical industry, gasification technology, aerospace, fuel cells and new energy. However, the high manufacturing cost has become the main factor hindering its widespread application.

[0004] Solid-phase additive manufacturing technology, also known as solid-state 3D printing or SSAM. Unlike traditional processing methods, solid-phase additive manufacturing technology builds three-dimensional objects by adding materials layer by layer, rather than removing materials to obtain the desired shape. Vacuum diffusion welding technology is the most widely used solid-phase additive manufacturing technology. It is a welding technology that forms a good joint at the interface of the welded workpieces through atomic diffusion under certain temperature, pressure and insulation time conditions. Because the welded workpieces do not melt and deform slightly during the welding process, it is a solid-phase welding method that is very suitable for constructing complex internal cavity structures. With the advancement of science and technology, diffusion welding is being widely used in aero-engine blades, compact microchannel heat exchangers, high heat flux density water cooling plates and other fields.

[0005] The manufacturing process of microchannel heat exchanger consists of several main parts: raw material plate processing - flow plate processing - diffusion welding - combination welding - product testing. The main processes for flow plate processing include chemical etching and mechanical processing. Mechanically processed microchannel plates are expensive and are currently only used in small quantities on difficult-to-etch materials such as high-temperature alloys and ceramics. Compared with mechanical processing, chemical etching is a process suitable for batch processing of flow plates. However, its processing cost is still higher than the demand for large-scale commercial promotion of microchannel heat exchangers. In addition, chemical etching is relatively mature for aluminum alloys, copper alloys, and stainless steel, while etching of high-temperature alloys, ceramics, etc. still cannot be achieved in industrial mass production, which seriously limits the scale promotion of microchannel heat exchangers.

[0006] The current manufacturing process of microchannel heat exchangers has disadvantages such as high channel plate processing cost, narrow range of processable materials (corrosion-resistant materials such as high-temperature alloys, ceramics, and Hastelloy alloys are not easy to process), great damage to materials during the diffusion welding process, and single processing materials. Summary of the invention

[0007] The purpose of the present invention is to overcome the defects of the prior art and provide a microchannel heat exchanger and a preparation method and application thereof.

[0008] The present invention solves the technical problem by adopting the following technical solutions.

[0009] The present invention provides a microchannel heat exchanger, which includes plates and cover plates that are alternately hot and cold and stacked in sequence, wherein the plates are composed of a base plate and grooves that are arranged at equal intervals along the width direction of the base plate, wherein the base plate is composed of a first welding area and a first corrosion-resistant area that are arranged at intervals, and the tops of two adjacent grooves are connected by a second welding area, and the projection of the second welding area on the base plate corresponds to the first welding area on the base plate, and the part between the base plate and the groove is composed of a support area and a second corrosion-resistant area on the surface of the support area. Under specific working conditions, the materials selected for the first welding area, the corrosion-resistant area, and the strength area are allowed to overlap.

[0010] The present invention also provides a method for preparing the above-mentioned microchannel heat exchanger, comprising: preparing the microchannel heat exchanger by layered laying and layered pre-pressing.

[0011] The present invention also provides an application of the above-mentioned microchannel heat exchanger in the field of high temperature and high pressure, and applies the microchannel heat exchanger to supercritical carbon dioxide heat exchange.

[0012] The present invention has the following beneficial effects:

[0013] The present invention provides a microchannel heat exchanger and its preparation method and application. The microchannel heat exchanger provided by the present invention includes plates and cover plates that are alternately hot and cold and stacked in sequence. The plates are composed of a substrate and grooves arranged at equal intervals along the width direction of the substrate, wherein the substrate is composed of a first welding area and a first corrosion-resistant area that are spaced apart, and the tops of two adjacent grooves are connected by a second welding area, and the projection of the second welding area on the substrate corresponds to the first welding area on the substrate, and the substrate and the grooves are composed of a support area and a second corrosion-resistant area on the surface of the support area. The above-mentioned microchannel heat exchanger provided by the present invention is prepared by layered laying and layered pre-pressing of alloy powders of different compositions. Through the gradient arrangement of the alloy powders, the weldable material system of the diffusion welding technology is expanded, and the material category of the microchannel heat exchanger is expanded, thereby providing a high-strength, high-corrosion-resistant, high-welding-reliability microchannel heat exchanger that can be used for corrosive media such as lead and bismuth, and it can be applied to heat exchange in high-temperature and high-pressure fields such as supercritical carbon dioxide. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0015] Figure 1 is a cross-sectional view of the heat exchanger core;

[0016] Figure 2 Different functional areas of the heat exchange plate;

[0017] Figure numbers: 1-1-cover plate, 1-2-cold side plate, 1-3-hot side plate, 2-1-first welding zone, 2-2-second welding zone, 2-3-first corrosion-resistant zone, 2-4-second corrosion-resistant zone, 2-5-support zone. DETAILED DESCRIPTION

[0018] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0019] A microchannel heat exchanger provided in an embodiment of the present invention and its preparation method and application are described in detail below.

[0020] In a first aspect, an embodiment of the present invention provides a microchannel heat exchanger, which includes plates and cover plates that are alternately hot and cold and stacked in sequence, wherein the plates are composed of a substrate and grooves arranged at equal intervals along the width direction of the substrate, wherein the substrate is composed of a first welding area and a first corrosion-resistant area that are spaced apart, and the tops of two adjacent grooves are connected by a second welding area, the projection of the second welding area on the substrate corresponds to the first welding area on the substrate, and the portion between the substrate and the groove is composed of a support area and a second corrosion-resistant area on the surface of the support area.

[0021] The microchannel heat exchanger designed in the embodiment of the present invention has a structure as follows Figure 1 As shown, the heat exchanger includes a cold side plate 1-2, a hot side plate 1-3, and a cover plate 1-1 stacked in sequence. The heat exchange plate (cold side plate or hot side plate) is pressed by powder, and its cross section is as follows Figure 2 As shown. According to the required functional characteristics, the heat exchange plate can be divided into the following areas: 2-1 first welding area, 2-2 second welding area, 2-3 first corrosion resistant area, 2-4 second corrosion resistant area, 2-5 support area.

[0022] In a second aspect, an embodiment of the present invention further provides a method for preparing the above-mentioned microchannel heat exchanger, comprising: preparing the microchannel heat exchanger by layered laying and layered pre-pressing.

[0023] In an optional embodiment, the steps are included: arranging easy-to-weld powder and corrosion-resistant powder at intervals and pre-pressing them once, then laying high-strength and high-temperature-resistant powder for a second pre-pressing of the flow channel shape, laying corrosion-resistant powder on the surface of the formed groove and pre-pressing it three times, and then laying easy-to-weld powder at the connection between the tops of two adjacent grooves and pre-pressing it four times, and then pre-pressing the whole five times to complete the plate production, and stacking the produced plates in sequence by alternating hot and cold, and then diffusion welding them after the stacking is completed, and finally welding the head and the connecting pipe to prepare a microchannel heat exchanger.

[0024] In an optional embodiment, the primary pre-pressing includes: arranging the easy-to-weld powder and the corrosion-resistant powder in the required mass ratio at intervals, and performing the primary pre-pressing with a pressing force of 10 to 50 MPa.

[0025] In an optional embodiment, the secondary pre-pressing, the tertiary pre-pressing, and the quadruple pre-pressing include: after the primary pre-pressing is completed, high-strength and high-temperature-resistant powder is laid, and the flow channel shape is pre-pressed using a special mold with a pressing force of 50-100MPa for the secondary pre-pressing; corrosion-resistant powder is laid on the surface of the formed groove with a pressing force of 20-70MPa for the third pre-pressing, and easy-to-weld powder is laid at the connection between the tops of two adjacent grooves with a pressing force of 20-70MPa for the fourth pre-pressing.

[0026] In an optional embodiment, the five pre-pressings include: after the surface is scanned and inspected to be qualified after four pre-pressings, the whole is pressed five times, and the pressing force is 120MPa to 250MPa.

[0027] In an optional embodiment, the easy-to-weld powder includes any one of 316L and pure nickel, the corrosion-resistant powder includes any one of FeAl3 and monel400, and the high-strength and high-temperature-resistant powder includes any one of 310S and inconel617.

[0028] In an optional embodiment, the number of powder layers for the first pre-pressing, the third pre-pressing, and the fourth pre-pressing is 1, the number of powder layers for the second pre-pressing is 5, and the thickness of each powder layer is 0.1-0.3 mm.

[0029] In an optional embodiment, after the first pre-pressing, the second pre-pressing, the third pre-pressing and the fourth pre-pressing are completed, the pre-pressing surface is purged to remove excess powder.

[0030] In an optional embodiment, the diffusion welding operation is as follows: the welding temperature is 1030±50°C, the heating rate is 2-10°C / min, the welding pressure is 2-15MPa, the insulation time is 1-8h, and rapid cooling is started after welding is completed to cool the workpiece to room temperature as soon as possible.

[0031] As can be seen from the above, an embodiment of the present invention provides a method for preparing a microchannel heat exchanger, and the preparation process is as follows: alloy powder is used as a unit for manufacturing, and the alloy powder is subjected to powder spreading, pressing, assembly, diffusion welding, combination welding and product inspection to prepare a microchannel heat exchanger, wherein the powder spreading and pressing processes can be repeated for multiple cycles.

[0032] The heat exchanger is manufactured by layered laying and layered pre-pressing. That is, the powder is laid from the bottom layer to the upper layer, and the thickness of each layer varies from 0.1 to 0.3 mm. The pre-pressure is generally 10 to 50 MPa, and the final pressing force is 120 MPa to 250 MPa. The pre-pressing adopts a relatively gentle vertical plane processing, and the final pressing can be carried out by hydraulic press plane pressing or rolling according to the equipment conditions. Depending on the type of powder, the pressing process can be carried out in vacuum or atmosphere to control the oxygen content in the powder.

[0033] After the channel plates are pressed, they are stacked in sequence and loaded into a vacuum diffusion welding furnace. The assembled microchannel heat exchanger core is welded, and a reasonable welding temperature is designed according to the material, and a reasonable insulation time and welding pressure are set according to the size of the microchannel heat exchanger core. After welding, the product core is sampled in the excess area, and the surface coloring is inspected to ensure the welding quality. The remaining pipes and heads are welded according to the heat exchanger design, and product testing is carried out.

[0034] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0035] Example 1

[0036] This embodiment designs an iron-based high-strength, high-corrosion-resistant, high-welding-reliability microchannel heat exchanger that can be used in corrosive media such as lead and bismuth, and can also be used in high-temperature and high-pressure fields such as supercritical dioxide. Figure 1 and Figure 2 , the preparation of the microchannel heat exchanger includes the following steps:

[0037] A special powder sieve is used to accurately lay a 0.3mm thick bottom powder, which consists of easy-to-weld powder 316L (corresponding to the first welding area 2-1 of the microchannel heat exchanger) and corrosion-resistant powder FeAl3 (corresponding to the first corrosion-resistant area 2-3 of the microchannel heat exchanger). They are arranged at intervals and pre-pressed after laying, with a pressing force of 50Mpa.

[0038] After compaction, high-strength and high-temperature resistant powder 310S (corresponding to the support area 2-5 of the microchannel heat exchanger) is laid in layers, with 5 layers of 0.3mm thickness per layer, and a special mold is used to pre-press the flow channel shape with a pre-tightening pressure of 60MPa. Use a shaping tool to scrape off excess powder, lay 0.3mm corrosion-resistant powder FeAl3 (corresponding to the second corrosion-resistant area 2-4 on the surface of the support area of ​​the microchannel heat exchanger) in the formed microchannel, and pre-press with a pre-tightening pressure of 30MPa. After pre-tightening, blow the pre-pressed surface to remove excess powder.

[0039] Easy-to-weld powder 316L is laid at the connection between two adjacent grooves (corresponding to the second welding area 2-2 of the microchannel heat exchanger) with a powder layer thickness of 0.3 mm and pressed to 30 MPa. After the pre-pressing is completed, the surface is purged.

[0040] Scan and inspect the surface after pre-pressing to confirm that there are no defects such as edge collapse and shrinkage holes.

[0041] The plate is finally pressed at a pressure of 190 MPa.

[0042] The pressed plates are stacked in sequence by alternating hot and cold methods, and after stacking, are placed in a vacuum diffusion welding furnace.

[0043] Turn on the diffusion welding furnace, set the parameters as welding temperature 1030℃, heating rate 5℃ / min, welding pressure 10MPa, and holding time 3h, weld the product, and turn on fast cooling after welding to cool the workpiece to room temperature as soon as possible.

[0044] After welding is completed, metallographic and mechanical properties test samples are taken from the excess area to observe whether they meet the design requirements. Fluorescence detection is also performed on the welding surface to observe whether there are any welding cracks.

[0045] Weld the heads and pipes, and perform pressure tests after welding to confirm that the products meet the design requirements.

[0046] Example 2

[0047] This embodiment designs an iron-based high-strength, high-corrosion-resistant, high-welding-reliability microchannel heat exchanger that can be used in corrosive media such as lead and bismuth, and can also be used in high-temperature and high-pressure fields such as supercritical dioxide. Figure 1 and Figure 2 , the preparation of the microchannel heat exchanger includes the following steps:

[0048] A special powder sieve is used to accurately lay the 0.3mm thick bottom powder, which consists of easy-to-weld powder 316L (corresponding to the first welding area 2-1 of the microchannel heat exchanger) and corrosion-resistant powder FeAl3 (corresponding to the first corrosion-resistant area 2-3 of the microchannel heat exchanger). They are arranged at intervals and pre-pressed after laying, with a pressing force of 30Mpa.

[0049] After compaction, high-strength and high-temperature resistant powder 310S (corresponding to the support area 2-5 of the microchannel heat exchanger) is laid in layers, with 5 layers of 0.3mm thickness per layer, and a special mold is used to pre-press the flow channel shape with a pre-tightening pressure of 150MPa. Use a shaping tool to scrape off excess powder, lay 0.3mm corrosion-resistant powder FeAl3 (corresponding to the second corrosion-resistant area 2-4 on the surface of the support area of ​​the microchannel heat exchanger) in the formed microchannel, and pre-press with a pre-tightening pressure of 70MPa. After pre-tightening, blow the pre-pressed surface to remove excess powder.

[0050] Easy-to-weld powder 316L is laid at the connection between two adjacent grooves (corresponding to the second welding area 2-2 of the microchannel heat exchanger) with a powder layer thickness of 0.3 mm and pressed to 70 MPa. After the pre-pressing is completed, the surface is purged.

[0051] Scan and inspect the surface after pre-pressing to confirm that there are no defects such as edge collapse and shrinkage holes.

[0052] The plate is finally pressed at a pressure of 250 MPa.

[0053] The pressed plates are stacked in sequence by alternating hot and cold methods, and after stacking, are placed in a vacuum diffusion welding furnace.

[0054] Turn on the diffusion welding furnace, set the parameters as welding temperature 1080℃, heating rate 10℃ / min, welding pressure 15MPa, and holding time 8h, weld the product, and turn on fast cooling after welding to cool the workpiece to room temperature as soon as possible.

[0055] After welding is completed, metallographic and mechanical properties test samples are taken from the excess area to observe whether they meet the design requirements. Fluorescence detection is also performed on the welding surface to observe whether there are any welding cracks.

[0056] Weld the heads and pipes, and perform pressure tests after welding to confirm that the products meet the design requirements.

[0057] Example 3

[0058] This embodiment designs a nickel-based high-strength, high-corrosion-resistant, high-welding-reliability microchannel heat exchanger that can be used in corrosive media such as lead and bismuth, and can also be used in high-temperature and high-pressure fields such as supercritical dioxide. Figure 1 and Figure 2 , the preparation of the microchannel heat exchanger includes the following steps:

[0059] A special powder sieve is used to accurately lay a 0.1mm thick bottom powder, which is composed of easy-to-weld pure nickel powder (corresponding to the first welding area 2-1 of the microchannel heat exchanger) and monel400 (monel alloy) (corresponding to the first corrosion-resistant area 2-3 of the microchannel heat exchanger). The powder is arranged at intervals and pre-pressed after laying, with a pressing force of 50Mpa.

[0060] After compaction, high-strength and high-temperature-resistant powder inconel617 (corresponding to the support area 2-5 of the microchannel heat exchanger) is laid in layers, with 5 layers of 0.3mm thickness per layer, and a special mold is used to pre-press the flow channel shape, with a pre-tightening pressure of 60MPa. Use a shaping tool to scrape off excess powder, lay 0.3mm corrosion-resistant powder monel400 (corresponding to the second corrosion-resistant area 2-4 on the surface of the support area of ​​the microchannel heat exchanger) in the formed microchannel, and pre-press it, with a pre-tightening pressure of 30MPa. After pre-tightening, blow the pre-pressed surface to remove excess powder.

[0061] Easy-to-weld pure nickel powder is laid at the connection between two adjacent grooves (corresponding to the second welding area 2-2 of the microchannel heat exchanger) with a powder layer thickness of 0.1 mm and pressed to 30 MPa. After the pre-pressing is completed, the surface is purged.

[0062] Scan and inspect the surface after pre-pressing to confirm that there are no defects such as edge collapse and shrinkage holes.

[0063] The plate is finally pressed at a pressure of 190 MPa.

[0064] The pressed plates are stacked in sequence by alternating hot and cold methods, and after stacking, are placed in a vacuum diffusion welding furnace.

[0065] Turn on the diffusion welding furnace, set the parameters as welding temperature 1030℃, heating rate 5℃ / min, welding pressure 10MPa, and holding time 3h, weld the product, and turn on fast cooling after welding to cool the workpiece to room temperature as soon as possible.

[0066] After welding is completed, metallographic and mechanical properties test samples are taken from the excess area to observe whether they meet the design requirements. Fluorescence detection is also performed on the welding surface to observe whether there are any welding cracks.

[0067] Weld the heads and pipes, and perform pressure tests after welding to confirm that the products meet the design requirements.

[0068] Example 4

[0069] This embodiment designs a nickel-based high-strength, high-corrosion-resistant, high-welding-reliability microchannel heat exchanger that can be used in corrosive media such as lead and bismuth, and can also be used in high-temperature and high-pressure fields such as supercritical dioxide. Figure 1 and Figure 2, the preparation of the microchannel heat exchanger includes the following steps:

[0070] A special powder sieve is used to accurately lay a 0.1mm thick bottom powder, which is composed of easy-to-weld pure nickel powder (corresponding to the first welding area 2-1 of the microchannel heat exchanger) and monel400 (monel alloy) (corresponding to the first corrosion-resistant area 2-3 of the microchannel heat exchanger). The powder is arranged at intervals and pre-pressed after laying, with a pressing force of 50Mpa.

[0071] After compaction, high-strength and high-temperature-resistant powder inconel617 (corresponding to the support area 2-5 of the microchannel heat exchanger) is laid in layers, with 5 layers of 0.3mm thickness per layer, and a special mold is used to pre-press the flow channel shape, with a pre-tightening pressure of 100MPa. Use a shaping tool to scrape off excess powder, lay 0.3mm corrosion-resistant powder monel400 (corresponding to the second corrosion-resistant area 2-4 on the surface of the support area of ​​the microchannel heat exchanger) in the formed microchannel, and pre-press it, with a pre-tightening pressure of 70MPa. After pre-tightening, blow the pre-pressed surface to remove excess powder.

[0072] Easy-to-weld pure nickel powder is laid at the connection between two adjacent grooves (corresponding to the second welding area 2-2 of the microchannel heat exchanger) with a powder layer thickness of 0.1 mm and pressed to 70 MPa. After the pre-pressing is completed, the surface is purged.

[0073] Scan and inspect the surface after pre-pressing to confirm that there are no defects such as edge collapse and shrinkage holes.

[0074] The plate is finally pressed at a pressure of 250 MPa.

[0075] The pressed plates are stacked in sequence by alternating hot and cold methods, and after stacking, are placed in a vacuum diffusion welding furnace.

[0076] Turn on the diffusion welding furnace, set the parameters as welding temperature 1080℃, heating rate 10℃ / min, welding pressure 15MPa, and holding time 8h, weld the product, and turn on fast cooling after welding to cool the workpiece to room temperature as soon as possible.

[0077] After welding is completed, metallographic and mechanical properties test samples are taken from the excess area to observe whether they meet the design requirements. Fluorescence detection is also performed on the welding surface to observe whether there are any welding cracks.

[0078] Weld the heads and pipes, and perform pressure tests after welding to confirm that the products meet the design requirements.

[0079] Compared with the prior art, the present invention has the following beneficial effects:

[0080] 1. The present invention adopts alloy powder + pre-pressing process to prepare the prefabricated flow channel plate, which completely gets rid of the selectivity of the etching process to the material;

[0081] 2. The present invention adopts alloy powder + pre-pressing process to prepare the prefabricated flow channel plate, without etching consumables, processing tools and other consumables, which greatly reduces the processing cost of the flow channel plate.

[0082] 3. The alloy powder + pre-pressing process used in the present invention to prepare the prefabricated flow channel plate technology increases the combination of microchannel heat exchanger material design, making it possible to combine the heat exchanger design requirements such as high strength, corrosion resistance, and high thermal conductivity that cannot be fully achieved by conventional materials into the same heat exchanger.

[0083] 4. By fine-tuning the ratio of elements in the alloy powder, the degradation of the base material properties caused by too long holding time or too high welding temperature during diffusion welding can be greatly reduced.

[0084] 5. Through the gradient arrangement of alloy powder, the weldable material system of diffusion welding technology is expanded, and the material category of microchannel heat exchanger is expanded.

[0085] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A microchannel heat exchanger, It is characterized in that The microchannel heat exchanger includes plates and cover plates that are alternately hot and cold and stacked in sequence, wherein the plates are composed of a base plate and grooves arranged at equal intervals along the width direction of the base plate, wherein the base plate is composed of a first welding area and a first corrosion-resistant area that are spaced apart, and the tops of two adjacent grooves are connected by a second welding area, a projection of the second welding area on the base plate corresponds to the first welding area on the base plate, and the portion between the base plate and the groove is composed of a support area and a second corrosion-resistant area on the surface of the support area.

2. A method for preparing the microchannel heat exchanger according to claim 1, It is characterized in that The microchannel heat exchanger is prepared by layered laying and layered pre-pressing.

3. The preparation method according to claim 2, It is characterized in that The method comprises the following steps: arranging easy-to-weld powder and corrosion-resistant powder at intervals and pre-pressing them once, then laying high-strength and high-temperature-resistant powder for secondary pre-pressing of the flow channel shape, laying corrosion-resistant powder on the surface of the formed groove and pre-pressing them three times, laying easy-to-weld powder at the connection between the tops of two adjacent grooves and pre-pressing them four times, and then pre-pressing the whole five times to complete the plate production, stacking the produced plates in sequence by alternating hot and cold, and then diffusion welding them after the stacking is completed, and finally welding the heads and the connecting pipes to prepare the microchannel heat exchanger.

4. The preparation method according to claim 3, It is characterized in that The primary pre-pressing comprises: arranging the easy-to-weld powder and the corrosion-resistant powder in the required mass ratio at intervals, and performing the primary pre-pressing with a pressing force of 10 to 50 MPa.

5. The preparation method according to claim 3, It is characterized in that The secondary pre-pressing, tertiary pre-pressing and quadruple pre-pressing include: after the primary pre-pressing is completed, high-strength and high-temperature-resistant powder is laid, and the flow channel shape is pre-pressed using a special mold with a pressing force of 50-100MPa for secondary pre-pressing; corrosion-resistant powder is laid on the surface of the formed groove with a pressing force of 20-70MPa for third pre-pressing, and easy-to-weld powder is laid at the connection between the tops of two adjacent grooves with a pressing force of 20-70MPa for fourth pre-pressing.

6. The preparation method according to claim 3, It is characterized in that The five pre-pressings include: after the surface is scanned and inspected to be qualified after four pre-pressings, the whole is pressed five times, and the pressing force is 120MPa to 250MPa.

7. The preparation method according to claim 3, It is characterized in that The easy-to-weld powder includes any one of 316L and pure nickel, and the corrosion-resistant powder includes FeAl 3 and any one of monel400, and any one of the high-strength and high-temperature-resistant powder 310S and inconel617.

8. The preparation method according to claim 3, It is characterized in that The number of powder layers for the first pre-pressing, the third pre-pressing, and the fourth pre-pressing is 1, the number of powder layers for the second pre-pressing is 5, and the thickness of each powder layer is 0.1-0.3mm. After the first pre-pressing, the second pre-pressing, the third pre-pressing, and the fourth pre-pressing are completed, the pre-pressing surface is purged to remove excess powder.

9. The preparation method according to claim 3, It is characterized in that The diffusion welding operation is as follows: the welding temperature is 1030±50°C, the heating rate is 2-10°C / min, the welding pressure is 2-15MPa, the insulation time is 1-8h, and after the welding is completed, fast cooling is turned on to cool the workpiece to room temperature as soon as possible.

10. Application of the microchannel heat exchanger according to claim 1 or the microchannel heat exchanger prepared by the preparation method according to any one of claims 2 to 9 in the field of high temperature and high pressure, It is characterized in that The microchannel heat exchanger is applied to supercritical carbon dioxide heat exchange.

Citation Information

Patent Citations

  • End face forming sealed plate heat exchanger

    CN101089535A

  • Double-side etching high-temperature and high-pressure printed circuit board heat exchanger

    CN105043144A

  • Brazed heat exchanger with high pressure resistance and high heat exchange rate

    CN112033192A

  • Heat exchanger and manufacturing method

    CN115265242A

  • Diffusion welding compact type heat exchanger with combined heat exchange plates

    CN212482206U