Preparation method of quick-drying residual chlorine detection test paper and residual chlorine detection test paper
By using the combination of liquid absorbing fiber layer and bonding layer and needle-punching treatment in the residual chlorine detection test paper, the problem of contamination of color-producing test paper in the undry color-developed test paper was solved, and the rapid drying and sufficient reaction residual chlorine detection test paper was achieved. Ensures the speed and accuracy of the detection.
Patent Information
- Application Number
- CN202411050102.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-12-06
AI Technical Summary
Existing residual chlorine detection papers are prone to contamination of the colorimetric card when they are not dry and colored, resulting in inaccurate detection data, and the substrate setting cannot completely avoid liquid applying to the colorimetric card, affecting the comparison results.
The liquid absorbing fiber layer is placed under the detection layer, and the bonding layer is used as a barrier layer and binder, and the fiber tangle point is formed in combination with acupuncture treatment to control the liquid absorption rate, achieve a quick drying effect and ensure the adequacy of the color development reaction. .
The quick-drying function of residual chlorine detection test strips is realized, which avoids liquid contamination and colorimetric card, and ensures the accuracy and speed of the test results.
Smart Images

Figure BDA0004974668300000081 
Figure BDA0004974668300000091
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of test papers, in particular to a preparation method of a quick-drying residual chlorine test paper and the residual chlorine test paper. Background Art
[0002] Chlorination disinfection is a commonly used technical means in water treatment, but after chlorination disinfection, the water will contain free residual chlorine composed of chlorine molecules. Excessive residual chlorine content in the water will be harmful to human health. Therefore, the residual chlorine content in the water needs to be tested after chlorination disinfection.
[0003] The residual chlorine test method in the prior art mainly adopts residual chlorine detector and colorimetry, but the residual chlorine detector and colorimetry need to adopt devices and equipment, and also need to configure solvent solution. The detection is time-consuming and laborious and requires professional personnel to operate, and it is impossible to perform rapid detection. Therefore, in order to be able to quickly detect residual chlorine, personnel in the field have disclosed a residual chlorine detection test paper, which loads the color developer onto a carrier and then seals and packages it. When in use, the solution to be tested is dropped onto the residual chlorine detection test paper for color development reaction, and after the reaction, it is visually compared with the standard colorimetric card to determine the residual chlorine content; such as a semi-quantitative detection method for total residual chlorine in water disclosed in Publication No. CN111610184A, and another such as a preparation method and application of a water quality residual chlorine and total chlorine detection test paper disclosed in Publication No. CN114460070A; the current residual chlorine detection test paper is simple to operate, easy to carry, does not require professional personnel to operate, and can quickly detect the liquid to be tested. The residual chlorine content in the residual chlorine test paper is measured; in order to more clearly compare the difference between the test paper and the colorimetric card after color development during use of the residual chlorine test paper, the colorimetric test paper is usually attached to the colorimetric card for comparison. When it is necessary to quickly detect, the color developer on the undried colorimetric test paper will be smeared on the colorimetric card, affecting the accuracy of the comparison data and contaminating the standard colorimetric card. Therefore, in order to avoid the above problems, a substrate is arranged at the bottom of the colorimetric test paper in the prior art, and the colorimetric test paper is loaded on the substrate to avoid the undried colorimetric test paper from contaminating the colorimetric card. Although the substrate can reduce the frequency of the above problems to a certain extent, the substrate is usually arranged with a larger area than the test paper to be tested in order to achieve the above effects. An overly large substrate will form color interference between the colorimetric card and the test paper to be tested during comparison, and the liquid on the test paper to be tested will still be smeared on the colorimetric card when the operation is improper, and the influence of the undried colorimetric test paper on the colorimetric card cannot be completely avoided. Summary of the invention
[0004] The invention aims at the problem that the undried residual chlorine colorimetric test paper in the prior art is easy to contaminate the colorimetric card during detection, and provides a preparation method of a quick-drying residual chlorine detection test paper and the residual chlorine detection test paper. The preparation method adopts a liquid-absorbing fiber layer placed below the detection layer, so that the liquid to be tested in the detection layer is absorbed by the liquid-absorbing fiber layer, so that the residual chlorine detection test paper can achieve the technical effect of quick drying. The bonding layer reagent in the method can be used as a bonding agent for the water-absorbing fiber layer and the detection layer, and can also be used as a barrier layer between the liquid-absorbing fiber layer and the detection layer after compounding, so as to block the liquid to be tested from directly contacting the liquid-absorbing fiber layer, so as to avoid the liquid to be tested being absorbed by the liquid-absorbing fiber layer before it is fully reacted. Then, the fibers of the liquid-absorbing fiber layer are pierced into the detection layer through a needle puncture treatment to form entanglement points, and the fibers of the entanglement points can be used as liquid-absorbing anchor points to absorb the liquid to be tested into the washing liquid fiber layer, so that the quick-drying residual chlorine detection test paper can achieve quick drying and ensure the full reaction of the color development reaction.
[0005] The specific technical scheme of the present invention is: A method for preparing a quick-drying residual chlorine detection test paper comprises the following preparation steps: soaking a test paper substrate with a color developing reagent and then drying it to form a detection layer; coating a binder on the surface of a liquid-absorbing fiber layer and then cooling it together with the detection layer to form a germ layer; and performing a needle-puncture treatment from the liquid-absorbing fiber layer to the detection layer to form the quick-drying residual chlorine detection test paper.
[0006] The invention provides a preparation method of a quick-drying residual chlorine detection test paper. The method adopts a liquid-absorbing fiber layer disposed below a detection layer, and the liquid-absorbing fiber layer absorbs the test liquid on the detection layer to realize quick drying of the residual chlorine detection test paper, so that the residual chlorine detection test paper can not contaminate a colorimetric card when performing a quick comparison. In addition, when designing the present application, it is found that when the liquid-absorbing fiber layer and the detection layer are directly compounded with an adhesive, if the adhesive forms a complete barrier between the liquid-absorbing fiber layer and the detection layer, the liquid-absorbing fiber layer will not be able to absorb the liquid of the detection layer. Therefore, it is necessary to prevent the adhesive from forming a complete barrier between the liquid-absorbing fiber layer and the detection layer. At the same time, if the adhesive layer does not directly form a barrier between the liquid-absorbing fiber layer and the detection layer, the liquid-absorbing fiber layer will quickly absorb the liquid of the detection layer, resulting in the detection layer not having a complete color development reaction and the liquid to be tested being completely absorbed. Therefore, controlling the liquid absorption rate of the washing liquid fiber layer to ensure a sufficient color development reaction of the detection layer is the key to the present application.
[0007] In view of the above content, the present invention is designed to first completely block the liquid-absorbing fiber layer and the detection layer through an adhesive layer, and then the fibers of the liquid-absorbing fiber layer pass through the adhesive layer formed by the adhesive to enter the detection layer. Therefore, the present invention adopts a needle-punching treatment to pierce the fibers of the liquid-absorbing fiber layer into the detection layer. The fibers of the liquid-absorbing fiber layer will form fiber entanglement points in the detection layer, and the fiber entanglement points will serve as water absorption anchor points to absorb the liquid in the detection layer into the liquid-absorbing fiber layer. By controlling the number of fiber entanglement points, the liquid absorption rate can also be controlled, so that the detection layer can fully perform a color development reaction and absorb the liquid in the detection layer into the liquid-absorbing fiber layer, thereby achieving quick drying of the residual chlorine detection test paper.
[0008] Preferably, the raw material of the liquid-absorbing fiber layer is one or more of polypropylene fiber or polyacrylonitrile fiber.
[0009] Preferably, the test paper substrate is one of filter paper and chromatography test paper.
[0010] Preferably, the coating thickness of the binder is 2 to 5 μm. The present invention optimizes the binder. The present application is used for rapid detection of residual chlorine. The acidity and oxidizability of the residual chlorine test liquid are relatively high. Therefore, it is necessary to select an acid-resistant and oxidizing binder to ensure that it will not be corroded by the test liquid during the residual chlorine detection process. In addition, the coating thickness also needs to be optimized to ensure the integrity of the membrane, while ensuring that the fibers of the liquid-absorbing fiber layer can be pierced into the detection layer after puncture, and that fiber entanglement points can be formed in the detection layer.
[0011] Preferably, the needle punching treatment is performed under the following conditions: the needle spacing is 5 to 50 mm; by controlling the needle spacing, the number of fiber entanglement points formed can be controlled, thereby controlling the liquid absorption rate of the liquid-absorbent fiber layer.
[0012] Preferably, the color developing reagent is TMB, a dispersant and a buffer.
[0013] Preferably, the pH value of the buffer solution is 6.2-7.0.
[0014] Preferably, the buffer is a phosphate buffer.
[0015] Preferably, the dispersant is polyvinyl pyrrolidone.
[0016] A quick-drying residual chlorine detection test paper is prepared by the preparation method of the quick-drying residual chlorine detection test paper. The residual chlorine detection test paper comprises a liquid-absorbing fiber layer, a bonding layer and a detection layer from bottom to top, and the fibers of the liquid-absorbing fiber layer are entangled with the fibers of the detection layer.
[0017] Compared with the prior art, this application has the following technical effects: The invention provides a preparation method of a quick-drying residual chlorine detection test paper and the residual chlorine detection test paper. The preparation method adopts a liquid-absorbing fiber layer disposed below a detection layer, so that a liquid to be detected in the detection layer is absorbed by the liquid-absorbing fiber layer, so that the residual chlorine detection test paper can achieve a technical effect of quick drying. The bonding layer reagent in the method can be used as a bonding agent for the water-absorbing fiber layer and the detection layer, and can also be used as a barrier layer between the liquid-absorbing fiber layer and the detection layer after compounding, so as to block the liquid to be detected from directly contacting the liquid-absorbing fiber layer, so as to avoid the liquid to be detected being absorbed by the liquid-absorbing fiber layer before being fully reacted. Then, the fibers of the liquid-absorbing fiber layer are pierced into the detection layer through a needle puncture treatment to form entanglement points, and the fibers of the entanglement points can be used as liquid-absorbing anchor points to absorb the liquid to be detected into the washing liquid fiber layer, so that the quick-drying residual chlorine detection test paper can achieve quick drying and ensure the full reaction of the color development reaction. DETAILED DESCRIPTION
[0018] The present invention will be further described below in conjunction with the embodiments.
[0019] Embodiment 1: A method for preparing a quick-drying residual chlorine detection test paper comprises the following steps: Preparation of the detection layer: 1.5 g / kg TMB, 3 g / kg polyvinyl pyrrolidone (PVP-K90) and 100 mM phosphate buffer were mixed to prepare a colorimetric reagent, and the filter paper was soaked in the colorimetric reagent. After the soaking was complete, the filter paper was taken out and placed in a drying oven at 70° C. to dry to prepare the detection layer; Preparation of germ layer: melt the adhesive (EVA hot melt adhesive) and apply it on the surface of the liquid-absorbing fiber layer (water-absorbing PP polyester non-woven fabric), laminate the detection layer and the lotion fiber layer coated with the adhesive, and then press and cool them under a roller press to form the germ layer; Preparation of quick-drying residual chlorine test paper: Place the germ layer on a needle puncture lathe for needle puncture treatment, with the liquid absorbing fiber layer side of the germ layer facing up and the detection layer side facing down. The conditions for the needle puncture treatment are: the needle puncture direction is from the liquid absorbing fiber layer to the detection layer, and the needle interval is 5 mm.
[0020] A residual chlorine detection test paper prepared by the above-mentioned quick-drying residual chlorine detection test paper preparation method comprises, from bottom to top, a liquid-absorbing fiber layer, a bonding layer and a detection layer, the length of the residual chlorine detection paper is 5 cm, the width is 0.5 cm, the thickness of the liquid-absorbing fiber layer is 0.2 mm, the thickness of the bonding layer is 2 μm, and the thickness of the detection layer is 0.2 mm.
[0021] Embodiment 2: A method for preparing a quick-drying residual chlorine detection test paper comprises the following steps: Preparation of the detection layer: 1.5 g / kg TMB, 3 g / kg polyvinyl pyrrolidone (PVP-K90) and 100 mM phosphate buffer were mixed to prepare a colorimetric reagent, and the filter paper was soaked in the colorimetric reagent. After the soaking was complete, the filter paper was taken out and placed in a drying oven at 70° C. to dry to prepare the detection layer; Preparation of germ layer: melt the adhesive (EVA hot melt adhesive) and apply it on the surface of the liquid-absorbing fiber layer (water-absorbing PP polyester non-woven fabric), laminate the detection layer and the lotion fiber layer coated with the adhesive, and then press and cool them under a roller press to form the germ layer; Preparation of quick-drying residual chlorine test paper: Place the germ layer on a needle puncture lathe for needle puncture treatment, with the liquid absorbing fiber layer side of the germ layer facing up and the detection layer side facing down. The conditions for the needle puncture treatment are: the needle puncture direction is from the liquid absorbing fiber layer to the detection layer, and the needle interval is 10 mm.
[0022] A residual chlorine detection test paper prepared by the above-mentioned quick-drying residual chlorine detection test paper preparation method comprises, from bottom to top, a liquid-absorbing fiber layer, a bonding layer and a detection layer, the residual chlorine detection paper is 5 cm long and 0.5 cm wide, the liquid-absorbing fiber layer is 0.2 mm thick, the bonding layer is 3 μm thick, and the detection layer is 0.2 mm thick.
[0023] Embodiment 3: A method for preparing a quick-drying residual chlorine detection test paper comprises the following steps: Preparation of the detection layer: 1.5 g / kg TMB, 3 g / kg polyvinyl pyrrolidone (PVP-K90) and 100 mM phosphate buffer were mixed to prepare a colorimetric reagent, and the filter paper was soaked in the colorimetric reagent. After the soaking was complete, the filter paper was taken out and placed in a drying oven at 70° C. to dry to prepare the detection layer; Preparation of germ layer: melt the adhesive (EVA hot melt adhesive) and apply it on the surface of the liquid-absorbing fiber layer (water-absorbing PP polyester non-woven fabric), laminate the detection layer and the lotion fiber layer coated with the adhesive, and then press and cool them under a roller press to form the germ layer; Preparation of quick-drying residual chlorine test paper: Place the germ layer on a needle puncture lathe for needle puncture treatment, with the liquid absorbing fiber layer side of the germ layer facing up and the detection layer side facing down. The conditions for the needle puncture treatment are: the needle puncture direction is from the liquid absorbing fiber layer to the detection layer, and the needle interval is 15 mm.
[0024] A residual chlorine detection test paper prepared by the above-mentioned quick-drying residual chlorine detection test paper preparation method comprises, from bottom to top, a liquid-absorbing fiber layer, a bonding layer and a detection layer. The residual chlorine detection test paper is 5 cm long and 0.5 cm wide, the liquid-absorbing fiber layer is 0.2 mm thick, the bonding layer is 4 μm thick, and the detection layer is 0.2 mm thick.
[0025] Embodiment 4: A method for preparing a quick-drying residual chlorine detection test paper comprises the following steps: Preparation of the detection layer: 1.5 g / kg TMB, 3 g / kg polyvinyl pyrrolidone (PVP-K90) and 100 mM phosphate buffer were mixed to prepare a colorimetric reagent, and the filter paper was soaked in the colorimetric reagent. After the soaking was complete, the filter paper was taken out and placed in a drying oven at 70° C. to dry to prepare the detection layer; Preparation of germ layer: melt the adhesive (EVA hot melt adhesive) and apply it on the surface of the liquid-absorbing fiber layer (water-absorbing PP / PE polyester non-woven fabric), laminate the detection layer and the lotion fiber layer coated with the adhesive, and then place them under a roller press to press and cool to form the germ layer; Preparation of quick-drying residual chlorine test paper: Place the germ layer on a needle puncture lathe for needle puncture treatment, with the liquid absorbing fiber layer side of the germ layer facing up and the detection layer side facing down. The conditions for the needle puncture treatment are: the needle puncture direction is from the liquid absorbing fiber layer to the detection layer, and the needle interval is 20 mm.
[0026] A residual chlorine detection test paper prepared by the above-mentioned quick-drying residual chlorine detection test paper preparation method comprises, from bottom to top, a liquid-absorbing fiber layer, a bonding layer and a detection layer, the residual chlorine detection paper is 5 cm long and 0.5 cm wide, the liquid-absorbing fiber layer is 0.2 mm thick, the bonding layer is 5 μm thick, and the detection layer is 0.2 mm thick.
[0027] Embodiment 5: A method for preparing a quick-drying residual chlorine detection test paper comprises the following steps: Preparation of the detection layer: 1.5 g / kg TMB, 3 g / kg polyvinyl pyrrolidone (PVP-K90) and 100 mM phosphate buffer were mixed to prepare a colorimetric reagent, and the filter paper was soaked in the colorimetric reagent. After the soaking was complete, the filter paper was taken out and placed in a drying oven at 70° C. to dry to prepare the detection layer; Preparation of germ layer: melt the adhesive (EVA hot melt adhesive) and apply it on the surface of the liquid absorbing fiber layer (water-absorbing PE polyester non-woven fabric), laminate the detection layer and the lotion fiber layer coated with the adhesive, and then press and cool them under a roller press to form the germ layer; Preparation of quick-drying residual chlorine test paper: Place the germ layer on a needle puncture lathe for needle puncture treatment, with the liquid absorbing fiber layer side of the germ layer facing up and the detection layer side facing down. The conditions for the needle puncture treatment are: the needle puncture direction is from the liquid absorbing fiber layer to the detection layer, and the needle spacing is 25 mm.
[0028] A residual chlorine detection test paper prepared by the above-mentioned quick-drying residual chlorine detection test paper preparation method comprises, from bottom to top, a liquid-absorbing fiber layer, a bonding layer and a detection layer, the residual chlorine detection paper is 5 cm long and 0.5 cm wide, the liquid-absorbing fiber layer is 0.2 mm thick, the bonding layer is 5 μm thick, and the detection layer is 0.2 mm thick.
[0029] Embodiment 6: A method for preparing a quick-drying residual chlorine detection test paper comprises the following steps: Preparation of the detection layer: 1.5 g / kg TMB, 3 g / kg polyvinyl pyrrolidone (PVP-K90) and 100 mM phosphate buffer were mixed to prepare a colorimetric reagent, and the filter paper was soaked in the colorimetric reagent. After the soaking was complete, the filter paper was taken out and placed in a drying oven at 70° C. to dry to prepare the detection layer; Preparation of germ layer: melt the adhesive (EVA hot melt adhesive) and apply it on the surface of the liquid-absorbing fiber layer (water-absorbing PP polyester non-woven fabric), laminate the detection layer and the lotion fiber layer coated with the adhesive, and then press and cool them under a roller press to form the germ layer; Preparation of quick-drying residual chlorine test paper: Place the germ layer on a needle puncture lathe for needle puncture treatment, with the liquid absorbing fiber layer side of the germ layer facing up and the detection layer side facing down. The conditions for the needle puncture treatment are: the needle puncture direction is from the liquid absorbing fiber layer to the detection layer, and the needle interval is 30 mm.
[0030] A residual chlorine detection test paper prepared by the above-mentioned quick-drying residual chlorine detection test paper preparation method comprises, from bottom to top, a liquid-absorbing fiber layer, a bonding layer and a detection layer, the residual chlorine detection paper is 5 cm long and 0.5 cm wide, the liquid-absorbing fiber layer is 0.2 mm thick, the bonding layer is 5 μm thick, and the detection layer is 0.2 mm thick.
[0031] Embodiment 7: A method for preparing a quick-drying residual chlorine detection test paper comprises the following steps: Preparation of the detection layer: 1.5 g / kg TMB, 3 g / kg polyvinyl pyrrolidone (PVP-K90) and 100 mM phosphate buffer were mixed to prepare a colorimetric reagent, and the filter paper was soaked in the colorimetric reagent. After the soaking was complete, the filter paper was taken out and placed in a drying oven at 70° C. to dry to prepare the detection layer; Preparation of germ layer: melt the adhesive (EVA hot melt adhesive) and apply it on the surface of the liquid absorbing fiber layer (water-absorbing PE polyester non-woven fabric), laminate the detection layer and the lotion fiber layer coated with the adhesive, and then press and cool them under a roller press to form the germ layer; Preparation of quick-drying residual chlorine test paper: Place the germ layer on a needle puncture lathe for needle puncture treatment, with the liquid absorbing fiber layer side of the germ layer facing up and the detection layer side facing down. The conditions for the needle puncture treatment are: the needle puncture direction is from the liquid absorbing fiber layer to the detection layer, and the needle spacing is 35 mm.
[0032] A residual chlorine detection test paper prepared by the above-mentioned quick-drying residual chlorine detection test paper preparation method comprises, from bottom to top, a liquid-absorbing fiber layer, a bonding layer and a detection layer, the residual chlorine detection paper is 5 cm long and 0.5 cm wide, the liquid-absorbing fiber layer is 0.2 mm thick, the bonding layer is 5 μm thick, and the detection layer is 0.2 mm thick.
[0033] Embodiment 8: A method for preparing a quick-drying residual chlorine detection test paper comprises the following steps: Preparation of the detection layer: 1.5 g / kg TMB, 3 g / kg polyvinyl pyrrolidone (PVP-K90) and 100 mM phosphate buffer were mixed to prepare a colorimetric reagent, and the filter paper was soaked in the colorimetric reagent. After the soaking was complete, the filter paper was taken out and placed in a drying oven at 70° C. to dry to prepare the detection layer; Preparation of germ layer: melt the adhesive (EVA hot melt adhesive) and apply it on the surface of the liquid-absorbing fiber layer (water-absorbing PP polyester non-woven fabric), laminate the detection layer and the lotion fiber layer coated with the adhesive, and then press and cool them under a roller press to form the germ layer; Preparation of quick-drying residual chlorine test paper: Place the germ layer on a needle puncture lathe for needle puncture treatment, with the liquid absorbing fiber layer side of the germ layer facing up and the detection layer side facing down. The conditions for the needle puncture treatment are: the needle puncture direction is from the liquid absorbing fiber layer to the detection layer, and the needle interval is 40 mm.
[0034] A residual chlorine detection test paper prepared by the above-mentioned quick-drying residual chlorine detection test paper preparation method comprises, from bottom to top, a liquid-absorbing fiber layer, a bonding layer and a detection layer, the residual chlorine detection paper is 5 cm long and 0.5 cm wide, the liquid-absorbing fiber layer is 0.2 mm thick, the bonding layer is 5 μm thick, and the detection layer is 0.2 mm thick.
[0035] Embodiment 9: A method for preparing a quick-drying residual chlorine detection test paper comprises the following steps: Preparation of the detection layer: 1.5 g / kg TMB, 3 g / kg polyvinyl pyrrolidone (PVP-K90) and 100 mM phosphate buffer were mixed to prepare a colorimetric reagent, and the filter paper was soaked in the colorimetric reagent. After the soaking was complete, the filter paper was taken out and placed in a drying oven at 70° C. to dry to prepare the detection layer; Preparation of germ layer: melt the adhesive (EVA hot melt adhesive) and apply it on the surface of the liquid-absorbing fiber layer (water-absorbing PP polyester non-woven fabric), laminate the detection layer and the lotion fiber layer coated with the adhesive, and then press and cool them under a roller press to form the germ layer; Preparation of quick-drying residual chlorine test paper: Place the germ layer on a needle puncture lathe for needle puncture treatment, with the liquid absorbing fiber layer side of the germ layer facing up and the detection layer side facing down. The conditions for the needle puncture treatment are: the needle puncture direction is from the liquid absorbing fiber layer to the detection layer, and the needle spacing is 45 mm.
[0036] A residual chlorine detection test paper prepared by the above-mentioned quick-drying residual chlorine detection test paper preparation method comprises, from bottom to top, a liquid-absorbing fiber layer, a bonding layer and a detection layer, the residual chlorine detection paper is 5 cm long and 0.5 cm wide, the liquid-absorbing fiber layer is 0.2 mm thick, the bonding layer is 5 μm thick, and the detection layer is 0.2 mm thick.
[0037] Embodiment 10: A method for preparing a quick-drying residual chlorine detection test paper comprises the following steps: Preparation of the detection layer: 1.5 g / kg TMB, 3 g / kg polyvinyl pyrrolidone (PVP-K90) and 100 mM phosphate buffer were mixed to prepare a colorimetric reagent, and the filter paper was soaked in the colorimetric reagent. After the soaking was complete, the filter paper was taken out and placed in a drying oven at 70° C. to dry to prepare the detection layer; Preparation of germ layer: melt the adhesive (EVA hot melt adhesive) and apply it on the surface of the liquid-absorbing fiber layer (water-absorbing PP polyester non-woven fabric), laminate the detection layer and the lotion fiber layer coated with the adhesive, and then press and cool them under a roller press to form the germ layer; Preparation of quick-drying residual chlorine test paper: Place the germ layer on a needle puncture lathe for needle puncture treatment, with the liquid absorbing fiber layer side of the germ layer facing up and the detection layer side facing down. The conditions for the needle puncture treatment are: the needle puncture direction is from the liquid absorbing fiber layer to the detection layer, and the needle interval is 50 mm.
[0038] A residual chlorine detection test paper prepared by the above-mentioned quick-drying residual chlorine detection test paper preparation method comprises, from bottom to top, a liquid-absorbing fiber layer, a bonding layer and a detection layer, the residual chlorine detection paper is 5 cm long and 0.5 cm wide, the liquid-absorbing fiber layer is 0.2 mm thick, the bonding layer is 5 μm thick, and the detection layer is 0.2 mm thick.
[0039] Comparative Example 1: Compared with the embodiment, the comparative example 1 did not adopt the acupuncture treatment, and the other conditions were the same as those of the embodiment.
[0040] Comparative Example 2: Compared with the embodiment, comparative example 2 adopts glue point compounding, the glue point interval is 3mm, the bonding point area is 5mm, and the other conditions are the same as those of the embodiment.
[0041] Comparative Example 3: Compared with the embodiment, the thickness of the adhesive layer of comparative example 3 is 50 μm, and the other conditions are the same as those of the embodiment.
[0042] Comparative Example 4: Compared with the embodiment, the needle interval of comparative example 4 is 1 cm, and the other conditions are the same as those of the embodiment.
[0043] Comparative Example 5: Compared with the embodiment, the needle spacing of comparative example 5 is 0.5 mm, and the other conditions are the same as those of the embodiment.
[0044] Comparative Example 6: Comparative Example 6 is a common residual chlorine test paper.
[0045] Test example: The residual chlorine detection test papers prepared in Examples 1 to 10 and Comparative Examples 1 to 6 were tested, and the testing steps included: Prepare samples to be tested, prepare samples to be tested with residual chlorine contents of 0.3 mg / L, 1.0 mg / L, 2.0 mg / L, 4.0 mg / L and 10.0 mg / L respectively, divide the samples to be tested into five test groups, namely A (0.3 mg / L), B (1.0 mg / L), C (2.0 mg / L), D (4.0 mg / L) and E (10.0 mg / L), use glass rods to dip the above five groups of samples to be tested respectively, and then apply them on the above residual chlorine test paper for detection; Stick the residual chlorine test paper on the blank colorimetric card every 1 minute, and record the time required for the colorimetric card to be uncontaminated. The time unit is min. The color difference value △E is tested on the test paper and the standard colorimetric card of the sample to be tested. The color difference value standard (△E is 0-0.25: very small or no, an ideal match; △E is 0.25-0.5: tiny, an acceptable match; △E is 0.5-1.0: tiny to medium, acceptable in some applications; △E is 1.0-2.0: medium, acceptable in specific applications; △E is 2.0-4.0: there is a gap, acceptable in specific applications; △E>4.0: very large, unacceptable in most applications) is tested using a colorimeter DS410; The preparation method of the standard colorimetric card of the sample to be tested comprises the following steps: using the same developer as that used to prepare the test paper (mixing 1.5 g / kg of TMB, 3 g / kg of polyvinyl pyrrolidone (PVP-K90) and 100 mM of phosphate buffer to prepare a colorimetric reagent), mixing the colorimetric reagent with the sample to be tested and fully coloring the mixture, soaking the test paper in the color-developed sample to be tested, taking it out and drying it after fully soaking it, and placing the dried standard colorimetric test paper on a blank colorimetric card to prepare a standard colorimetric card; The test results are shown in Table 1; Table 1 Test results As shown in Table 1, Examples 1 to 10 are chlorine residual test papers prepared by the preparation method of the quick-drying chlorine residual test paper provided by the present application. The quick-drying time of the chlorine residual test paper of Examples 1 to 10 is 2 to 3 minutes, and the color difference values of Group A, Group B, Group C, Group D and Group E at different concentrations with the standard colorimetric card are all in the range of 0 to 0.25, and there is no color difference discernible by the naked eye; the above results show that the quick-drying chlorine residual test paper provided by the present application has a quick-drying function, which can ensure that the liquid to be tested fully reacts with the test paper when the test paper is used and quickly absorbs the liquid in the test paper layer, so that the test paper can not contaminate the colorimetric card during rapid detection.
[0046] In comparative example 1, no acupuncture treatment was performed, and comparative example 1 required more than 60 minutes to dry. Since no acupuncture treatment was performed, the liquid-absorbing fiber layer and the test paper layer were blocked by the adhesive layer, and the liquid-absorbing fiber layer could not exert its liquid-absorbing capacity. Therefore, the test paper layer could only lose water through natural evaporation for a long time.
[0047] In Comparative Example 2, a glue-dotting compounding method is adopted. After the glue-dotting compounding, the adhesive layer is compounded with the liquid-absorbing fiber layer and the test paper layer in the form of connecting points. The liquid-absorbing fiber layer and the test paper layer are in contact through the gaps between adjacent connecting points. However, since the gaps between adjacent connecting points are large, the liquid-absorbing fiber layer quickly absorbs the liquid to be tested in the test paper layer, resulting in the liquid to be tested and the color developing test paper being absorbed by the liquid-absorbing fiber layer before they are fully colored. When the concentration is low, the color development speed is fast and the difference is small. When the concentration is high, the color development speed is slow, and the color difference is greater, and there will be visible color difference, which will lead to inaccurate test results in actual use.
[0048] When the bonding layer in Comparative Example 3 is too thick, it will also affect the liquid absorption speed. When the bonding layer is too thick, since the bonding layer uses hot-melt adhesive resin, the elasticity of the hot-melt adhesive resin itself will cause the fiber absorption rate to be significantly reduced, so that the absorption time is increased to more than 15 minutes, which significantly increases the absorption rate of the liquid-absorbing fiber layer. In addition, if a bonding layer with a higher structural strength is used, it will make it impossible to perform needle punching treatment.
[0049] Comparative Examples 4 and 5 respectively investigated the needle spacing of the needle punching treatment. The results showed that if the needle spacing is too small, it will lead to an increase in the fiber entanglement points and a too fast liquid absorption speed. If the needle spacing is too large, it will lead to insufficient fiber entanglement points and a slow liquid absorption speed. In addition, if the needle spacing is too small, the bonding layer will be cut off, causing the membrane structure of the bonding layer to be destroyed.
[0050] Comparative Example 6 is a common residual chlorine detection test paper, and the drying time of Comparative Example 6 is significantly shorter than the quick-drying residual chlorine detection test paper provided in the present application.
[0051] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing a quick-drying residual chlorine test paper, characterized in that: The method comprises the following preparation steps: soaking a test paper substrate with a color developing reagent and then drying it to form a detection layer; coating a binder on the surface of a liquid absorbing fiber layer and then cooling it together with the detection layer to form a germ layer; and performing a needle-puncture treatment from the liquid absorbing fiber layer to the detection layer to form a quick-drying residual chlorine detection test paper.
2. The method for preparing quick-drying residual chlorine test paper according to claim 1, wherein The raw material of the liquid-absorbing fiber layer is one or more of polypropylene fiber and polyacrylonitrile fiber.
3. The preparation method of quick-drying residual chlorine detection test paper according to claim 1, characterized in that, The test paper substrate is one of filter paper and chromatography test paper.
4. The preparation method of quick-drying residual chlorine detection test paper according to claim 1, characterized in that, The coating thickness of the adhesive is 2-5 μm.
5. The preparation method of quick-drying residual chlorine detection test paper according to claim 4, characterized in that, The conditions of the acupuncture treatment are: the needle spacing is 5-50 mm.
6. The method for preparing a quick-drying residual chlorine test paper according to claim 4, wherein: The color developing reagent is TMB, a dispersant and a buffer.
7. The method for preparing the quick-drying residual chlorine test paper according to claim 6, wherein: The pH value of the buffer solution is 6.2-7.
0.
8. The preparation method of the quick-drying residual chlorine detection test paper according to claim 6 or 7, characterized in that, The buffer is phosphate buffer.
9. The method for preparing the quick-drying residual chlorine test paper according to claim 6, wherein: The dispersant is polyvinyl pyrrolidone.
10. A quick-drying residual chlorine test paper, characterized in that: The residual chlorine detection test paper is made by the preparation method of the quick-drying residual chlorine detection test paper according to any one of claims 1 to 9, wherein the residual chlorine detection test paper comprises, from bottom to top, a liquid-absorbing fiber layer, a bonding layer and a detection layer, and the fibers of the liquid-absorbing fiber layer are entangled with the fibers of the detection layer.