Pattern forming method
A three-layer resist process with a specific resist underlayer film composition addresses the challenges of forming thick films with uniformity and adhesion in 3D-NAND flash memories, achieving high-precision patterns and improved manufacturing efficiency.
Patent Information
- Application Number
- CN202410713093.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-11-09
- Filing Date
- 2024-06-04
- Publication Date
- 2024-12-06
AI Technical Summary
Existing pattern forming methods for 3D-NAND flash memories face challenges in forming thick resist films with uniformity and adhesion, leading to issues like film roughness and peeling, which are exacerbated by the increasing number of vertical layers, making it difficult to achieve high precision and cost-effective manufacturing.
A pattern forming method using a resist underlayer film forming composition comprising a specific resin and organic solvent, applied in a three-layer resist process, which includes forming a resist underlayer film, a silicon-containing intermediate film, and a resist upper layer film, followed by sequential dry etching to transfer patterns to these films and the substrate, ensuring excellent dry etching resistance, adhesion, and film forming properties.
The method enables the formation of high-precision step-shaped patterns with improved film uniformity and adhesion, suitable for complex structures like 3D-NAND flash memories, even with high aspect ratios, by using a resist underlayer film with adjusted phenolic hydroxyl group ratios and additives for enhanced properties.
Smart Images

Figure CN119087742A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a pattern forming method. Background Art
[0002] The integrated circuit (IC) industry has achieved a reduction in bit cost by moving to smaller shapes. However, as the limit size is further miniaturized, the current photolithography technology cannot achieve the same low manufacturing cost. NAND flash memory manufacturers are exploring the technology of overlapping multiple layers of memory cells to achieve greater storage capacity and reduce the manufacturing cost per bit. By reducing manufacturing costs and miniaturizing important features, a stacked 3D structure for NAND use has been developed. Such 3D-NAND devices have high density, high speed and low cost compared to known 2D planar NAND devices.
[0003] In the manufacture of three-dimensional stacked semiconductor memories such as 3D-NAND flash memories, there is a step of etching a multilayer film into a staircase shape using plasma. In the step of etching the multilayer film into a staircase shape, etching of the multilayer film with a mask formed on the surface and trimming of the mask on the multilayer film are alternately performed. This mask uses a thick KrF photoresist that can be trimmed and etched multiple times (Patent Document 1).
[0004] On the other hand, the 3D-NAND design increases from 64 vertical layers to more than 128 layers, requiring thicker resists. In order to use thick resist films in KrF lithography that can resolve patterns at the micron level, inherent technical issues will be associated with it. In order to pattern the thick resist film, sufficient film transmittance is required at the exposure wavelength (248nm) so that the incident radiation can reach the bottom of the film. In addition, the thick resist film used in 3D-NAND applications will undergo a series of vertical and horizontal "pullback" etching steps at each stage.
[0005] Patent Document 2 reports a KrF resist with a thickness of 15 μm, but if a thick resist film is subjected to etching, the uniformity of the film structure may be affected, and the roughness of the step-shaped cross-section may increase. An ideal mask should be able to maintain the physical structure of the film after each etching process, and when more layers are expected, etching using only known resist films is approaching its applicability limit.
[0006] One method to solve such a problem is the multilayer resist method. This method is to insert a resist lower film having a different etching selectivity from the photoresist film (i.e., the resist upper film) between the resist upper film and the substrate to be processed, and after the resist upper film has a pattern, the resist upper film pattern is used as a dry etching mask to transfer the pattern to the resist lower film by dry etching, and then the resist lower film is used as a dry etching mask to transfer the pattern to the substrate to be processed by dry etching.
[0007] One of the multilayer resist methods is a three-layer resist method that can be implemented using a general resist composition used in the single-layer resist method. In this three-layer resist method, for example, an organic film obtained from a novolac resin or the like is formed on a substrate to be processed as a resist lower film, a silicon-containing resist intermediate film is formed thereon as a resist intermediate film, and a normal organic photoresist film is formed thereon as a resist upper film. When dry etching is performed using fluorine-based gas plasma, the organic resist upper film can achieve a good etching selectivity ratio with respect to the silicon-containing resist intermediate film, so that the resist upper film pattern can be transferred to the silicon-containing resist intermediate film by dry etching using fluorine-based gas plasma. According to this method, even when using a resist composition that is difficult to form a pattern with a sufficient film thickness for directly processing a substrate or a resist composition that does not have sufficient dry etching resistance for substrate processing, the pattern can be transferred to a silicon-containing resist intermediate film (resist intermediate film). If the pattern transfer is subsequently performed by dry etching using oxygen or hydrogen gas plasma, a pattern of an organic film (resist lower film) made of a phenolic varnish resin or the like that has sufficient dry etching resistance for substrate processing can be obtained.
[0008] As for the problems when the step-shaped pattern is formed using the above-mentioned three-layer resist method, the film-forming property and dry etching resistance when the resist lower film is formed into a thick film can be cited. The resist lower film forming composition uses a polymer with a rigid aromatic ring structure, so it shows excellent dry etching resistance (patent document 3). However, due to the rigid structure, poor film formation such as cracking is prone to occur when the thick film is formed. In addition, the complex viscosity of the resin with phenolic hydroxyl groups increases, so the fluidity of the resist lower layer forming composition decreases, and it is considered difficult to form a thick film with one coating. On the other hand, it has been reported that the use of a resin modified with phenolic hydroxyl groups in the resist lower film will show excellent fluidity (patent document 4). However, when such a phenolic hydroxyl-modified resin is used to form a thick film in the resist lower film, there is a concern that it will peel off from the substrate due to insufficient adhesion to the substrate.
[0009] Prior art literature
[0010] Patent Literature
[0011] [Patent Document 1] Japanese Patent Application Publication No. 2020-187352
[0012] [Patent Document 2] Japanese Patent Application Publication No. 2021-063217
[0013] [Patent Document 3] Japanese Patent Application Publication No. 2005-128509
[0014] [Patent Document 4] Japanese Patent Application Publication No. 2017-119671 Summary of the invention
[0015] [Problems to be solved by the invention]
[0016] In view of the above situation, an object of the present invention is to provide a pattern forming method capable of forming a step-shaped pattern with high precision by using a resist underlayer film forming composition having excellent dry etching resistance and excellent film forming properties and substrate adhesion compared to the known KrF resist.
[0017] [Methods for solving problems]
[0018] In order to solve the above problems, the present invention provides a pattern forming method, which is a method for forming a pattern on a processed substrate, characterized by:
[0019] The following steps are involved:
[0020] (I-1) after applying a resist underlayer film forming composition on a substrate to be processed, forming a resist underlayer film by heat treatment,
[0021] (I-2) forming a silicon-containing resist intermediate film on the resist underlayer film,
[0022] (I-3) forming a resist upper layer film on the aforementioned silicon-containing resist intermediate film using a photoresist material,
[0023] (I-4) after pattern exposure of the resist upper layer film, developing with a developer to form a pattern on the resist upper layer film,
[0024] (I-5) using the patterned resist upper layer film as a mask, dry etching is performed to transfer a pattern to the silicon-containing resist intermediate film,
[0025] (I-6) using the silicon-containing resist intermediate film to which the pattern has been transferred as a mask, dry etching is performed to transfer the pattern to the resist lower layer film,
[0026] (I-7) using the resist underlayer film to which the pattern has been transferred as a mask, processing the substrate to be processed to form a pattern on the substrate to be processed,
[0027] (I-8) trimming the resist underlayer film to which the pattern has been transferred,
[0028] (I-9) using the trimmed resist underlayer film pattern as a mask, processing the substrate to be processed to form a step-shaped pattern on the substrate to be processed,
[0029] The resist underlayer film-forming composition comprises (A) a resin and (B) an organic solvent.
[0030] The resin (A) is a resin having a structural unit represented by the following general formula (1), and when the ratio of the phenolic hydroxyl groups contained in the resin (A) is a and the ratio of the groups modified by the phenolic hydroxyl groups is b, the following relations are satisfied: a+b=1, 0.1≤a≤0.5, 0.5≤b≤0.9:
[0031] [Chemistry 1]
[0032]
[0033] In the general formula (1), R 01 is a saturated or unsaturated monovalent organic group having 1 to 30 carbon atoms which may be substituted, R 02 is a hydrogen atom or a saturated or unsaturated monovalent organic group having 1 to 30 carbon atoms which may be substituted. X is a divalent organic group having 1 to 30 carbon atoms, and p is 0 or 1. When p is 0, m2 is an integer of 0 to 3, n2 is an integer of 1 to 4, and m2+n2 is an integer of 1 to 4. When p is 1, m2 is an integer of 0 to 5, n2 is an integer of 1 to 6, and m2+n2 is an integer of 1 to 6.
[0034] Such a pattern forming method can have excellent fluidity and substrate adhesion, and by adjusting the ratio of the structure within the above range, a thick resist underlayer film with good film forming properties can be formed. Moreover, even if the processed substrate has a height difference, the height difference of the processed substrate can be filled without pores, and a flat film can be formed. Furthermore, a resist underlayer film with excellent dry etching resistance compared to the known KrF resist can be formed with a thick film, and a resist pattern can be transferred to the processed substrate with high precision.
[0035] Furthermore, in the present invention, it is preferred that the steps (I-8) to (I-9) are repeated to form a plurality of step-shaped patterns on the substrate to be processed.
[0036] According to such a pattern forming method, a step-shaped pattern can be transferred to a substrate to be processed with high accuracy.
[0037] Furthermore, in the present invention, it is preferred that the substrate to be processed use a multilayer film in which polysilicon layers are stacked, or a multilayer film in which SiN layers and SiO layers are alternately stacked.
[0038] Such a pattern forming method is suitable for manufacturing three-dimensional stacked semiconductor memories such as 3D-NAND flash memories.
[0039] In the present invention, it is preferred that the substrate to be processed use a multilayer film in which polysilicon layers and SiO layers are alternately stacked, or a multilayer film in which SiN layers and SiO layers are alternately stacked.
[0040] Such a pattern forming method is suitable for manufacturing three-dimensional stacked semiconductor memories such as 3D-NAND flash memories.
[0041] Furthermore, in the present invention, the resist underlayer film is preferably formed to have a thickness of at least 3 μm.
[0042] According to such a pattern forming method, a plurality of step-shaped patterns can be transferred to a substrate to be processed with high accuracy.
[0043] At this time, in the step (I-1), it is preferred that the resist underlayer film be applied to a thickness of at least 3 μm by a single coating.
[0044] Such a pattern forming method is preferable because it is possible to transfer a plurality of step-shaped patterns to a substrate to be processed with high accuracy by applying the resist underlayer film forming composition once.
[0045] In the present invention, the resin (A) preferably has a weight average molecular weight of 3,000 to 20,000.
[0046] By containing such a (A) resin, a thick resist underlayer film having excellent film-forming properties and film thickness uniformity can be formed.
[0047] Furthermore, in the present invention, the resist underlayer film forming composition preferably contains (C) a base generator.
[0048] According to such a pattern forming method, a thick resist underlayer film having excellent substrate adhesion can be formed.
[0049] In this case, the base generator (C) is preferably any of those represented by the following general formulas (2), (3) and (4).
[0050] [Chemistry 2]
[0051]
[0052] In the formula, R 1 ~R 3Each independently represents a linear, branched or cyclic alkyl group having 1 to 10 carbon atoms or an alkenyl group having 2 to 10 carbon atoms, which may be substituted by a heteroatom or have an intervening heteroatom, or an aryl group having 6 to 18 carbon atoms or an aralkyl group having 7 to 18 carbon atoms, which may be substituted by a heteroatom or have an intervening heteroatom. 1 , R 2 and R 3 Any two of X may also be bonded to each other and form a ring together with the sulfur atom in the formula. - represents an organic or inorganic anion that is a counter ion. - OH not included - . R 4 and R 5 Each independently represents an aryl group having 6 to 20 carbon atoms which may be substituted with or interposed with a hetero atom, and a part or all of the hydrogen atoms thereof may be substituted with a linear, branched or cyclic alkyl or alkoxy group having 1 to 10 carbon atoms. 4 and R 5 They may also bond to each other and to form a ring together with the iodine atom in the formula. 6 , R 7 , R 8 and R 9 Each independently represents a hydrogen atom, or a linear, branched, or cyclic alkyl group having 1 to 20 carbon atoms or an alkenyl group having 2 to 20 carbon atoms, which may be substituted by a heteroatom or have an intervening heteroatom, or an aryl group having 6 to 18 carbon atoms or an aralkyl group having 7 to 18 carbon atoms, which may be substituted by a heteroatom or have an intervening heteroatom. 6 , R 7 , R 8 and R 9 Any two or more of the may be bonded to each other and form a ring together with the nitrogen atom in the formula.
[0053] According to the pattern forming method using the resist underlayer film forming composition containing such a (C) base generator, a resist underlayer film having a thick film and excellent substrate adhesion can be formed.
[0054] In this case, X in the above general formulas (2), (3) and (4) - It is preferred to use any anion selected from the group consisting of a structure represented by any one of the following general formulae (5), (6) and (7), and chloride ion, bromide ion, iodide ion, fluoride ion, cyanide ion, nitrate ion and nitrite ion.
[0055] [Chemistry 3]
[0056]
[0057] In the formula, R 10It represents a linear, branched, or cyclic alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms, which may contain one or more selected from an ether group, an ester group, and a carbonyl group, and some or all of the hydrogen atoms in these groups may be substituted with one or more selected from a halogen atom, a hydroxyl group, a carboxyl group, an amino group, and a cyano group. 11 R represents an aryl group having 6 to 20 carbon atoms, wherein a part or all of the hydrogen atoms of the aryl group may be substituted with one or more selected from a halogen atom, a hydroxyl group, a carboxyl group, an amino group, and a cyano group. 12 , R 13 , and R 14 Each independently represents a hydrogen atom, a halogen atom other than a fluorine atom, or a linear, branched, or cyclic alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms, which may contain one or more selected from an ether group, an ester group, and a carbonyl group, and a part or all of the hydrogen atoms in these groups may be substituted by one or more selected from a halogen atom, a hydroxyl group, a carboxyl group, an amino group, and a cyano group. 12 , R 13 , and R 14 Two or more of them may be bonded to each other to form a ring.
[0058] According to the pattern forming method using the resist underlayer film forming composition containing such a base generator (C), a resist underlayer film having a thick film and excellent substrate adhesion can be formed.
[0059] In the present invention, in the general formula (1), the R 02 It is preferably a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, or a structure represented by the following general formula (8).
[0060] [Chemistry 4]
[0061]
[0062] In the general formula (8), * represents the bonding site to the oxygen atom, R A is a divalent organic group having 1 to 10 carbon atoms which may be substituted, R B It is a hydrogen atom or an optionally substituted monovalent organic group having 1 to 10 carbon atoms.
[0063] According to the pattern forming method using the resin (A) having such a structure, excellent fluidity can be imparted to the resist underlayer film-forming composition, so that a thick resist underlayer film having good film-forming properties can be formed.
[0064] In the present invention, it is preferred that the resist underlayer film forming composition further contains one or more selected from (D) a crosslinking agent, (E) a fluidity promoter, and (F) a surfactant.
[0065] By using the resist underlayer film forming composition containing the above additives, various properties required for forming a resist underlayer film, such as film forming properties, filling characteristics, dry etching resistance, and substrate adhesion, can be adjusted within appropriate ranges.
[0066] In the present invention, the method of forming a circuit pattern on the resist upper layer film preferably uses optical lithography with a wavelength of 5 nm to 300 nm, direct drawing using an electron beam, nanoimprinting, or a combination thereof.
[0067] According to such a pattern forming method, a pattern with small edge roughness can be formed.
[0068] In the present invention, the developing method is preferably alkali developing or organic solvent developing.
[0069] According to such a pattern forming method, a pattern with small edge roughness and little residue in the resist dissolving portion can be formed.
[0070] Furthermore, in the present invention, the substrate to be processed is preferably a structure having an aspect ratio of 5 or more or a substrate having a height difference.
[0071] The pattern forming method of the present invention is particularly useful for microfabrication of substrates having such structures or height differences, since it uses a resist underlayer film forming composition having a high degree of embedding properties, and is suitable for forming a complex step-shaped pattern.
[0072] [Effects of the Invention]
[0073] As described above, the pattern forming method of the present invention is extremely useful for fine patterning for semiconductor device manufacturing because it uses a resist underlayer film forming composition that has excellent dry etching resistance and excellent film forming properties and substrate adhesion compared to the known KrF resist. In particular, in the fine patterning process using the multilayer resist method in the semiconductor device manufacturing step, on a processed substrate with a large aspect ratio, such as a 3D-NAND memory with high lamination progress, and especially having a difficult-to-fill portion, a resist underlayer film can be formed with excellent filling properties without causing defects such as voids and peeling, and further, a pattern forming method using a resist underlayer film forming composition having appropriate planarization properties, etching properties, and optical properties can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0074] Figure 1 (A) to (L) are explanatory diagrams of an example (three-layer resist process) of the pattern forming method of the present invention.
[0075] Figure 2 (M) to (O) are explanatory diagrams of the landfill characteristic evaluation method. DETAILED DESCRIPTION
[0076] As described above, a pattern forming method capable of forming a staircase-shaped pattern with high precision is required in the step of etching a multilayer film represented by a 3D-NAND memory in which high lamination is progressing into a staircase shape.
[0077] The inventor of the present application speculated that by using a multilayer resist method using a resist underlayer film, a step-shaped pattern can be formed on a processed substrate with high precision. On the other hand, in order to take into account the film forming property and dry etching resistance that are issues in forming a thick film of the resist underlayer film, a pattern forming method using various resist underlayer film forming compositions was explored. As a result, it was found that a pattern forming method using a resist underlayer film material containing a resin having a specific structure is very effective, and the present invention was completed.
[0078] That is, the present invention provides a pattern forming method, which is a method for forming a pattern on a processed substrate, characterized by:
[0079] The following steps are involved:
[0080] (I-1) after applying a resist underlayer film forming composition on a substrate to be processed, forming a resist underlayer film by heat treatment,
[0081] (I-2) forming a silicon-containing resist intermediate film on the resist underlayer film,
[0082] (I-3) forming a resist upper layer film on the aforementioned silicon-containing resist intermediate film using a photoresist material,
[0083] (I-4) after pattern exposure of the resist upper layer film, developing with a developer to form a pattern on the resist upper layer film,
[0084] (I-5) using the patterned resist upper layer film as a mask, dry etching is performed to transfer a pattern to the silicon-containing resist intermediate film,
[0085] (I-6) using the silicon-containing resist intermediate film to which the pattern has been transferred as a mask, dry etching is performed to transfer the pattern to the resist lower layer film,
[0086] (I-7) using the resist underlayer film to which the pattern has been transferred as a mask, processing the substrate to be processed to form a pattern on the substrate to be processed,
[0087] (I-8) trimming the resist underlayer film to which the pattern has been transferred,
[0088] (I-9) using the trimmed resist underlayer film pattern as a mask, processing the substrate to be processed to form a step-shaped pattern on the substrate to be processed,
[0089] The resist underlayer film-forming composition comprises (A) a resin and (B) an organic solvent.
[0090] As for the aforementioned (A) resin, a constituent unit represented by the following general formula (1) is used, and when the proportion of phenolic hydroxyl groups contained in the aforementioned (A) resin is a and the proportion of groups modified by phenolic hydroxyl groups is b, it satisfies the relationship of a+b=1, 0.1≤a≤0.5, and 0.5≤b≤0.9.
[0091] [Chemistry 5]
[0092]
[0093] In the general formula (1), R 01 is a saturated or unsaturated monovalent organic group having 1 to 30 carbon atoms which may be substituted, R 02 is a hydrogen atom or a saturated or unsaturated monovalent organic group having 1 to 30 carbon atoms which may be substituted. X is a divalent organic group having 1 to 30 carbon atoms, and p is 0 or 1. When p is 0, m2 is an integer of 0 to 3, n2 is an integer of 1 to 4, and m2+n2 is an integer of 1 to 4. When p is 1, m2 is an integer of 0 to 5, n2 is an integer of 1 to 6, and m2+n2 is an integer of 1 to 6.
[0094] The present invention is described in detail below, but the present invention is not limited thereto.
[0095] <Pattern Formation Method>
[0096] The present invention provides a pattern forming method, which is a method for forming a pattern on a processed substrate.
[0097] Its characteristics are:
[0098] The following steps are involved:
[0099] (I-1) after applying a resist underlayer film forming composition on a substrate to be processed, forming a resist underlayer film by heat treatment,
[0100] (I-2) forming a silicon-containing resist intermediate film on the resist underlayer film,
[0101] (I-3) forming a resist upper layer film on the aforementioned silicon-containing resist intermediate film using a photoresist material,
[0102] (I-4) after pattern exposure of the resist upper layer film, developing with a developer to form a pattern on the resist upper layer film,
[0103] (I-5) using the patterned resist upper layer film as a mask, dry etching is performed to transfer a pattern to the silicon-containing resist intermediate film,
[0104] (I-6) using the silicon-containing resist intermediate film to which the pattern has been transferred as a mask, dry etching is performed to transfer the pattern to the resist lower layer film,
[0105] (I-7) using the resist underlayer film to which the pattern has been transferred as a mask, processing the substrate to be processed to form a pattern on the substrate to be processed,
[0106] (I-8) trimming the resist underlayer film to which the pattern has been transferred,
[0107] (I-9) using the trimmed resist underlayer film pattern as a mask, processing the substrate to be processed to form a step-shaped pattern on the substrate to be processed,
[0108] The resist underlayer film-forming composition comprises (A) a resin and (B) an organic solvent.
[0109] As for the aforementioned (A) resin, a constituent unit represented by the following general formula (1) is used, and when the proportion of phenolic hydroxyl groups contained in the aforementioned (A) resin is a and the proportion of groups modified by phenolic hydroxyl groups is b, it satisfies the relationship of a+b=1, 0.1≤a≤0.5, and 0.5≤b≤0.9.
[0110] [Chemistry 6]
[0111]
[0112] In the general formula (1), R 01 is a saturated or unsaturated monovalent organic group having 1 to 30 carbon atoms which may be substituted, R 02 is a hydrogen atom or a saturated or unsaturated monovalent organic group having 1 to 30 carbon atoms which may be substituted. X is a divalent organic group having 1 to 30 carbon atoms, and p is 0 or 1. When p is 0, m2 is an integer of 0 to 3, n2 is an integer of 1 to 4, and m2+n2 is an integer of 1 to 4. When p is 1, m2 is an integer of 0 to 5, n2 is an integer of 1 to 6, and m2+n2 is an integer of 1 to 6.
[0113] use Figure 1 The present invention provides the following pattern forming method using a three-layer resist process. Figure 1(A) is to form a resist underlayer film 3 on a workpiece layer 2 on a workpiece substrate 1 using the resist underlayer film forming composition. For example, silicon nitride can be used for the workpiece substrate 1, and for example, silicon oxide can be used for the workpiece layer 2. Then, as Figure 1 (B), a silicon-containing resist intermediate film 4 is formed on the resist lower layer film 3 using a silicon-containing resist intermediate film material. Then, as Figure 1 (C), a photoresist material is used to form a resist upper film 5 on the aforementioned silicon-containing resist intermediate film 4. Then, as Figure 1 (D), after the exposure portion 6 of the resist upper film is subjected to pattern exposure, as Figure 1 (E), developing with a developer to form a resist upper film pattern 5a on the resist upper film, and Figure 1 (F), the patterned resist upper film is used as a mask to dry-etch the silicon-containing resist intermediate film to transfer the silicon-containing resist intermediate film pattern 4a, such as Figure 1 (G), using the silicon-containing resist intermediate film having the transferred pattern as a mask, dry etching is performed on the resist lower film to transfer the resist lower film pattern 3a, such as Figure 1 (H), using the above-mentioned patterned resist lower layer film as a mask, the processed layer on the above-mentioned processed substrate 1 is processed to form a pattern 2a in the above-mentioned processed layer, such as Figure 1 (I), the processed layer having the pattern 2a formed thereon is used as a mask to process the processed substrate to form the pattern 1a. Then, as Figure 1 (J), the aforementioned resist lower film pattern is trimmed to form a trimmed resist lower film pattern 3b, such as Figure 1 (K), the trimmed resist lower film pattern 3b is used as a mask to process the pattern formed in the aforementioned processed layer to form a pattern 2b, such as Figure 1 (L), the processed layer on which the pattern 2b is formed is used as a mask, and the processed substrate on which the pattern is formed is processed to form the pattern 1b. By such a pattern forming method, Figure 1 (L) can form a step-like pattern on the processed substrate.
[0114] Furthermore, it is preferred that the above steps (I-8) to (I-9) are repeated to form a plurality of step-shaped patterns on the above-mentioned processed substrate.
[0115] The processed substrate preferably has a structure with a multilayer stack of a polysilicon layer and a silicon oxide (SiO) layer, a silicon oxide (SiO) layer and a silicon nitride (SiN) layer, or a polysilicon layer, and more preferably has a multilayer stack of a silicon oxide (SiO) layer and a silicon nitride (SiN) layer. That is, the processed substrate preferably uses a multilayer film stacked with a polysilicon layer, or a multilayer film alternately stacked with SiN layers and SiO layers, and the processed substrate preferably uses a multilayer film alternately stacked with a polysilicon layer and a SiO layer, or a multilayer film alternately stacked with SiN layers and SiO layers. The SiO layer and the SiN layer can be formed using various techniques known in the technical field, such as chemical vapor deposition (CVD) such as plasma enhanced CVD (PECVD) or low pressure CVD (LPCVD), and atomic layer deposition (ALD).
[0116] The aforementioned processed substrate may also be a structure having an aspect ratio of 5 or more or a substrate having a height difference.
[0117] The pattern forming method of the present invention is particularly useful for microfabrication of substrates having such structures or height differences, since it uses a resist underlayer film forming composition having a high degree of embedding properties, and is suitable for forming a complex step-shaped pattern.
[0118] The resist underlayer film in the above three-layer resist treatment shows resistance to etching by fluorine-based gas. Therefore, in the above three-layer resist treatment, dry etching of the processed substrate using the resist underlayer film as a mask is preferably performed using an etching gas mainly composed of fluorine-based gas.
[0119] The above-mentioned three-layer resist underlayer film processed by the resist is preferably formed by spin-coating the above-mentioned resist underlayer film forming composition on the processed substrate, and the processed substrate coated with the above-mentioned resist underlayer film forming composition is preferably formed by heat treating the processed substrate at a temperature in the range of 100°C to 600°C for 10 to 600 seconds.
[0120] The method of spin-coating the resist underlayer film forming composition described above on the substrate to be processed, and heat-treating the substrate to be processed coated with the resist underlayer film forming composition in a gas environment with an oxygen concentration of 1% or more and 21% or less to form a resist underlayer film is preferred. Or the method of spin-coating the resist underlayer film forming composition described above on the substrate to be processed, and heat-treating the substrate to be processed coated with the resist underlayer film forming composition in a gas environment with an oxygen concentration of less than 1% is preferred.
[0121] The method for forming the resist lower film in the pattern forming method of the present invention can apply the resist lower film forming composition on the processed substrate using a spin coating method or the like. By using a spin coating method or the like, good filling characteristics can be obtained. After spin coating, in order to evaporate the solvent and prevent mixing with the resist upper film and the silicon-containing resist intermediate film, and to promote the crosslinking reaction, baking can be performed. The baking is preferably carried out at a temperature of 100°C to 600°C, more preferably in a temperature range of 100°C to 400°C, and more preferably in a temperature range of 150°C to 350°C, preferably in a range of 10 seconds to 600 seconds, and more preferably in a range of 10 to 300 seconds. By appropriately adjusting the baking temperature and time within the above range, flattening, filling characteristics, and curing characteristics suitable for the application can be obtained. When the baking temperature is above 100°C, the curing is fully carried out, and mixing with the resist upper film or the silicon-containing resist intermediate film does not occur. When the baking temperature is 600° C. or lower, thermal decomposition of the resin can be suppressed, the film thickness does not decrease, and the film surface becomes uniform.
[0122] The gas environment during baking can be either an oxygen-containing environment (oxygen concentration 1% to 21%) in air or a non-oxygen environment (nitrogen concentration 1%) in nitrogen. For example, when the substrate being processed is easily oxidized by air, heat treatment in a gas environment with an oxygen concentration of less than 1% and forming a hardened film can inhibit damage to the substrate.
[0123] The silicon-containing resist intermediate film in the above three-layer resist treatment shows resistance to etching by oxygen-based gases. Therefore, in the above three-layer resist treatment, dry etching of the resist lower film using the silicon-containing resist intermediate film as a mask is preferably performed using an etching gas mainly composed of oxygen-based gases.
[0124] For the silicon-containing resist intermediate film in the three-layer resist treatment, it is also preferable to use a polysiloxane-based intermediate film. By giving the silicon-containing resist intermediate film an antireflection effect, reflection can be suppressed. In particular, if a material containing a large amount of aromatic groups and having a high etching selectivity with the substrate is used as the resist lower film for 193nm exposure, the k value will become higher and the substrate reflection will increase, but by giving it an absorption with an appropriate k value as the silicon-containing resist intermediate film, reflection can be suppressed and the substrate reflection can be reduced to less than 0.5%. For the silicon-containing resist intermediate film with an antireflection effect, it is preferable to use anthracene as a pendant group for 248nm and 157nm exposure, and it is preferable to use a polysiloxane with a phenyl group or a light-absorbing group with a silicon-silicon bond as a pendant group and cross-linked with acid or heat for 193nm exposure.
[0125] Furthermore, in the present invention, a pattern forming method using a four-layer resist process using an organic antireflection film (BARC) or an adhesion film between the silicon-containing resist intermediate film and the resist upper film may be employed.
[0126] A pattern forming method is provided, comprising the following steps:
[0127] forming a resist underlayer film on a substrate to be processed using the resist underlayer film-forming composition;
[0128] On the resist underlayer film, a silicon-containing resist intermediate film is formed using a silicon-containing resist intermediate film material.
[0129] forming a BARC or a bonding film on the aforementioned silicon-containing resist intermediate film,
[0130] A photoresist material is used to form a resist upper film on the BARC or the adhesion film.
[0131] After the resist upper layer film is subjected to pattern exposure, it is developed with a developer to form a pattern on the resist upper layer film.
[0132] The patterned resist upper layer film is used as a mask to dry-etch the BARC or the adhesion film and the silicon-containing resist intermediate film to transfer the pattern.
[0133] The silicon-containing resist intermediate film having the transferred pattern is used as a mask to dry-etch the resist lower film to transfer the pattern.
[0134] The substrate to be processed is processed using the resist underlayer film to which the pattern has been transferred as a mask to form a pattern on the substrate to be processed.
[0135] Furthermore, an inorganic hard mask intermediate film may be formed instead of forming a silicon-containing resist intermediate film. In this case, a pattern forming method is provided, which comprises at least the following steps:
[0136] forming a resist underlayer film on a substrate to be processed using the resist underlayer film-forming composition;
[0137] An inorganic hard mask intermediate film selected from a silicon oxide film, a silicon nitride film, and a silicon oxide nitride film is formed on the resist underlayer film.
[0138] A photoresist composition is used to form a resist upper film on the inorganic hard mask intermediate film, and a circuit pattern is formed on the resist upper film.
[0139] The inorganic hard mask intermediate film is etched to form a pattern using the patterned resist upper layer film as a mask.
[0140] The above-mentioned patterned inorganic hard mask intermediate film is used as a mask to etch the above-mentioned resist underlayer film to form a pattern.
[0141] Furthermore, the substrate to be processed is etched using the patterned resist underlayer film as a mask to form a pattern on the substrate to be processed. According to such a pattern forming method, a semiconductor device circuit pattern can be formed on the substrate.
[0142] As described above, when an inorganic hard mask intermediate film is formed on the resist lower film, a silicon oxide film, a silicon nitride film, and a silicon oxide nitride film (SiON film) can be formed by a CVD method, an ALD method, or the like. For example, a method for forming a silicon nitride film is described in Japanese Patent Publication No. 2002-334869 and International Publication No. 2004 / 066377. The film thickness of the inorganic hard mask intermediate film is preferably 5 to 200 nm, and more preferably 10 to 100 nm. In addition, it is most preferable to use a SiON film that has a high effect as an anti-reflective film as the inorganic hard mask intermediate film. The substrate temperature when forming the SiON film is 300 to 500°C, so the resist lower film needs to withstand a temperature of 300 to 500°C. The resist underlayer film forming composition used in the present invention has high heat resistance and can withstand high temperatures of 300°C to 500°C, so a combination of an inorganic hard mask intermediate film formed by a CVD method or an ALD method and a resist underlayer film formed by a spin coating method may be used. Alternatively, a method of forming an inorganic hard mask intermediate film by spin coating a material containing a metal oxide may be used.
[0143] As described above, a photoresist film as a resist upper film may be formed on the inorganic hard mask intermediate film, and an organic antireflection film (BARC) or a bonding film may be formed on the inorganic hard mask intermediate film by spin coating and a photoresist film may be formed thereon. In particular, when a SiON film is used as an inorganic hard mask intermediate film, the two antireflection films of the SiON film and the BARC can suppress reflection even in immersion exposure with a high NA exceeding 1.0. Another benefit of forming a BARC is that it has the effect of reducing the tailing of the photoresist pattern directly on the SiON film.
[0144] In the above pattern forming method, the resist upper layer film may be positive or negative, and the same photoresist composition as commonly used may be used. In addition, the photoresist composition may also contain metal atoms such as Sn, In, Ga, Ge, Al, Ce, La, Cs, Zr, Hf, Ti, Bi, Sb, and Zn. When the resist upper layer film is formed using the above photoresist composition, it may be formed by a spin coating method or by a vapor deposition process such as a CVD method or an ALD method.
[0145] When the photoresist composition is formed by spin coating, the photoresist composition is pre-baked after coating, preferably at 60 to 180° C. for 10 to 300 seconds. Then, exposure is performed according to the usual method, and post-exposure baking (PEB) and development are performed to obtain a resist pattern. In addition, the thickness of the resist upper layer film is not particularly limited, but 10 to 500 nm, particularly 20 to 400 nm is preferred.
[0146] When the photoresist composition is formed by evaporation treatment using a CVD method or an ALD method, the photoresist composition is a EUV-sensitive metal oxide-containing film, and the metal is selected from Sn, Zr, Hf, Ti, Bi, Sb, etc., among which Sn with excellent EUV sensitivity is preferred. The metal oxide-containing film may also be a photosensitive organic metal oxide film such as an organic tin oxide (for example, a halogenated alkyl Sn, an alkoxyalkyl Sn, or an amide alkyl Sn). Some specific examples of suitable precursors include trimethyltin chloride, dimethyltin dichloride, methyltin trichloride, tris(dimethylamino)methyltin(IV), and (dimethylamino)trimethyltin(IV).
[0147] Films containing metal oxides can also be deposited by PECVD or PEALD using a Lam Vector (registered trademark) tool, for example. In the ALD embodiment, the Sn oxide precursor is separated from the O precursor / plasma. The evaporation temperature is preferably in the range of 50°C to 600°C. The evaporation pressure is preferably between 100 and 6,000 mTorr. The flow rate of the precursor liquid of the metal oxide-containing film (for example, organic tin oxide precursor) can be 0.01 to 10 cmm, and the gas flow rate (CO2, CO, Ar, N2) can be 100 to 10,000 sccm. The plasma power can be 200 to 1,000 W per 300 mm wafer station by using high-frequency plasma (for example, 13.56 MHz, 27.1 MHz, or higher frequencies). The evaporation thickness is preferably 100 to 2,000 angstroms.
[0148] The exposure light is high-energy radiation having a wavelength of 300 nm or less, and specifically, for example, excimer lasers of 248 nm, 193 nm, and 157 nm, soft X-rays of 3 to 20 nm, electron beams, X-rays, and the like.
[0149] The method for forming the circuit pattern on the resist upper layer film is preferably a pattern forming method using optical lithography with a wavelength of 5 nm to 300 nm, direct drawing using an electron beam, nanoimprinting, or a combination thereof.
[0150] Furthermore, the development method of the above-mentioned pattern forming method is preferably alkali development or organic solvent development.
[0151] The obtained resist pattern is then used as a mask for etching. The etching of the silicon-containing resist intermediate film and the inorganic hard mask intermediate film in the three-layer resist process is performed using a fluorine-based gas and the upper resist pattern as a mask. In this way, the silicon-containing resist intermediate film pattern and the inorganic hard mask intermediate film pattern are formed.
[0152] Next, the obtained silicon-containing resist interlayer film pattern and inorganic hard mask interlayer film pattern are used as masks to perform etching of the resist underlayer film. The etching of the resist underlayer film is preferably performed using an etching gas mainly containing oxygen-based gas.
[0153] The subsequent etching of the substrate to be processed can also be performed by conventional methods. By repeating a series of well-controlled etching of SiO and SiN and trimming of the resist underlayer film, a step-shaped pattern is formed on the substrate to be processed. Figure 1 (H) shows the structure after the initial silicon oxide etching, Figure 1 (I) shows the structure after the initial silicon nitride etching. When the first pair of silicon oxide and silicon nitride are removed by etching, as shown in FIG. Figure 1 (J), a controlled trimming step of the resist underlayer film is performed. Then, using the trimmed resist underlayer film, as Figure 1 As shown in (K) and (L), the first and second series of silicon oxides and silicon nitrides are etched. Then, the resist underlayer film is trimmed again, and the first, second and third pairs of silicon oxides / nitrides are etched. Then, the controlled trimming of the resist underlayer film is performed again. Appropriate etching of silicon oxides and silicon nitrides and trimming of the resist underlayer film and chemistry are known in the art, and dry etching is typical. When the dry etching of silicon oxide / nitride is performed mainly with fluorocarbon gas, the silicon-containing resist intermediate film pattern in the three-layer resist process is peeled off while the processed substrate is processed.
[0154] The resist underlayer film used in the pattern forming method of the present invention has excellent etching resistance during etching of the substrate to be processed, so that a step-shaped pattern can be processed on the substrate to be processed with high precision.
[0155] The number of times the resist underlayer film can be trimmed may be limited, for example, by its original thickness and etching selectivity. When the minimum thickness limit is reached, the remaining resist underlayer film is generally stripped, and a new resist underlayer film pattern is formed using a three-layer resist process. The new resist underlayer film is patterned, and the oxide layer and the nitride layer are etched, and the resist underlayer film is trimmed as described above with respect to the original resist underlayer film, and the formation of the step-shaped pattern is continued. This process can be repeated several times until the desired step pattern is formed, and is generally repeated several times until the pattern reaches the expected surface of the substrate, generally the silicon surface of the substrate.
[0156] In the pattern forming method of the present invention, a resist underlayer film having excellent dry etching resistance compared to the known KrF resist is used, so more step patterns can be formed on the substrate to be processed by forming the resist underlayer film once, which is also ideal from the viewpoint of productivity.
[0157] From the above viewpoint, the resist underlayer film is preferably formed to have a thickness of at least 3 μm, that is, the resist underlayer film is preferably at least 3 μm, more preferably at least 5 μm, more preferably at least 8 μm, and particularly preferably at least 10 μm.
[0158] By forming the resist underlayer film with such a thickness, more step-shaped patterns can be formed on the substrate to be processed, which is preferable.
[0159] Furthermore, in the step (I-1), the resist underlayer film is preferably coated with a thickness of at least 3 μm by one coating. That is, the resist underlayer film is preferably coated with a thickness of at least 3 μm by one coating, more preferably at least 5 μm, more preferably at least 8 μm, and particularly preferably at least 10 μm.
[0160] It is desirable to form a resist underlayer film having such a film thickness by a single coating process because a process with excellent productivity can be constructed.
[0161] In the process using the known KrF resist, the resist needs to be thickened to improve the dry etching resistance, but as the film thickness increases, the resolution of the resist pattern deteriorates. On the other hand, the method of the present invention using a three-layer resist process can thin the resist upper film by using a resist lower film with excellent dry etching resistance, and can resolve a good resist pattern. Not limited to KrF, by using ArF resist, a finer pattern can be formed.
[0162] <Resist Underlayer Film Forming Composition>
[0163] The composition for forming an anti-etching agent underlayer film used in the pattern forming method of the present invention contains (A) a resin and (B) an organic solvent. The aforementioned (A) resin uses a structural unit represented by the following general formula (1) and when the proportion of phenolic hydroxyl groups contained in the aforementioned (A) resin is a and the proportion of groups modified by phenolic hydroxyl groups is b, it satisfies the relationship of a+b=1, 0.1≤a≤0.5, and 0.5≤b≤0.9.
[0164] [Chemistry 7]
[0165]
[0166] In the general formula (1), R 01is a saturated or unsaturated monovalent organic group having 1 to 30 carbon atoms which may be substituted, R 02 is a hydrogen atom or a saturated or unsaturated monovalent organic group having 1 to 30 carbon atoms which may be substituted. X is a divalent organic group having 1 to 30 carbon atoms, and p is 0 or 1. When p is 0, m2 is an integer of 0 to 3, n2 is an integer of 1 to 4, and m2+n2 is an integer of 1 to 4. When p is 1, m2 is an integer of 0 to 5, n2 is an integer of 1 to 6, and m2+n2 is an integer of 1 to 6.
[0167] The resin (A) preferably has a weight average molecular weight of 3,000 to 20,000.
[0168] In the resist underlayer film forming composition, the content of the resin (A) is preferably 20% by mass or more, more preferably 25% by mass or more, and even more preferably 30% by mass or more, based on the entire composition.
[0169] The resist underlayer film-forming composition contains the (A) resin in the above ratio, so that a thick resist underlayer film can be formed by a single coating.
[0170] [(A) Resin]
[0171] The above-mentioned (A) resin has the constituent unit represented by the above-mentioned general formula (1) and when the proportion of phenolic hydroxyl groups contained in the above-mentioned (A) resin is a and the proportion of groups modified by phenolic hydroxyl groups is b, it satisfies the relationship of a+b=1, 0.1≤a≤0.5, 0.5≤b≤0.9, and it is preferred to contain any of novolac type phenol units and novolac type naphthol units.
[0172] The (A) resin containing such a structural unit is preferred because a thick resist underlayer film having excellent dry etching resistance can be formed.
[0173] When the resin (A) is a resin having a structural unit represented by the general formula (1), a resist underlayer film-forming composition having better thermal fluidity and substrate affinity can be provided, and a thick resist underlayer film having excellent etching resistance can be formed without film formation defects such as cracks.
[0174] In the above general formula (1), R 01The saturated or unsaturated monovalent organic group having 1 to 30 carbon atoms which may be substituted may be represented by: a monovalent saturated hydrocarbon group such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, isopentyl, sec-pentyl, tert-pentyl, etc.; a monovalent unsaturated chain hydrocarbon group such as vinyl, propenyl, butenyl, pentenyl, ethynyl, propynyl, etc.; a monocyclic saturated cyclic hydrocarbon group such as cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, etc.; a monovalent monocyclic unsaturated cyclic hydrocarbon group such as cyclobutenyl, cyclopentenyl, cyclohexenyl, etc.; a monovalent polycyclic cyclic hydrocarbon group such as norbornyl and adamantyl, etc.; a monovalent aromatic hydrocarbon group such as phenyl, methylphenyl, naphthyl, methylnaphthyl, anthracenyl, methylanthracenyl, etc.; and the like.
[0175] The above R 01 Other examples of the organic groups represented include alkoxy groups such as methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, isobutoxy, sec-butoxy, tert-butoxy, n-pentoxy, and n-hexoxy, and alkoxycarbonyl groups such as methoxycarbonyl, ethoxycarbonyl, n-propoxycarbonyl, isopropoxycarbonyl, n-butoxycarbonyl, isobutoxycarbonyl, sec-butoxycarbonyl, tert-butoxycarbonyl, n-pentoxycarbonyl, and n-hexoxycarbonyl.
[0176] A part or all of the hydrogen atoms possessed by the above-mentioned saturated hydrocarbon groups, unsaturated chain hydrocarbon groups, monocyclic saturated cyclic hydrocarbon groups, monocyclic unsaturated cyclic hydrocarbon groups, polycyclic cyclic hydrocarbon groups, aromatic hydrocarbon groups, alkoxy groups, alkoxycarbonyl groups, etc. may also be substituted, for example, halogen atoms such as fluorine atoms, chlorine atoms, bromine atoms, iodine atoms, hydroxyl groups, cyano groups, carboxyl groups, nitro groups, amino groups, alkoxy groups, alkoxycarbonyl groups, acyl groups, alkoxycarbonyloxy groups, aryl groups, aliphatic heterocyclic groups such as lactone groups, aromatic heterocyclic groups such as furyl groups and pyridyl groups, etc.
[0177] Considering the landfill characteristics and raw material acquisition, the above R 01 The organic group represented by is preferably methyl.
[0178] In the above general formula (1), X represents a divalent organic group having 1 to 30 carbon atoms, for example, a methylene group, an alkanediyl group such as ethanediyl, propanediyl, butanediyl, pentanediyl, hexanediyl, octanediyl, and decanediyl, a cyclopropanediyl group, a cyclobutanediyl group, a cyclopentanediyl group, a cyclohexanediyl group, a cycloheptanediyl group, a cyclooctanediyl group, a cyclodecanediyl group, a monocyclic cycloalkanediyl group such as a methylcyclohexanediyl group and an ethylcyclohexanediyl group, a bicyclo[2.2.1]heptanediyl group, a bicyclo[2.2.2]octanediyl group, a tricyclo[5.2.1.0] 2,6 ]Decanediyl (dicyclopentylidene), tricyclo[3.3.1.1 3,7 ]Decanediyl, tetracyclo[6.2.1.1 3,6 .0 2,7] polycyclic cycloalkanediyl such as dodecanediyl and adamantanediyl, and arenediyl such as phenylene and naphthylene.
[0179] Examples of the alkanediyloxy group represented by X include groups formed by combining the above alkanediyl group with an oxygen atom, etc. Examples of the cycloalkanediyloxy group represented by X include groups formed by combining the above cycloalkanediyl group with an oxygen atom, etc.
[0180] A part or all of the hydrogen atoms possessed by the above-mentioned alkanediyl, cycloalkanediyl, alkanediyloxy, cycloalkanediyloxy and arenediyl groups may be substituted. The substituents are, for example: 01 Examples of substituents which the organic groups represented may have include the same groups and the like.
[0181] Examples of the organic group represented by X include groups represented by the following formula.
[0182] [Chemistry 8]
[0183]
[0184] In the above formula, * represents an atomic bond.
[0185] In view of landfill properties and raw material availability, the organic group represented by X is preferably a methylene group.
[0186] In the above general formula (1), R 02 is a hydrogen atom or a saturated or unsaturated monovalent organic group having 1 to 30 carbon atoms which may be substituted, R 02 The preferred structure of is, for example, a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, and any of the structures represented by the following general formula (8).
[0187] [Chemistry 9]
[0188]
[0189] In the general formula (8), * represents the bonding site to the oxygen atom, R A is a divalent organic group having 1 to 10 carbon atoms which may be substituted, R B It is a hydrogen atom or an optionally substituted monovalent organic group having 1 to 10 carbon atoms.
[0190] In the above general formula (8), R A Examples of the divalent organic group having 1 to 10 carbon atoms include methylene, ethanediyl, propanediyl, butanediyl, pentanediyl, hexanediyl, octanediyl, decanediyl and other alkanediyl groups, benzenediyl, methylbenzenediyl, naphthalenediyl and other aromatic diyl groups.
[0191] In the above general formula (8), R BThe monovalent organic group having 1 to 10 carbon atoms represented by is exemplified by alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, n-hexyl, n-octyl, and n-decyl, and aryl groups such as phenyl, tolyl, xylyl, mesityl, and naphthyl.
[0192] Some or all of the hydrogen atoms possessed by the above-mentioned alkanediyl, arenediyl, alkyl, aryl, etc. may be substituted, and the substituents, for example, are: 01 Examples of substituents which the organic groups represented may have include the same groups and the like.
[0193] Particularly preferred examples include the following structures. With such a structure, fluidity becomes good, and the embedding characteristics and planarization characteristics are improved. In addition, heat resistance and film forming properties become good, and the generation of sublimates during heat curing can be suppressed, the contamination of the device caused by the sublimates can be suppressed, and the generation of coating defects can be suppressed.
[0194] [Chemistry 10]
[0195]
[0196] In the above formula, * represents a bonding site to an oxygen atom.
[0197] In the resin having the structural unit represented by the general formula (1), the structure represented by the ratio b can be specifically exemplified as follows, but is not limited to these.
[0198] [Chemistry 11]
[0199]
[0200] Furthermore, in the above-mentioned (A) resin, when the ratio of phenolic hydroxyl groups is a and the ratio of groups modified by phenolic hydroxyl groups is b, a and b satisfy the relationship of a+b=1, 0.1≤a≤0.5, and 0.5≤b≤0.9. The relationship between a and b is preferably a+b=1, 0.15≤a≤0.4, and 0.6≤b≤0.85. When the ratio of b is less than 0.5, the contribution of hydrogen bonds of phenolic hydroxyl groups increases, and the complex viscosity of the resin increases, so that the fluidity is lowered, and there is a concern that the filling characteristics are deteriorated. When the ratio of b exceeds 0.9, the ratio of phenolic hydroxyl groups in the resin decreases, and there is a concern that the substrate adhesion with the substrate to be processed is deteriorated.
[0201] In the above general formula (1), p is 0 or 1. When p is 0, m2 is an integer of 0 to 3, n2 is an integer of 1 to 4, and m2+n2 is an integer of 1 to 4. When p is 1, m2 is an integer of 0 to 5, n2 is an integer of 1 to 6, and m2+n2 is an integer of 1 to 6.
[0202] The weight average molecular weight of the resin (A) used in the resist underlayer film forming composition is preferably 3,000 to 20,000. The weight average molecular weight is a value measured by gel permeation chromatography (tetrahydrofuran solvent, polystyrene standard). The weight average molecular weight of the resin (A) is preferably 3,000 to 20,000, more preferably 3,500 to 15,000, and even more preferably 4,000 to 10,000. If the weight average molecular weight is 3,000 or more, the device will not be contaminated by the increase of sublimates during film firing. On the other hand, if the weight average molecular weight is 20,000 or less, sufficient thermal fluidity is exhibited, and excellent film-forming properties and embedding properties can be imparted. In this way, by adjusting the molecular weight of the resin within an appropriate range, it is possible to achieve a balance between the film-forming properties and embedding properties caused by the deterioration of thermal fluidity accompanying the increase in the molecular weight of the resin, and the increase in sublimates and the deterioration of film thickness uniformity caused by the low molecular weight components in the resin accompanying the decrease in the molecular weight.
[0203] In addition, the ratio Mw / Mn of the weight average molecular weight Mw and the number average molecular weight Mn of the above-mentioned (A) resin obtained by gel permeation chromatography in terms of polystyrene is preferably 2.00≤Mw / Mn≤5.00, and 2.50≤Mw / Mn≤4.00 is more ideal. If Mw / Mn is 5.00 or less, there will be no contamination of the device due to the increase of sublimates during film firing. On the other hand, if Mw / Mn is 2.00 or more, it will show sufficient thermal fluidity because it contains low molecular weight components, and can provide excellent landfill properties. In this way, by adjusting the ratio Mw / Mn of the weight average molecular weight Mw and the number average molecular weight Mn of the resin within an appropriate range, it is possible to take into account the opposite properties of the film-forming properties and landfill properties caused by the deterioration of thermal fluidity due to the monodispersion of the resin, and the increase of sublimates and the deterioration of film thickness uniformity caused by the low molecular weight components in the resin due to polydispersion.
[0204] In the present invention, the resin (A) may be used alone or in combination of two or more. Alternatively, a resin not containing the structural unit represented by the general formula (1) may be used in combination. The resin that can be mixed in this case is not particularly limited, and known resins can be used. Specifically, acrylic resins, styrene resins, phenolic resins, polyether resins, and epoxy resins are preferred. These resins are preferably mixed according to the purpose.
[0205] The pattern forming method of the present invention may further blend other compounds or polymers into the resist underlayer film forming composition according to the purpose. The blending compound or the blending polymer has the effect of improving the film-forming property of spin coating and the filling property on a substrate with a height difference by mixing with the resin having the structural unit represented by the general formula (1). In addition, the blending compound or the blending polymer is preferably a compound having a phenolic hydroxyl group.
[0206] Such materials, for example, phenol, o-cresol, m-cresol, p-cresol, 2,3-dimethylphenol, 2,5-dimethylphenol, 3,4-dimethylphenol, 3,5-dimethylphenol, 2,4-dimethylphenol, 2,6-dimethylphenol, 2,3,5-trimethylphenol, 3,4,5-trimethylphenol, 2-tert-butylphenol, 3-tert-butylphenol, 4-tert-butylphenol, 2-phenylphenol, 3-phenylphenol, 4-phenylphenol, 3,5-diphenylphenol, 2-naphthylphenol, 3-naphthylphenol, 4-naphthylphenol, 4-tritylphenol, resorcinol, 2-methylresorcinol, 4-methylresorcinol, 5-methylresorcinol, catechol, 4-tert-butylcatechol, 2 -Methoxyphenol, 3-methoxyphenol, 2-propylphenol, 3-propylphenol, 4-propylphenol, 2-isopropylphenol, 3-isopropylphenol, 4-isopropylphenol, 2-methoxy-5-methylphenol, 2-tert-butyl-5-methylphenol, gallol, thymol, isothymol, 4,4'-(9H-fluorene-9-ylidene)bisphenol, 2,2'-dimethyl-4,4'-(9H-fluorene-9-ylidene)bisphenol, 2,2'-diallyl-4,4'-(9H-fluorene-9-ylidene)bisphenol, 2,2'-difluoro-4,4'-(9H-fluorene-9-ylidene)bisphenol, 2,2'-diphenyl-4,4'-(9H-fluorene-9-ylidene)bisphenol, 2,2'-dimethoxy 4,4'-(9H-fluorene-9-ylidene)bisphenol, 2,3,2',3'-tetrahydro-(1,1')-spirobiindene-6,6'-diol, 3,3,3',3'-tetramethyl-2,3,2',3'-tetrahydro-(1,1')-spirobiindene-6,6'-diol, 3,3,3',3',4,4'-hexamethyl-2 ,3,2',3'-tetrahydro-(1,1')-spirobiindene-6,6'-diol, 2,3,2',3'-tetrahydro-(1,1')-spirobiindene-5,5'-diol, 5,5'-dimethyl-3,3,3',3'-tetramethyl-2,3,2',3'-tetrahydro-(1,1')-spirobiindene-6,6'-diol, 1- Naphthol, 2-naphthol, 2-methyl-1-naphthol, 4-methoxy-1-naphthol, 7-methoxy-2-naphthol and dihydroxynaphthalene such as 1,5-dihydroxynaphthalene, 1,7-dihydroxynaphthalene and 2,6-dihydroxynaphthalene, methyl 3-hydroxynaphthalene-2-carboxylate, indene, hydroxyindene, benzofuran, hydroxyanthracene, vinylnaphthalene, biphenyl, bisphenol, triphenol, dicyclopentadiene, tetrahydroindene, 4-vinylcyclohexene, norbornene, 5-vinylnorbornene-2-ene, α-pinene, β-pinene, limonene and other novolac resins, polyhydroxystyrene, polystyrene, polyvinylnaphthalene, polyvinylanthracene, polyvinylcarbazole, polyindene, polyvinylnaphthalene, polynorbornene, polycyclodecene, polytetracyclododecene, polytricyclo[2.2.1.0(2,6)]heptane (poly-nortricyclene), poly(meth)acrylate and copolymers thereof. In addition, naphthol dicyclopentadiene copolymers described in Japanese Patent Application Laid-Open No. 2004-205685, fluorene bisphenol novolac resins described in Japanese Patent Application Laid-Open No. 2005-128509, ethylene naphthalene copolymers described in Japanese Patent Application Laid-Open No. 2005-250434, fullerenes having phenol groups described in Japanese Patent Application Laid-Open No. 2006-227391, bisphenol compounds and novolac resins thereof described in Japanese Patent Application Laid-Open No. 2006-293298, adamantane phenol compounds and novolac resins thereof described in Japanese Patent Application Laid-Open No. 2006-285095, bisnaphthol compounds and novolac resins thereof described in Japanese Patent Application Laid-Open No. 2010-122656, fullerene resin compounds described in Japanese Patent Application Laid-Open No. 2008-158002, etc. may also be blended.
[0207] [(B) Organic solvent]
[0208] The (B) organic solvent that can be used in the resist underlayer film forming composition used in the pattern forming method of the present invention is not particularly limited as long as it can dissolve or disperse the aforementioned resin (A), and it is preferably one that can also dissolve or disperse the later-mentioned (C) base generator, (D) cross-linking agent, (E) fluidity promoter, (F) surfactant, and (G) plasticizer.
[0209] Specifically, an organic solvent described in paragraphs
[0091] to
[0092] of Japanese Patent Application Laid-Open No. 2007-199653 may be added. More specifically, propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, 2-heptanone, cyclopentanone, cyclohexanone, and γ-butyrolactone, or a mixture containing one or more of these is preferably used.
[0210] The amount of the organic solvent (B) to be added is preferably adjusted in accordance with the set film thickness of the resist underlayer film, and is generally preferably in the range of 100 to 50,000 parts by mass relative to 100 parts by mass of the resin (A). In order to form a thick resist underlayer film, 100 to 400 parts by mass is more preferred, 100 to 300 parts by mass is more preferred, 100 to 250 parts by mass is particularly preferred, and 100 to 200 parts by mass is most preferred. By setting the amount of the organic solvent to be added to this extent, a thicker resist underlayer film can be formed, and the resist underlayer film-forming composition having excellent embedding properties and substrate adhesion is more suitable for use.
[0211] [(C) Base Generator]
[0212] The resist underlayer film forming composition used in the pattern forming method of the present invention contains (C) a base generator, so that even when a thick resist underlayer film is formed, the resist underlayer film can be formed with good adhesion to the substrate to be processed without causing problems such as substrate peeling during dry etching. In order to maximize the effect of the base generator, it is preferably not accompanied by an acid generator.
[0213] In the present invention, the base generator refers to a base generated by a change in its chemical structure due to external stimulation such as light or heat, and is also called a "potential base" or "base precursor". The generated base is not limited to general bases such as ammonia and amines, but may also be a chemical species that has the effect of increasing the ionicity of the phenolic hydroxyl group in the resin (A).
[0214] The base generator of the component (C) is not particularly limited, and a known base generator can be used. When the resist underlayer film-forming composition is used to form a film, the phenolic hydroxyl group in the resin (A) becomes ionic and the alternation with the substrate increases when heated, and it is estimated that the film-forming property is improved. Therefore, the base generator (C) is preferably a compound that exhibits alkalinity due to thermal decomposition. The reason is that the resist underlayer film-forming composition containing such a component (C) can take into account both the thermal fluidity of the film and the alternation with the substrate by adjusting the addition amount of the component (C).
[0215] As described above, when an alkali generator (also referred to as a hot alkali generator) that exhibits alkalinity due to thermal decomposition is used as component (C), the alkali generated is a cation that becomes excessive in the system due to the evaporation or decomposition of anions, specifically, triphenylsulfonium cations, tetrabutylammonium cations, etc. Because of this, the ionicity (polarity) of the phenolic hydroxyl group in the (A) resin is improved, and even if it is a substrate that has been subjected to a hydrophobic treatment such as HMDS treatment, the adhesion between the resist lower film forming composition and the substrate is improved due to the alternating action of polar groups such as silanol groups present on its surface. On the other hand, before heating, that is, before the alkali is generated, the above-mentioned action does not occur, so the fluidity of the resist lower film forming composition itself is maintained. In this way, a resist lower film with excellent film-forming properties can be formed.
[0216] Furthermore, as the base generator (C), any of those represented by the following general formulas (2), (3) and (4) is more preferably used.
[0217] [Chemistry 12]
[0218]
[0219] In the formula, R 1 ~R 3Each independently represents a linear, branched or cyclic alkyl group having 1 to 10 carbon atoms or an alkenyl group having 2 to 10 carbon atoms, which may be substituted by a heteroatom or have an intervening heteroatom, or an aryl group having 6 to 18 carbon atoms or an aralkyl group having 7 to 18 carbon atoms, which may be substituted by a heteroatom or have an intervening heteroatom. 1 , R 2 and R 3 Any two of X may also be bonded to each other and form a ring together with the sulfur atom in the formula. - represents an organic or inorganic anion that is a counter ion. - OH not included - . R 4 and R 5 Each independently represents an aryl group having 6 to 20 carbon atoms which may be substituted with or interposed with a hetero atom, and a part or all of the hydrogen atoms thereof may be substituted with a linear, branched or cyclic alkyl or alkoxy group having 1 to 10 carbon atoms. 4 and R 5 They may also bond to each other and to form a ring together with the iodine atom in the formula. 6 , R 7 , R 8 and R 9 Each independently represents a hydrogen atom, or a linear, branched, or cyclic alkyl group having 1 to 20 carbon atoms or an alkenyl group having 2 to 20 carbon atoms, which may be substituted by a heteroatom or have an intervening heteroatom, or an aryl group having 6 to 18 carbon atoms or an aralkyl group having 7 to 18 carbon atoms, which may be substituted by a heteroatom or have an intervening heteroatom. 6 , R 7 , R 8 and R 9 Any two or more of the may be bonded to each other and form a ring together with the nitrogen atom in the formula.
[0220] In the above general formula (2), R 1 , R 2 and R 3 , specifically, for example, alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, tert-butyl, cyclopropyl, cyclopentyl, cyclohexyl, cyclopropylmethyl, 4-methylcyclohexyl, cyclohexylmethyl, norbornyl, adamantyl, alkenyl groups such as vinyl, allyl, propenyl, butenyl, hexenyl, cyclohexenyl, aryl groups such as phenyl, naphthyl, thienyl, aralkyl groups such as benzyl, 1-phenylethyl, 2-phenylethyl, etc., preferably aryl groups. In addition, a part of the hydrogen atoms of these groups may be replaced by heteroatoms such as oxygen atoms, sulfur atoms, nitrogen atoms, and halogen atoms, and heteroatoms such as oxygen atoms, sulfur atoms, and nitrogen atoms may be inserted, and as a result, hydroxyl groups, cyano groups, carbonyl groups, ether bonds, ester bonds, sulfonate bonds, carbonate bonds, lactone rings, sultone rings, carboxylic anhydrides, halogenated alkyl groups, etc. may be formed or inserted.
[0221] R 1 , R 2 and R 3 When any two of them are bonded to each other directly or through an oxygen atom, a methylene group, a sulfone group or a carbonyl group, in addition to the dibenzothiophene skeleton and the phenoxathiin skeleton, the following partial structures can also be listed, but are not limited to these. In the following formula, any position on the aromatic ring can also have a substituent.
[0222] [Chemistry 13]
[0223]
[0224] More specifically, the sulfonium cations include triphenylsulfonium, 4-hydroxyphenyldiphenylsulfonium, bis(4-hydroxyphenyl)phenylsulfonium, tris(4-hydroxyphenyl)sulfonium, 4-tert-butoxyphenyldiphenylsulfonium, bis(4-tert-butoxyphenyl)phenylsulfonium, tris(4-tert-butoxyphenyl)sulfonium, 3-tert-butoxyphenyldiphenylsulfonium, bis(3-tert-butoxyphenyl)phenylsulfonium, tris(3-tert-butoxyphenyl)sulfonium, 4-tert-butylphenyldiphenylsulfonium, tris(4-tert-butylphenyl)sulfonium, 3,4-di-tert-butoxyphenyldiphenylsulfonium, bis(3,4-di-tert-butoxyphenyl)sulfonium, diphenylsulfonium, (4-tert-butoxycarbonylmethoxyphenyl)sulfonium, (4-tert-butoxyphenyl)bis(4-dimethylaminophenyl)sulfonium, (4-tert-butoxyphenyl)bis(4-dimethylaminophenyl)sulfonium, (4-tert-butoxyphenyl)bis(4-dimethylaminophenyl)sulfonium, (4-n-hexyloxy-3,5-dimethylphenyl)bis(4-hydroxy-3,5-dimethylphenyl)sulfonium, (4-n-hexyloxy-3,5-dimethylphenyl)bis(4-tert-butoxyphenyl)sulfonium, and the like. In addition, 4-methacryloyloxyphenyl diphenylsulfonium, 4-acryloyloxyphenyl diphenylsulfonium, 4-methacryloyloxyphenyl dimethylsulfonium, 4-acryloyloxyphenyl dimethylsulfonium, (4-methacryloyloxy-3,5-dimethylphenyl) diphenylsulfonium, (4-acryloyloxy-3,5-dimethylphenyl) diphenylsulfonium, etc. are mentioned. More preferred are triphenylsulfonium, 4-tert-butylphenyl diphenylsulfonium, 4-tert-butoxyphenyl diphenylsulfonium, 10-phenylphenoxathiol, S-phenyl dibenzothiophenium, etc. Among them, more preferred are triphenylsulfonium, 4-tert-butylphenyl diphenylsulfonium, and 4-tert-butoxyphenyl diphenylsulfonium.
[0225] In the above general formula (3), R 4 and R 5Specifically, the substitution position of phenyl, naphthyl and substituent is arbitrary, for example, tolyl, xylyl, trimethylphenyl, ethylphenyl, isopropylphenyl, tert-butylphenyl, 1-adamantylphenyl, triisopropylphenyl, tricyclohexylphenyl, methoxyphenyl, ethoxyphenyl, butoxyphenyl, hydroxyphenyl, dihydroxyphenyl, trimethoxyphenyl, methylthiophenyl, biphenyl, fluorophenyl, difluorophenyl, bromophenyl, iodophenyl, N,N-diphenylaminophenyl, acetoxyphenyl, acetylaminophenyl, 2,2,2-trifluoroethoxyphenyl, (2-methoxyethoxy)phenyl, hydroxynaphthyl, dihydroxynaphthyl, 2,2,2-trifluoroethoxynaphthyl, (2-methoxyethoxy)naphthyl, etc., but are not limited to these.
[0226] Just R 4 and R 5 For example, unsubstituted phenyl or phenyl having a substituent selected from halogen atoms, alkyl groups and alkoxy groups at the para position of the iodine atom is preferred, and phenyl, 4-tert-butylphenyl, 4-fluorophenyl and the like are particularly preferred.
[0227] R 4 and R 5 When the groups are bonded directly or via an oxygen atom, a methylene group, a sulfone group or a carbonyl group, the partial structures shown below can be cited, but are not limited to these. In the following formula, any position on the aromatic ring may have a substituent.
[0228] [Chemistry 14]
[0229]
[0230] More specifically, examples of the iodonium cation are shown below, but are not limited thereto. In the following formula, tBu is a tert-butyl group, and Ph is a phenyl group.
[0231] [Chemistry 15]
[0232]
[0233] The ammonium cation represented by the general formula (4) above includes ammonium cations and quaternary ammonium cations to which a proton is added to the nitrogen atom of ammonia, primary, secondary, tertiary aliphatic amines, mixed amines, aromatic amines, heterocyclic amines, nitrogen-containing compounds having a carboxyl group, nitrogen-containing compounds having a sulfonyl group, nitrogen-containing compounds having a hydroxyl group, nitrogen-containing compounds having a hydroxyphenyl group, alcoholic nitrogen-containing compounds, etc.
[0234] Specifically, primary aliphatic amines such as methylammonium, ethylammonium, n-propylammonium, isopropylammonium, n-butylammonium, isobutylammonium, sec-butylammonium, tert-butylammonium, amylammonium, tert-amylammonium, cyclopentylammonium, hexylammonium, cyclohexylammonium, heptylammonium, octylammonium, nonylammonium, decylammonium, dodecylammonium, cetylammonium, aminomethylammonium, 2-aminoethylammonium, and secondary aliphatic amines such as dimethylammonium, diethylammonium, di-n-propylammonium, diisopropylammonium, di-n-butylammonium, diisobutylammonium, di-sec-butylammonium, diamylammonium, dicyclopentylammonium, dihexylammonium, dicyclohexylammonium, diheptylammonium ammonium, trimethylammonium, triethylammonium, tri-n-propylammonium, triisopropylammonium, tri-n-butylammonium, triisobutylammonium, tri-sec-butylammonium, tripentylammonium, tricyclopentylammonium, trihexylammonium, tricyclohexylammonium, triheptylammonium, trioctylammonium, trinonylammonium, tridecylammonium, tridodecylammonium, tridodecylammonium, tricetylammonium, dimethyl(dimethylamino)methylammonium, methyl-2-(methylamino)ethylammonium, etc.; tertiary aliphatic amines such as trimethylammonium, triethylammonium, tri-n-propylammonium, triisopropylammonium, tri-n-butylammonium, triisobutylammonium, tri-sec-butylammonium, tripentylammonium, tricyclopentylammonium, trihexylammonium, tricyclohexylammonium, triheptylammonium, trioctylammonium, trinonylammonium, tridecylammonium, tridodecylammonium, tricetylammonium, dimethyl(dimethylamino)methylammonium, dimethyl(2-dimethylaminoethyl)ammonium, etc.
[0235] Moreover, examples of the mixed amines include dimethylethylammonium, methylpropylammonium, benzylammonium, phenethylammonium, benzyldimethylammonium and the like. Specific examples of aromatic amines and heterocyclic amines include anilinium derivatives (e.g., anilinium, N-methylanilinium, N-ethylanilinium, n-propylanilinium, N,N-dimethylanilinium, 2-methylanilinium, 3-methylanilinium, 4-methylanilinium, ethylanilinium at any substitution position, propylanilinium at any substitution position, trimethylanilinium at any substitution position, 2-nitroanilinium, 3-nitroanilinium, 4-nitroanilinium, 2,4-dinitroanilinium, 2,6-dinitroanilinium, 3,5-dinitroanilinium, N,N-dimethyltoluinium at any substitution position), diphenyl (p-toluene) derivatives. ammonium, methyldiphenylammonium, triphenylammonium, aminophenylammonium substituted at any position, naphthylammonium, aminonaphthylammonium substituted at any position, pyrrolinium derivatives (e.g., pyrrolinium, 2H-pyrrolinium, 1-methylpyrrolinium, 2,4-dimethylpyrrolinium, 2,5-dimethylpyrrolinium, N-methylpyrrolinium, etc.), oxazolium derivatives (e.g., oxazolium, isoxazolium, etc.), thiazolium derivatives (e.g., thiazolium, isothiazolium, etc.), imidazolium derivatives (e.g., imidazolium, 4-methylimidazolium, 4-methyl-2-phenylimidazolium, etc.), pyrazolium derivatives, furazanium derivatives, 2-methyl-1-pyrrolinium, etc. and the like), imidazolinium derivatives, imidazolidinium derivatives, pyridinium derivatives (e.g., pyridinium, methylpyridinium, ethylpyridinium, propylpyridinium, butylpyridinium, 4-(1-butylpentyl)pyridinium, dimethylpyridinium, trimethylpyridinium, triethylpyridinium, phenylpyridinium, 3-methyl-2-phenylpyridinium, 4-tert-butylpyridinium, diphenylpyridinium, benzylpyridinium, methoxypyridinium, butoxypyridinium, dimethoxypyridinium, 4-pyrrolidinylpyridinium, 2-(1-ethyl)pyridinium, 2-(2-methyl-2-phenyl ...
[0063] The invention also includes but is not limited to: 1,2-dopamine derivatives, 1,2-dopamine derivatives, 1,2-dopamine derivatives, 1,2-dopamine derivatives, 1,2-dopamine derivatives, 1,2-dopamine derivatives, 1,2-dopamine derivatives, 1,2-dopamine derivatives, 1,2-dopamine derivatives, 1,2-dopamine derivatives, 1,2-dopamine derivatives, 1,2-dopamine derivatives, 1,2-dopamine derivatives, 1,2-dopamine derivatives, 1,2-dopamine derivatives, 1,2-dopamine derivatives, 1,2-dopamine derivatives, 1,2-dopamine derivatives, 1,2-dopamine derivatives, 1,2-dopamine derivatives, 1,2-dopamine derivatives, 1,2-dopamine derivatives, 1,2-dopamine derivatives, 1,2-dopamine derivatives, 1,2-dopamine derivatives, 1,2-dopamine derivatives, 1,2-dopamine derivatives, 1,2-dopamine derivatives, 1,2-dopamine derivatives, 1,2-dopamine derivatives, 1,2-dopamine derivatives, 1,2-dopamine derivatives, 1,2-dopamine derivatives,
[0236] In addition, the nitrogen-containing compounds having a carboxyl group include carboxyphenylamine, carboxyindolium, amino acid derivatives (for example, nicotinic acid, alanine, arginine, aspartic acid, glutamic acid, glycine, histidine, isoleucine, glycylleucine, leucine, methionine, phenylalanine, threonine, lysine, 3-aminopyrazine-2-carboxylic acid, methoxyalanine and other proton addition products), the nitrogen-containing compounds having a sulfonyl group include 3-pyridiniumsulfonic acid, the nitrogen-containing compounds having a hydroxyl group, the nitrogen-containing compounds having a hydroxyphenyl group, and the nitrogen-containing compounds having an alcoholic group include 2-hydroxypyridinium, hydroxyanilinium at any substituted position, hydroxy-methyl-anilinium at any substituted position, hydroxyquinolinium, dihydroxy Quinolinium, 2-hydroxyethylammonium, bis(2-hydroxyethyl)ammonium, tris(2-hydroxyethyl)ammonium, ethylbis(2-hydroxyethyl)ammonium, diethyl(2-hydroxyethyl)ammonium, hydroxypropylammonium, bis(hydroxypropyl)ammonium, tris(hydroxypropyl)ammonium, 4-(2-hydroxyethyl)morpholinium, 2-(2-hydroxyethyl)pyridinium, 1-(2-hydroxyethyl)piperazinium, 1-[2-(2-hydroxyethoxy)ethyl]piperazinium, (2-hydroxyethyl)piperazinium, 1-(2-hydroxyethyl)pyrrolidinium, 1-(2-hydroxyethyl)-2-pyrrolidinium, 2,3-dihydroxypropylpiperidinium, 2,3-dihydroxypropylpyrrolidinium, 8-hydroxyjulolidineium, 3-hydroxyquinuclidinium, and the like.
[0237] Specific examples of the quaternary ammonium salt include tetramethylammonium, triethylmethylammonium, tetraethylammonium, tetrabutylammonium, tetraoctylammonium, dodecyldimethylammonium, tridecylmethylammonium, hexadecyltrimethylammonium, stearyltrimethylammonium, benzyltrimethylammonium, benzyltriethylammonium, benzyltributylammonium, and 2-hydroxyethyltrimethylammonium.
[0238] The ammonium cation is preferably a quaternary ammonium cation, and tetramethylammonium cation, tetraethylammonium cation and tetrabutylammonium cation are particularly preferred.
[0239] In this case, X in the above general formulas (2), (3) and (4) - It is more preferably any anion selected from the group consisting of a structure represented by any one of the following general formulae (5), (6) and (7), and chloride ion, bromide ion, iodide ion, fluoride ion, cyanide ion, nitrate ion and nitrite ion.
[0240] [Chemistry 16]
[0241]
[0242] In the formula, R 10It represents a linear, branched, or cyclic alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms, which may contain one or more selected from an ether group, an ester group, and a carbonyl group, and some or all of the hydrogen atoms in these groups may be substituted with one or more selected from a halogen atom, a hydroxyl group, a carboxyl group, an amino group, and a cyano group. 11 R represents an aryl group having 6 to 20 carbon atoms, wherein a part or all of the hydrogen atoms of the aryl group may be substituted with one or more selected from a halogen atom, a hydroxyl group, a carboxyl group, an amino group, and a cyano group. 12 , R 13 , and R 14 Each independently represents a hydrogen atom, a halogen atom other than a fluorine atom, or a linear, branched, or cyclic alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms, which may contain one or more selected from an ether group, an ester group, and a carbonyl group, and a part or all of the hydrogen atoms in these groups may be substituted by one or more selected from a halogen atom, a hydroxyl group, a carboxyl group, an amino group, and a cyano group. 12 , R 13 , and R 14 Two or more of them may be bonded to each other to form a ring.
[0243] Specific examples of the carboxylic acid anion represented by the general formula (5) include formic acid anion, acetic acid anion, propionic acid anion, butyric acid anion, isobutyric acid anion, valeric acid anion, isovaleric acid anion, trimethylacetic acid anion, hexanoic acid anion, octanoic acid anion, cyclohexanecarboxylic acid anion, cyclohexylacetic acid anion, lauric acid anion, myristic acid anion, palmitic acid anion, stearic acid anion, phenylacetic acid anion, diphenylacetic acid anion, phenoxyacetic acid anion, mandelic acid anion, acid) anion, benzoylformate anion, cinnamic acid anion, dihydrocinnamic acid anion, benzoic acid anion, methylbenzoic acid anion, salicylic acid anion, naphthalenecarboxylic acid anion, anthracenecarboxylic acid anion, anthraquinonecarboxylic acid anion, glycolic acid anion, trimethylacetic acid anion, lactic acid anion, methoxyacetic acid anion, 2-(2-methoxyethoxy)acetic acid anion, 2-(2-(2-methoxyethoxy)ethoxy)acetic acid anion ions, bisphenol acid anions, monochloroacetic acid anions, dichloroacetic acid anions, trichloroacetic acid anions, trifluoroacetic acid anions, pentafluoropropionic acid anions, heptafluorobutyric acid anions, 2-hydroxy-2,2-bis(trifluoromethyl)acetic acid anions, and monoanions of dicarboxylic acids such as succinic acid, tartaric acid, glutaric acid, pimelic acid, sebacic acid, phthalic acid, isophthalic acid, terephthalic acid, naphthalene dicarboxylic acid, cyclohexane dicarboxylic acid, and cyclohexene dicarboxylic acid can also be mentioned.
[0244] Specific examples of the aromatic hydrocarbon sulfonate anion represented by the general formula (6) include benzenesulfonate, 4-toluenesulfonate, 2-toluenesulfonate, xylenesulfonate substituted at any position, trimethylbenzenesulfonate, mesitylenesulfonate, 4-methoxybenzenesulfonate, 4-ethylbenzenesulfonate, 2,4,6-triisopropylbenzenesulfonate, 1-naphthalenesulfonate, 2-naphthalenesulfonate, anthraquinone-1-sulfonate, anthraquinone-2-sulfonate, 4-(4-methylbenzenesulfonyloxy)benzenesulfonate, 3,4-bis(4-methylbenzenesulfonyloxy)benzenesulfonate, 6-(4-methylbenzenesulfonyloxy)naphthalene-2-sulfonate, 4-phenoxybenzenesulfonate, 4-diphenylmethylbenzenesulfonate, 2,4-dinitrobenzenesulfonate, and dodecylbenzenesulfonate.
[0245] Specific examples of the alkanesulfonate anion represented by the general formula (7) include methanesulfonate, ethanesulfonate, propanesulfonate, butanesulfonate, pentanesulfonate, hexanesulfonate, cyclohexanesulfonate, octanesulfonate, and 10-camphorsulfonate.
[0246] Furthermore, X in the above general formulae (2), (3) and (4) - The boiling point of the conjugate acid XH is more preferably 200° C. or less. In the present specification, the boiling point is a value at 1 atmosphere (1013 hPa).
[0247] X in the above general formulae (2), (3) and (4) - Particularly preferred are trifluoroacetic acid anion, pentafluoropropionic acid anion, 2-hydroxy-2,2-bis(trifluoromethyl)acetic acid anion, chloride ion and nitrate ion.
[0248] The aforementioned (C) base generator may include any combination of the aforementioned specific examples of cations and specific examples of anions, but is not limited thereto. Also, the following are examples of the ideal structure. Also, in the following formula, tBu is a tert-butyl group.
[0249] [Chemistry 17]
[0250]
[0251] The aforementioned (C) base generators can exhibit alkalinity in accordance with the firing temperature of the resist lower film material by using one alone or in combination of two or more, and can appropriately adjust the balance between film-forming properties and flatness for hydrophobic substrates. The amount of the (C) base generator added is preferably 0.1 to 10 parts by mass, and more preferably 0.3 to 3 parts by mass, relative to 100 parts by mass of the aforementioned (A) resin. If the amount of the (C) base generator added is within the aforementioned range, a sufficient film-forming property improvement effect can be obtained, and there is no risk of deterioration of the in-plane uniformity of the film due to decomposition and sublimation, or a decrease in the curability of the compound or resin due to alkalinity.
[0252] The (C) base generator used in the resist underlayer film forming composition is preferably represented by the general formula (2) or (4), and particularly preferably represented by the general formula (2).
[0253] The resist underlayer film-forming composition preferably further contains one or more selected from the group consisting of (D) a crosslinking agent, (E) a fluidity promoter, and (F) a surfactant.
[0254] [(D) Cross-linking agent]
[0255] In addition, a (D) crosslinking agent may be added to the resist underlayer film forming composition used in the pattern forming method of the present invention. The crosslinking agent used is not particularly limited, and various well-known systems of crosslinking agents can be widely used. For example, hydroxymethyl or alkoxymethyl type crosslinking agents (polynuclear phenol crosslinking agents) of polynuclear phenols, melamine crosslinking agents, glycoluril crosslinking agents, benzoguanamine crosslinking agents, urea crosslinking agents, β-hydroxyalkylamide crosslinking agents, isocyanurate crosslinking agents, aziridine crosslinking agents, oxazoline crosslinking agents, and epoxy crosslinking agents. The amount of the crosslinking agent (D) added is preferably 1 to 50 parts by mass, and more preferably 5 to 30 parts by mass, relative to 100 parts by mass of the aforementioned (A) resin.
[0256] Specific examples of the melamine-based crosslinking agent include hexamethoxymethylated melamine, hexabutoxymethylated melamine, alkoxy and / or hydroxyl-substituted melamines thereof, and partially self-condensed products thereof.
[0257] Specific examples of the glycoluril-based crosslinking agent include tetramethoxymethyl glycoluril, tetrabutoxymethyl glycoluril, alkoxy and / or hydroxyl-substituted products thereof, and partial self-condensation products thereof.
[0258] Specific examples of the benzoguanamine-based crosslinking agent include tetramethoxymethylated benzoguanamine, tetrabutoxymethylated benzoguanamine, alkoxy and / or hydroxyl-substituted products thereof, and partial self-condensation products thereof.
[0259] Specific examples of the urea crosslinking agent include dimethoxymethylated dimethoxyethylene urea, alkoxy and / or hydroxyl-substituted products thereof, and partial self-condensates thereof.
[0260] Specific examples of the β-hydroxyalkylamide crosslinking agent include N,N,N',N'-tetrakis(2-hydroxyethyl)adipamide.
[0261] Specific examples of the isocyanurate crosslinking agent include triglycidyl isocyanurate and triallyl isocyanurate.
[0262] Specific examples of the aziridine crosslinking agent include 4,4′-bis(ethyleneiminocarbonylamino)diphenylmethane and 2,2-bishydroxymethylbutanol-tris[3-(1-aziridinyl)propionate].
[0263] Oxazoline crosslinking agents include, for example, 2,2'-isopropylidenebis(4-benzyl-2-oxazoline), 2,2'-isopropylidenebis(4-phenyl-2-oxazoline), 2,2'-methylenebis-4,5-diphenyl-2-oxazoline, 2,2'-methylenebis-4-phenyl-2-oxazoline, 2,2'-methylenebis-4-tert-butyl-2-oxazoline, 2,2'-bis(2-oxazoline), 1,3-phenylenebis(2-oxazoline), 1,4-phenylenebis(2-oxazoline), and 2-isopropenyloxazoline copolymers.
[0264] Specific examples of the epoxy crosslinking agent include diglycidyl ether, ethylene glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, 1,4-cyclohexanedimethanol diglycidyl ether, poly(glycidyl methacrylate), trimethylolethane triglycidyl ether, trimethylolpropane triglycidyl ether, and pentaerythritol tetraglycidyl ether.
[0265] Specific examples of the polynuclear phenol-based crosslinking agent include compounds represented by the following general formula (XL-1).
[0266] [Chemistry 18]
[0267]
[0268] In the general formula (XL-1), Q is a single bond or a q-valent hydrocarbon group having 1 to 20 carbon atoms. R3 is a hydrogen atom or an alkyl group having 1 to 20 carbon atoms. q is an integer of 1 to 5.
[0269] Q is a single bond or a q-valent hydrocarbon group having 1 to 20 carbon atoms. Q is an integer of 1 to 5, preferably 2 or 3. Specifically, Q is a group obtained by removing q hydrogen atoms from methane, ethane, propane, butane, isobutane, pentane, cyclopentane, hexane, cyclohexane, methylpentane, methylcyclohexane, dimethylcyclohexane, trimethylcyclohexane, benzene, toluene, xylene, ethylbenzene, ethylisopropylbenzene, diisopropylbenzene, methylnaphthalene, ethylnaphthalene, or eicosane. R3 is a hydrogen atom or an alkyl group having 1 to 20 carbon atoms. Specifically, the alkyl group having 1 to 20 carbon atoms is, for example, methyl, ethyl, propyl, isopropyl, butyl, isobutyl, pentyl, isopentyl, hexyl, octyl, ethylhexyl, decyl, or eicosyl, and a hydrogen atom or a methyl group is preferred.
[0270] Examples of compounds represented by the general formula (XL-1) include the following compounds. Among them, trisphenolmethane, trisphenolethane, 1,1,1-tris(4-hydroxyphenyl)ethane, and hexamethoxymethylated tris(4-hydroxyphenyl)-1-ethyl-4-isopropylbenzene are preferred from the viewpoint of improving the hardening property and film thickness uniformity of the resist underlayer film. R3 is the same as described above.
[0271] [Chemistry 19]
[0272]
[0273] [Chemistry 20]
[0274]
[0275] [(E) Flowability enhancer]
[0276] Furthermore, the resist underlayer film forming composition used in the pattern forming method of the present invention may contain (E) a fluidity enhancer. The fluidity enhancer (E) preferably has a weight loss rate of less than 30% at 30°C to 190°C and a weight loss rate of 98% or more at 30°C to 350°C.
[0277] The fluidity enhancer having a weight loss rate of less than 30% between 30°C and 190°C and a weight loss rate of 98% or more between 30°C and 350°C is preferably used because its evaporation during heat treatment is suppressed, the viscosity is sufficiently kept low, the thermal fluidity is excellent, and the residual fluidity enhancer in the resist underlayer film after firing is small. In this specification, the weight loss rate is a value obtained by TG (thermogravimetric) measurement using a differential thermobalance.
[0278] The upper limit of the temperature range in which the weight loss rate of the fluidity enhancer (E) does not reach 30% is preferably 210° C., and more preferably 230° C. When the weight loss rate of the fluidity enhancer does not reach 30% within the above temperature range, the filling / planarization characteristics can be further improved.
[0279] The upper limit of the temperature range in which the weight reduction rate of the fluidity promoter (E) is 98% or more is preferably 330° C., and more preferably 310° C. By setting the temperature in which the weight reduction rate of the fluidity promoter is 98% or more to the above temperature range, the residual fluidity promoter in the resist underlayer film after firing can be reduced.
[0280] By adding the above-mentioned fluidity promoter, the thermal fluidity of the resist underlayer film forming composition from the start of heat treatment to hardening due to the crosslinking reaction is improved, so that the embedding / planarization characteristics are excellent. On the other hand, the fluidity promoter is reduced by heat treatment, evaporation, etc., so that the etching resistance and optical characteristics are not impaired.
[0281] A more preferred embodiment of the fluidity enhancer (E) is, for example, one or more compounds selected from the group consisting of the following general formulae (i) to (iii).
[0282] [Chemistry 21]
[0283]
[0284] In the general formula (i), R' 1 Each independently represents a hydrogen atom, a hydroxyl group, or an optionally substituted organic group having 1 to 10 carbon atoms. 1 W is a phenylene group or a divalent group represented by the following general formula (i-1). 2 , W 3 is a single bond or a divalent group represented by any one of the following formulas (i-2). 1 is an integer from 1 to 10, n 1 An integer from 0 to 5.
[0285] [Chemistry 22]
[0286]
[0287] In the general formula (i-1), * represents the bonding position, R' 10 , R' 11 , R' 12 , R' 13 W is a hydrogen atom, a hydroxyl group, or an organic group having 1 to 10 carbon atoms. 10 , W 11 Each independently represents a single bond or a carbonyl group. 10 、m 11 is an integer from 0 to 10, m 10 +m 11 ≥1.
[0288] [Chemistry 23]
[0289]
[0290] In formula (i-2), * represents a bonding position.
[0291] [Chemistry 24]
[0292]
[0293] In the general formula (ii), R' 2 Each independently represents a hydrogen atom or an optionally substituted organic group having 1 to 10 carbon atoms. 4 W is a divalent group represented by the following general formula (ii-1). 5 It is a single bond or a divalent group represented by any one of the following formulas (ii-2). 2is an integer from 2 to 10, n 3 An integer from 0 to 5.
[0294] [Chemistry 25]
[0295]
[0296] In the general formula (ii-1), * represents the bonding position, R 20 , R 21 , R 22 , R 23 is a hydrogen atom, a hydroxyl group, or an organic group having 1 to 10 carbon atoms. 20 、m 21 is an integer from 0 to 10, m 20 +m 21 ≥1.
[0297] [Chemistry 26]
[0298]
[0299] In formula (ii-2), * represents a bonding position.
[0300] [Chemistry 27]
[0301]
[0302] In the general formula (iii), R' 3 , R' 4 is a hydrogen atom, a hydroxyl group, or an organic group having 1 to 10 carbon atoms which may be substituted, and may be bonded to each other to form a ring structure. 5 , R' 6 is an organic group having 1 to 10 carbon atoms, R' 5 A group containing an aromatic ring or one of the divalent groups represented by the following general formula (iii-1). 6 , W 7 It is a single bond or a divalent group represented by any one of the following formulas (iii-2), and at least one of them is a divalent group represented by any one of the following formulas (iii-2).
[0303] [Chemistry 28]
[0304]
[0305] In the general formula (iii-1), * represents the bonding position, W 30 It is an organic group having 1 to 4 carbon atoms.
[0306] [Chemistry 29]
[0307]
[0308] In formula (iii-2), * represents a bonding position.
[0309] In the above general formula (i), R' 1 Each is independently a hydrogen atom, a hydroxyl group, or an optionally substituted organic group having 1 to 10 carbon atoms.
[0310] Here, in the present invention, the "organic group" refers to a group containing at least one carbon atom, and may further contain a hydrogen atom, and may also contain a nitrogen atom, an oxygen atom, a sulfur atom, a silicon atom, a halogen atom, and the like.
[0311] R' 1 It can be a single type or a mixture of multiple types. 1 More specifically, for example, a hydrogen atom, a hydroxyl group, a methyl group, an ethyl group, a vinyl group, a 2,2,2-trifluoroethyl group, a propyl group, an isopropyl group, an allyl group, a butyl group, a sec-butyl group, a tert-butyl group, an isobutyl group, a pentyl group, a cyclopentyl group, a hexyl group, a cyclohexyl group, a cyclohexenyl group, a decyl group, a methoxy group, an ethoxy group, a propoxy group, an isopropoxy group, a butoxy group, a sec-butoxy group, a tert-butoxy group, a norbornyl group, an adamantyl group, a phenyl group, a toluoyl group, a xylyl group, a naphthyl group, a benzyl group, a 2-furyl group, and a 2-tetrahydrofuranyl group. Among these, a hydrogen atom is more preferable.
[0312] W 1 W is a phenylene group or a divalent group represented by the above general formula (i-1). 2 , W 3 is a single bond or a divalent group represented by any one of the above formula (i-2). 1 is an integer from 1 to 10, n 1 Each independently represents an integer from 0 to 5.
[0313] R' 10 , R' 11 , R' 12 , R' 13 More specifically, it is a hydrogen atom, a hydroxyl group, or an organic group having 1 to 10 carbon atoms. More specifically, for example, a hydrogen atom, a hydroxyl group, a methyl group, an ethyl group, a vinyl group, a 2,2,2-trifluoroethyl group, a propyl group, an isopropyl group, an allyl group, a butyl group, a sec-butyl group, a tert-butyl group, an isobutyl group, a pentyl group, a cyclopentyl group, a hexyl group, a cyclohexyl group, a cyclohexenyl group, a decyl group, a methoxy group, an ethoxy group, a propoxy group, an isopropoxy group, a butoxy group, a sec-butoxy group, a tert-butoxy group, a norbornyl group, an adamantyl group, a phenyl group, a toluoyl group, a xylyl group, a naphthyl group, a benzyl group, a 2-furyl group, and a 2-tetrahydrofuranyl group. Among these, a hydrogen atom and a methyl group are more preferred, and a hydrogen atom is more desirable.
[0314] W 10 , W 11 Each independently represents a single bond or a carbonyl group. 10 、m 11 is an integer from 0 to 10, m10 +m 11 ≥1.
[0315] In the above general formula (ii), R' 2 Each is independently a hydrogen atom or an optionally substituted organic group having 1 to 10 carbon atoms.
[0316] R' 2 It can be a single type or a mixture of multiple types. 2 More specifically, for example, a hydrogen atom, a methyl group, an ethyl group, a vinyl group, a 2,2,2-trifluoroethyl group, a propyl group, an isopropyl group, an allyl group, a butyl group, a sec-butyl group, a tert-butyl group, an isobutyl group, a pentyl group, a cyclopentyl group, a hexyl group, a cyclohexyl group, a cyclohexenyl group, a decyl group, a methoxy group, an ethoxy group, a propoxy group, an isopropoxy group, a butoxy group, a sec-butoxy group, a tert-butoxy group, a norbornyl group, an adamantyl group, a phenyl group, a toluoyl group, a xylyl group, a naphthyl group, a benzyl group, a 2-furyl group, and a 2-tetrahydrofuranyl group. Among these, a hydrogen atom is more preferable.
[0317] W 4 W is a divalent group represented by the above general formula (ii-1). 5 is a single bond or a divalent group represented by any one of the above formula (ii-2). 2 is an integer from 2 to 10, n 3 An integer from 0 to 5.
[0318] R 20 , R 21 , R 22 , R 23 , more specifically, for example, a hydrogen atom, a hydroxyl group, a methyl group, an ethyl group, a vinyl group, a 2,2,2-trifluoroethyl group, a propyl group, an isopropyl group, an allyl group, a butyl group, a sec-butyl group, a tert-butyl group, an isobutyl group, a pentyl group, a cyclopentyl group, a hexyl group, a cyclohexyl group, a cyclohexenyl group, a decyl group, a methoxy group, an ethoxy group, a propoxy group, an isopropoxy group, a butoxy group, a sec-butoxy group, a tert-butoxy group, a norbornyl group, an adamantyl group, a phenyl group, a toluoyl group, a xylyl group, a naphthyl group, a benzyl group, a 2-furyl group, and a 2-tetrahydrofuranyl group. Among these, a hydrogen atom and a methyl group are more preferred, and a hydrogen atom is more desirable.
[0319] m 20 、m 21 is an integer from 0 to 10, m 20 +m 21 ≥1.
[0320] In the above general formula (iii), R' 3 , R' 4It is a hydrogen atom, a hydroxyl group, or an organic group having 1 to 10 carbon atoms which may be substituted, and may be bonded to each other to form a ring structure. More specifically, for example, a hydrogen atom, a hydroxyl group, a methyl group, an ethyl group, a vinyl group, a 2,2,2-trifluoroethyl group, a propyl group, an isopropyl group, an allyl group, a butyl group, a sec-butyl group, a tert-butyl group, an isobutyl group, a pentyl group, a cyclopentyl group, a hexyl group, a cyclohexyl group, a cyclohexenyl group, a decyl group, a methoxy group, an ethoxy group, a propoxy group, an isopropoxy group, a butoxy group, a sec-butoxy group, a tert-butoxy group, a norbornyl group, an adamantyl group, a phenyl group, a toluoyl group, a xylyl group, a naphthyl group, a benzyl group, a 2-furanyl group, and a 2-tetrahydrofuranyl group. Among these, a hydrogen atom is more desirable.
[0321] R' 5 is an organic group having 1 to 10 carbon atoms and containing an aromatic ring or one of the divalent groups represented by the general formula (iii-1). 6 is an organic group having 1 to 10 carbon atoms. Examples of the organic group having 1 to 10 carbon atoms include the organic group 3 , R' 4 Groups cited.
[0322] W 6 , W 7 It is a single bond or a divalent group represented by any one of the above formula (iii-2), and at least one of them is a divalent group represented by any one of the above formula (iii-2).
[0323] W 30 It is an organic group having 1 to 4 carbon atoms. More specifically, it includes methylene, ethylene, propylene, butylene, trimethylene, and tetramethylene. Among these, ethylene is more preferred.
[0324] More specifically, the compound represented by the general formula (i) is exemplified below, but is not limited thereto.
[0325] [Chemistry 30]
[0326]
[0327] More specifically, the compound represented by the general formula (ii) is exemplified below, but is not limited thereto.
[0328] [Chemistry 31]
[0329]
[0330] More specifically, the compound represented by the general formula (iii) is exemplified below, but is not limited thereto.
[0331] [Chemistry 32]
[0332]
[0333] If the film-forming properties of the resist underlayer film forming composition, the filling / planarization performance of the substrate, etc. are comprehensively considered, it is ideal that the (E) fluidity promoter used in the above-mentioned resist underlayer film forming composition is an aromatic compound having a benzyl group or a benzoyl group, especially the aromatic compounds as follows.
[0334] (i) (Poly)ethylene glycol dibenzoate
[0335] (ii) (Poly)ethylene glycol dibenzyl ether
[0336] (iii) (Poly)propylene glycol dibenzyl ether
[0337] (iv) (Poly)butylene glycol dibenzyl ether
[0338] (v) Straight-chain aliphatic dicarboxylic acid dibenzyl ester
[0339] (vi) (Poly)ethylene glycol monobenzyl ether
[0340] (vii) (Poly)phenylene ether
[0341] [Chemistry 33]
[0342]
[0343] In addition, n in the above formula is an integer within the range of molecular weight of 500 or less, and is applicable only to this formula.
[0344] The (E) fluidity enhancer used in the resist underlayer film forming composition preferably has a structure having both a hydrophobic portion consisting of an aromatic ring and a hydrophilic portion consisting of the following (E-1) structure. Such a fluidity enhancer (E) has excellent compatibility with the (A) resin, (B) organic solvent, (C) base generator and other additives, and can improve the fluidity of the composition without impairing film forming properties and storage stability.
[0345] [Chemistry 34]
[0346]
[0347] In the formula, * represents a bonding position, and W is an organic group having 1 to 4 carbon atoms.
[0348] The amount of the fluidity promoter (E) added is preferably 5 to 100 parts by mass, more preferably 10 to 50 parts by mass, relative to 100 parts by mass of the resin (A). If the amount of the fluidity promoter (E) added is 5 parts by mass or more, the fluidity improvement effect of the resist underlayer film-forming composition can be fully obtained. On the other hand, if the amount of the fluidity promoter (E) added is 100 parts by mass or less, the film-forming property and dry etching resistance of the obtained coating film are excellent.
[0349] The (E) fluidity improver may be used alone or in combination of two or more.
[0350] [(F) Surfactant]
[0351] In order to improve the coating property of spin coating, a surfactant (F) may be added to the resist underlayer film forming composition used in the pattern forming method of the present invention. The surfactant (F) may be, for example, the surfactant described in paragraphs
[0142] to
[0147] of Japanese Patent Application Laid-Open No. 2009-269953. The amount of the surfactant (F) added is preferably 0.01 to 10 parts by mass, more preferably 0.05 to 5 parts by mass, relative to 100 parts by mass of the resin (A).
[0352] [(G) Plasticizer]
[0353] In addition, in order to further improve the planarization / burying characteristics, a (G) plasticizer may be added to the resist underlayer film forming composition used in the pattern forming method of the present invention. There are no special restrictions on the (G) plasticizer, and plasticizers of various known systems can be widely used. For example, low molecular weight compounds such as phthalates, adipic acid esters, phosphates, trimellitic acid esters, and citrates, polyethers, polyesters, and polymers such as polyacetal polymers recorded in Japanese Patent Gazette No. 2013-253227. The amount of the (G) plasticizer added is preferably 1 to 100 parts by mass, and more preferably 5 to 30 parts by mass, relative to 100 parts by mass of the aforementioned (A) resin.
[0354] In the resist underlayer film forming composition of the present invention, in order to impart the filling / planarizing properties similarly to the plasticizer, a liquid additive having a polyethylene glycol or polypropylene glycol structure, or a pyrolyzable polymer having a weight loss rate of 40% by mass or more between 30° C. and 250° C. and a weight average molecular weight of 300 to 200,000 is preferably used. The pyrolyzable polymer preferably contains a repeating unit having an acetal structure represented by the following general formula (DP1) or (DP1a).
[0355] [Chemistry 35]
[0356]
[0357] In the general formula (DP1), R6 is a hydrogen atom or an optionally substituted saturated or unsaturated monovalent organic group having 1 to 30 carbon atoms. Y is a saturated or unsaturated divalent organic group having 2 to 30 carbon atoms.
[0358] [Chemistry 36]
[0359]
[0360] In the general formula (DP1a), R 6a Y is an alkyl group having 1 to 4 carbon atoms. a It is a saturated or unsaturated divalent hydrocarbon group having 4 to 10 carbon atoms, and may have an ether bond. n represents the average number of repeating units and is 3 to 500.
[0361] Example
[0362] The following examples and comparative examples are given to specifically illustrate the present invention, but the present invention is not limited to these descriptions. In addition, the molecular weight and dispersity are measured by the following method. The weight average molecular weight (Mw) and dispersity (Mw / Mn) converted to polystyrene are determined by gel permeation chromatography (GPC) using tetrahydrofuran as the eluent.
[0363] Resin raw materials:
[0364] [Chemistry 37]
[0365]
[0366] Resins used as intermediates:
[0367] [Chemistry 38]
[0368]
[0369] Modifying agent:
[0370] [Chemistry 39]
[0371]
[0372] The above-mentioned resins (A-1) to (A-8) were synthesized in the following manner.
[0373] (Synthesis Example A-1)
[0374] Synthesis of resin (A-1)
[0375] [Chemistry 40]
[0376]
[0377] Under nitrogen atmosphere, 188.2 g of resin raw material (B-1), 81.3 g of resin raw material (B-7), 9.0 g of oxalic acid, and 100 g of dioxane were added, and the reaction was carried out at an internal temperature of 100°C for 24 hours. After the reaction was completed, it was cooled to room temperature, 2,000 ml of MIBK was added, and it was washed 6 times with 500 ml of pure water. The organic layer was recovered, and the pressure was reduced to 2 mmHg at an internal temperature of 150°C, and the water, solvent, and residual monomers were removed under reduced pressure to obtain resin (A-1).
[0378] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, and the following results were obtained.
[0379] (A-1): Mw=2,500, Mw / Mn=2.87
[0380] (Synthesis Example A-2)
[0381] Synthesis of resin (A-2)
[0382] [Chemistry 41]
[0383]
[0384] Under nitrogen atmosphere, 216.3 g of resin raw material (B-2), 81.3 g of resin raw material (B-7), 10.8 g of oxalic acid, and 200 g of dioxane were added, and the reaction was carried out at an internal temperature of 100°C for 24 hours. After the reaction was completed, it was cooled to room temperature, 2,000 ml of MIBK was added, and it was washed 6 times with 500 ml of pure water. The organic layer was recovered, and the pressure was reduced to 2 mmHg at an internal temperature of 150°C, and the water, solvent, and residual monomers were removed under reduced pressure to obtain resin (A-2).
[0385] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, and the following results were obtained.
[0386] (A-2): Mw=3,300, Mw / Mn=3.50
[0387] (Synthesis Example A-3)
[0388] Synthesis of resin (A-3)
[0389] [Chemistry 42]
[0390]
[0391] Under nitrogen atmosphere, 144.2 g of resin raw material (B-3), 53.2 g of resin raw material (B-7), and 250 g of PGME (propylene glycol monomethyl ether) were added and homogenized at an internal temperature of 100°C. Then, a mixed solution of 3.0 g of p-toluenesulfonic acid monohydrate and 7.1 g of PGME, which had been mixed and homogenized in advance, was slowly added dropwise, and the mixture was reacted at an internal temperature of 120°C for 8 hours. After the reaction was completed, the mixture was cooled to room temperature, 2,000 ml of MIBK was added, and the mixture was washed 6 times with 500 ml of pure water. The organic layer was dried under reduced pressure to obtain resin (A-3).
[0392] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, and the following results were obtained.
[0393] (A-3): Mw=2,900, Mw / Mn=2.26
[0394] (Synthesis Example A-4)
[0395] Synthesis of resin (A-4)
[0396] [Chemistry 43]
[0397]
[0398] Under nitrogen atmosphere, 144.2 g of resin raw material (B-4), 40.6 g of resin raw material (B-7), and 250 g of PGME (propylene glycol monomethyl ether) were added and homogenized at an internal temperature of 100°C. Then, a mixed solution of 3.0 g of p-toluenesulfonic acid monohydrate and 7.1 g of PGME, which had been mixed and homogenized, was slowly added dropwise, and the mixture was reacted at an internal temperature of 120°C for 8 hours. After the reaction was completed, the mixture was cooled to room temperature, 2,000 ml of MIBK was added, and the mixture was washed 6 times with 500 ml of pure water. The organic layer was dried under reduced pressure to obtain resin (A-4).
[0399] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, and the following results were obtained.
[0400] (A-4): Mw=3,300, Mw / Mn=2.26
[0401] (Synthesis Example A-5)
[0402] Synthesis of resin (A-5)
[0403] [Chemistry 44]
[0404]
[0405] Under nitrogen atmosphere, 160.2 g of resin raw material (B-5), 40.6 g of resin raw material (B-7), and 250 g of PGME (propylene glycol monomethyl ether) were added and homogenized at an internal temperature of 100°C. Then, a mixed solution of 3.2 g of p-toluenesulfonic acid monohydrate and 8.0 g of PGME, which had been mixed and homogenized in advance, was slowly added dropwise, and the mixture was reacted at an internal temperature of 120°C for 8 hours. After the reaction was completed, the mixture was cooled to room temperature, 2,000 ml of MIBK was added, and the mixture was washed 6 times with 500 ml of pure water. The organic layer was dried under reduced pressure to obtain resin (A-5).
[0406] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, and the following results were obtained.
[0407] (A-5): Mw=3,400, Mw / Mn=2.54
[0408] (Synthesis Example A-6)
[0409] Synthesis of resin (A-6)
[0410] [Chemistry 45]
[0411]
[0412] Under nitrogen atmosphere, 160.2 g of resin raw material (B-6), 40.6 g of resin raw material (B-7), and 300 g of PGME (propylene glycol monomethyl ether) were added and homogenized at an internal temperature of 100°C. Then, a mixed solution of 3.2 g of p-toluenesulfonic acid monohydrate and 8.0 g of PGME, which had been mixed and homogenized in advance, was slowly added dropwise, and the mixture was reacted at an internal temperature of 120°C for 8 hours. After the reaction was completed, the mixture was cooled to room temperature, 2,000 ml of MIBK was added, and the mixture was washed 6 times with 500 ml of pure water, and the organic layer was dried under reduced pressure to obtain resin (A-6).
[0413] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, and the following results were obtained.
[0414] (A-6): Mw=3,300, Mw / Mn=2.41
[0415] (Synthesis Example A-7)
[0416] Synthesis of resin (A-7)
[0417] [Chemistry 46]
[0418]
[0419] Under a nitrogen environment, 94.1 g of resin raw material (B-1), 89.8 g of resin raw material (B-8), and 400 g of dichloromethane were added to prepare a uniform dispersion at an internal temperature of 30°C. After that, 211 g of methanesulfonic acid was added over 2 hours, and the reaction was carried out at an internal temperature of 30°C for 24 hours. After the reaction was completed, it was cooled to room temperature, 2,000 ml of MIBK was added, and the mixture was washed 6 times with 500 ml of pure water, and the organic layer was dried under reduced pressure. 300 g of THF was added to the residue to prepare a uniform solution, and then crystallized in 2,000 g of hexane. The precipitated crystals were separated by filtration, washed twice with 500 g of hexane, and recovered. The recovered crystals were vacuum dried at 70°C to obtain resin (A-7).
[0420] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, and the following results were obtained.
[0421] (A-7): Mw=6,300, Mw / Mn=3.11
[0422] (Synthesis Example A-8)
[0423] Synthesis of comparative resin (A-8)
[0424] [Chemistry 47]
[0425]
[0426] Under nitrogen atmosphere, 100.0 g of monomer (B-9), 3.85 g of V-601 (2,2'-azobis(isobutyric acid) dimethyl ester, manufactured by Wako Pure Chemical Industries, Ltd.), and 340 g of PGMEA (propylene glycol monomethyl ether acetate) were measured in a 1 L graduated cylinder, and the mixture was degassed while stirring to prepare a monomer-polymerization initiator solution. 60 g of PGMEA was weighed in another 1 L flask under nitrogen atmosphere, and the mixture was degassed while stirring, and then heated until the internal temperature reached 80°C. After the aforementioned monomer-polymerization initiator solution was added dropwise over 4 hours, the temperature of the polymerization liquid was maintained at 80°C, stirring was continued for 16 hours, and then cooled to room temperature. The obtained polymerization liquid was added dropwise to 5,000 g of vigorously stirred hexane, and the precipitated polymer was filtered. Then, the obtained polymer was washed twice with 600 g of hexane, and vacuum dried at 50°C for 20 hours to obtain a comparative resin (A-8) in the form of a white powder.
[0427] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, and the following results were obtained.
[0428] (A-8): Mw=8,500, Mw / Mn=2.50
[0429] Synthesis of Resins (X-1) to (X-9), Comparative Example Resins (R-2) to (R-3), (R-5) to (R-6), and Comparative Example Compound (R-7)
[0430] [Synthesis Example 1] Synthesis of Resin (X-1)
[0431] [Chemistry 48]
[0432]
[0433] Under nitrogen atmosphere, add 20.0 g of resin (A-1), 31.3 g of potassium carbonate, and 100 g of DMF, and prepare a uniform dispersion at an internal temperature of 50°C. Slowly add 16.2 g of the modifying agent (c-1), and react at an internal temperature of 50°C for 24 hours. Add 300 ml of methyl isobutyl ketone and 300 g of pure water to the reaction solution, dissolve the precipitated salt, remove the separated water layer, add 1,500 g of hexane to obtain the organic layer, and remove the upper layer. Then, dissolve it again with 300 ml of methyl isobutyl ketone, wash it 6 times with 100 g of 3% nitric acid aqueous solution and 100 g of pure water, and then reduce the pressure to dry the organic layer to obtain resin (X-1).
[0434] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, and the following results were obtained.
[0435] (X-1): Mw=6,000, Mw / Mn=3.61
[0436] [Synthesis Examples 2 to 14] Synthesis of Resins (X-2) to (X-9), Comparative Example Resins (R-2) to (R-3), and (R-5)
[0437] Resins (A-1) to (A-8), modifiers (c-1) to (c-3), and potassium carbonate were used in the same reaction conditions as in Synthesis Example 1 except that the feed amounts shown in Tables 1 to 3 were used to obtain resins (X-2) to (X-9) shown in Tables 1 to 3 and comparative resins (R-2) to (R-3) and (R-5) as products. The weight average molecular weight (Mw) and dispersity (Mw / Mn) of these resins were calculated and are shown in Table 4. Comparative resins (A-8) (R-1) and resin (A-2) (R-4) are also shown.
[0438] [Table 1]
[0439]
[0440] [Table 2]
[0441]
[0442] [Table 3]
[0443]
[0444] [Synthesis Examples 15-16] Synthesis of Comparative Example Resin (R-6) and Comparative Example Compound (R-7) The following raw materials were used in the synthesis of Comparative Example Resin (R-6) and Comparative Example Compound (R-7). Raw materials:
[0445] [Chemistry 49]
[0446]
[0447] [Synthesis Example 15]
[0448] Synthesis of Comparative Example Resin (R-6)
[0449] [Chemistry 50]
[0450]
[0451] In a nitrogen atmosphere, 90.1 g of raw material (A-9), 9.7 g of resin raw material (B-8), and 270 g of 2-methoxy-1-propanol were added. After a uniform solution was prepared at a liquid temperature of 80°C, 18 g of a 20% p-toluenesulfonic acid solution in 2-methoxy-1-propanol was slowly added, and the mixture was stirred at a liquid temperature of 110°C for 8 hours. After cooling to room temperature, 600 g of methyl isobutyl ketone was added, and the organic layer was washed 5 times with 200 g of pure water, and then dried under reduced pressure. 320 g of THF was added to the residue, and the polymer was reprecipitated with 1,350 g of hexane. The precipitated polymer was separated by filtration and dried under reduced pressure to obtain the comparative example resin (R-6).
[0452] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, and the following results were obtained.
[0453] (R-6): Mw=3,460, Mw / Mn=4.60
[0454] [Synthesis Example 16]
[0455] Synthesis of Compound (R-7) for Comparative Example
[0456] [Chemistry 51]
[0457]
[0458] In a nitrogen atmosphere, 15.4 g of the raw material (A-10), 13.6 g of the raw material (A-11), 1.0 g of the raw material (A-12) and 60 g of 2-methoxy-1-propanol were stirred at an internal temperature of 100°C to prepare a uniform solution, and then 1.00 g of benzyltriethylammonium chloride was added and stirred at an internal temperature of 110°C for 12 hours. After cooling to room temperature, 200 ml of methyl isobutyl ketone was added, and the mixture was washed twice with 100 g of a 1 wt% ammonia aqueous solution, twice with 100 g of a 3% nitric acid aqueous solution, and five times with 100 g of ultrapure water. The organic layer was dried under reduced pressure to obtain a comparative example compound (R-7).
[0459] The weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, and the following results were obtained.
[0460] (R-7): Mw=910, Mw / Mn=1.03
[0461] [Table 4]
[0462] (A) Resin M Mw / Mn X-1 6,000 3.61 X-2 7,400 3.51 X-3 8,000 3.60 X-4 6,500 3.10 X-5 5,900 2.43 X-6 7,000 2.68 X-7 6,600 2.83 X-8 7,200 3.41 X-9 7,100 3.35 R-1 8,500 2.50 R-2 10,000 2.55 R-3 10,000 2.60 R-4 3,300 3.50 R-5 9,400 3.59 R-6 3,460 4.60 R-7 910 1.03
[0463] [Preparation of Resist Underlayer Film-Forming Compositions (UL-1 to 10, Comparative Examples UL-1 to 8)]
[0464] Resins (X-1) to (X-9), (R-1) to (R-7), base generators (C-1) to (C-4), crosslinking agent (D-1), and fluidity promoter (E-1) were dissolved in an organic solvent containing 0.1 mass% FC-4430 (3M Corporation product, refined by our company) in the proportions shown in Table 6, and filtered with a 0.1 μm fluororesin filter to prepare a composition for forming an anti-etching agent underlayer film (UL-1 to 10, comparison examples UL-1 to 8).
[0465] [(C) Base Generator]
[0466] The base generators (C-1 to C-4) used in the resist underlayer film forming composition are shown below.
[0467] [Chemistry 52]
[0468]
[0469] [(D) Cross-linking agent]
[0470] The cross-linking agent (D-1) used in the resist underlayer film forming composition is shown below.
[0471] [Chemistry 53]
[0472]
[0473] [(E) Flowability enhancer]
[0474] The fluidity improving agent (E-1) used in the resist underlayer film forming composition is shown in Table 5 below.
[0475] [Table 5]
[0476]
[0477] [Table 6]
[0478]
[0479]
[0480] [Evaluation of Solvent Resistance and Film Thickness Uniformity (Examples 1-1 to 1-10, Comparative Examples 1-1 to 1-8)]
[0481] The above-prepared resist lower film forming composition (UL-1 to 10, comparative examples UL-1 to 8) was coated on a silicon substrate, and after being fired at each baking temperature for 60 seconds, the film thickness from the center to the periphery of the substrate was measured, and the average film thickness (a [nm]) was calculated. Then, PGMEA solvent was dispensed on it, left for 30 seconds and spun dry, and baked at 100°C for 60 seconds to evaporate PGMEA, and the film thickness (b [nm]) was measured. The difference in film thickness before and after PGMEA treatment was calculated (residual film rate: (b / a) × 100).
[0482] In addition, the film thickness from the center to the periphery of the substrate was measured for the resist underlayer film fired under each condition, and the film thickness difference between the maximum film thickness and the minimum film thickness relative to the average film thickness (a) was less than 5%, and it was rated as "good", and it was rated as "poor" when it was 5% or more. Furthermore, the film forming properties of the produced resist underlayer film were observed under an optical microscope, and it was rated as "good" when there were no defects such as cracks and wrinkles, and it was rated as "poor" when cracks and wrinkles were observed.
[0483] The results are shown in Table 7.
[0484] [Table 7]
[0485]
[0486]
[0487] As shown in Table 7, Examples 1-1 to 1-10 using the resist underlayer film-forming compositions UL-1-1 to 1-10 used in the pattern forming method of the present invention showed good film-forming properties and film thickness uniformity when forming a thick film. In addition, the residual film rate ((b / a)×100) after the PGMEA rinsing treatment was 99% or more, indicating that a crosslinking reaction occurred and sufficient solvent resistance was exhibited.
[0488] On the other hand, when using Comparison Examples 1-1, 1-4, and 1-6 in which the content of groups modified with phenolic hydroxyl groups is outside the scope of the present invention, Comparison Example UL-1, Comparison Example UL-4, and Comparison Example UL-6, it is possible that the viscosity of the resin is high and the fluidity during spin coating is insufficient, and deterioration in film thickness uniformity is observed.
[0489] In Comparative Examples 1-7 of Comparative Example UL-7 using the comparative example resin (R-6) having a rigid cardo structure and Comparative Examples 1-8 of Comparative Example UL-8 using the comparative example compound (R-7) containing a monomolecular compound, cracks were observed on the surface of the resist underlayer film after the substrate was fired. In addition, the presence of cracks confirmed the degradation of the film thickness uniformity. It can be said that when forming a thick film of 3 μm or more, it is preferable to use a resin containing either a novolac type phenol unit or a novolac type naphthol unit.
[0490] [Etching resistance (Examples 2-1 to 2-10, Comparative Examples 2-1 to 2-7)]
[0491] The above-mentioned resist underlayer film-forming compositions (UL-1 to 10 and comparative examples UL-1 to 6) with good solvent resistance evaluation were coated on a silicon substrate and fired at 250°C for 60 seconds using a hot plate to form a resist underlayer film, and the film thickness a was measured. Comparative Example A comparative example KrF photoresist material was coated on a silicon substrate and fired at 100°C for 60 seconds using a hot plate to form a resist upper layer film, and the film thickness a was measured.
[0492] For the comparative example KrF photoresist material (KrF single-layer resist), a polymer represented by a KrF single-layer resist polymer (KRP1), acid generators (PAG2 and PAG3), and a basic compound (Amine2) are dissolved in a solvent containing 0.1 mass % of a surfactant FC-4430 (manufactured by Sumitomo 3M Co., Ltd.) according to the proportions shown in Table 8, and the mixture is filtered through a 0.1 μm fluororesin filter to prepare the solution.
[0493] [Table 8]
[0494]
[0495] Single-layer resist polymer for KrF (KRP1)
[0496] Mw = 15,000, Mw / Mn = 1.98
[0497] [Chemistry 54]
[0498]
[0499] PAG2 (acid generator): 10-(4-butoxyphenyl)diphenylsulfonium camphorsulfonate
[0500] PAG3 (acid generator): bis(cyclohexylsulfonyl)diazomethane
[0501] Amine2 (basic compound): tris(2-methoxyethyl)amine
[0502] Next, etching was performed using CF4 gas under the following conditions using an etching device Telius manufactured by Tokyo Electron, and the film thickness b was measured. From the film thickness etched during the specified time using CF4 gas (film thickness a-film thickness b), the film thickness etched in 1 minute was calculated and defined as the etching rate A (nm / min). When the etching rate A was below 75nm / min, it was rated as "A" (good), when it exceeded 75nm / min and was below 80nm / min, it was rated as "B" (slightly good), and when it exceeded 80nm / min, it was rated as "C" (poor). The results are shown in Table 9.
[0503] The etching conditions are as follows.
[0504] Dry etching conditions of CF4 gas
[0505] Chamber pressure: 50mT
[0506] RF power (upper): 500W
[0507] RF power (lower): 300W
[0508] CF4 gas flow rate: 150sccm
[0509] CHF3 gas flow rate: 50sccm
[0510] Time: 30 seconds
[0511] [Table 9]
[0512]
[0513]
[0514] As shown in Table 9, Examples 2-1 to 2-10 using the resist underlayer film forming compositions UL-1-1 to 1-10 used in the pattern forming method of the present invention showed excellent dry etching resistance compared with Comparative Example 2-7 using a single-layer resist for KrF. However, Comparative Examples UL-1 to 3 and Comparative Example UL-6 using styrene-based resins different from the resist underlayer film forming compositions used in the pattern forming method of the present invention showed unsatisfactory dry etching resistance.
[0515] [Landfilling Characteristics (Examples 3-1 to 3-10, Comparative Examples 3-1 to 3-6)]
[0516] The resist underlayer film forming compositions (UL-1 to 10 and comparative examples UL-1 to 6) used for the above solvent resistance evaluation were applied on a Figure 2 The SiO2 wafer substrate 7 having a dense hole pattern (hole diameter 0.45 μm, hole depth 11.0 μm, distance between the centers of two adjacent holes 1.00 μm) as shown in (M) (plan view) and (N) (cross-sectional view) is fired at the temperature described in Table 7 for 60 seconds to form a mold as shown in Figure 2The resist underlayer film 8 shown in (O). The cross-sectional shape of each wafer substrate obtained was observed using a scanning electron microscope (SEM) to confirm whether there was no void inside the hole and whether the pattern side wall and the interface between the resist underlayer film material were not peeled off but filled with the resist underlayer film. The results are shown in Table 10. When a resist underlayer film forming composition with poor filling characteristics was used, voids occurred inside the hole in this evaluation. Furthermore, when a resist underlayer film forming composition with poor adhesion was used, peeling occurred at the interface between the pattern side wall or the substrate and the resist underlayer film material in this evaluation. When a resist underlayer film forming composition with good filling characteristics and adhesion was used, in this evaluation, Figure 2 As shown in (O), the inside of the hole is filled with the resist underlayer film without voids or peeling.
[0517] [Table 10]
[0518]
[0519] As shown in Table 10, Examples 3-1 to 3-10 using the resist underlayer film forming compositions UL-1 to 10 used in the pattern forming method of the present invention can fill the hole pattern without voids and peeling, and it is found that the filling property and adhesion are excellent.
[0520] On the other hand, in Comparative Examples 3-1, 3-4, and 3-6 using Comparative Examples UL-1, UL-4, and UL-6, the resin contained a large amount of hydroxyl groups and had insufficient fluidity, so voids were probably generated due to poor filling.
[0521] In Comparative Examples 3-2, 3-3, and 3-5 using Comparative Examples UL-2, UL-3, and UL-5, although voids did not occur, peeling due to insufficient adhesion was observed. This is believed to be due to insufficient hydroxyl groups in the resin.
[0522] [Pattern Formation Method (Examples 4-1 to 4-10, Comparative Examples 4-1 to 4-4)]
[0523] The above-mentioned resist lower film forming composition (UL-1 to 10 and comparative examples UL-1 to 3) was coated on a SiO2 substrate treated with HMDS (90°C x 60 seconds), and fired at 250°C for 60 seconds in the atmosphere to form a resist lower film with a film thickness of 3,000 nm. A resist intermediate film material (SOG-1) containing silicon atoms was coated thereon, and baked at 220°C for 60 seconds to form a resist intermediate film with a film thickness of 45 nm. A single-layer resist for ArF of a resist upper film material was coated thereon, and baked at 105°C for 60 seconds to form a photoresist film with a film thickness of 100 nm.
[0524] The silicon-containing anti-etching intermediate film material (SOG-1) is prepared by dissolving a polymer represented by an ArF silicon-containing intermediate film polymer (SiP1) and a thermal cross-linking catalyst (CAT1) in an organic solvent containing 0.1 mass % FC-4430 (produced by Sumitomo 3M Co., Ltd.) in the proportions shown in Table 11, and filtering with a fluororesin filter with a pore size of 0.1 μm to prepare the silicon-containing anti-etching intermediate film material (SOG-1).
[0525] [Table 11]
[0526]
[0527] The structural formulas of the ArF silicon-containing intermediate film polymer (SiP1) and the thermal crosslinking catalyst (CAT1) used are shown below.
[0528] [Chemistry 55]
[0529]
[0530] As an anti-etching agent upper layer film material (single-layer anti-etching agent for ArF), a polymer (RP1), an acid generator (PAG1), and a basic compound (Amine1) are dissolved in a solvent containing 0.1 mass % of a surfactant FC-4430 (manufactured by Sumitomo 3M Co., Ltd.) according to the proportions shown in Table 12, and the mixture is filtered through a 0.1 μm fluororesin filter to prepare the material.
[0531] [Table 12]
[0532]
[0533] The polymer (RP1), the acid generator (PAG1), and the basic compound (Amine1) used for the resist upper layer film material (single-layer resist for ArF) are shown below.
[0534] [Chemistry 56]
[0535]
[0536] Next, the film was exposed with an ArF immersion exposure device (manufactured by Nikon Co., Ltd.; NSR-S610C, NA0.85, σ0.75, conventional type, 6% half-step phase shift mask), baked at 100°C for 60 seconds (PEB), and developed with a 2.38% by mass tetramethylammonium hydroxide (TMAH) aqueous solution to obtain a 0.5 μm and 1:5 positive line and space pattern (resist pattern).
[0537] Next, using an etching apparatus Telius manufactured by Tokyo Electron, the resist pattern was used as a mask to etch the resist intermediate film by dry etching to form a resist intermediate film pattern, the obtained resist intermediate film pattern was used as a mask to etch the resist lower film to form a resist lower film pattern, and the obtained resist lower film pattern was used as a mask to perform etching on the SiO2 film. The etching conditions are as follows.
[0538] Transfer conditions of the resist pattern to the resist intermediate film.
[0539] Chamber pressure: 80mT
[0540] RF power (upper): 500W
[0541] RF power (lower): 300W
[0542] CF4 gas flow rate: 150sccm
[0543] CHF3 gas flow rate: 50sccm
[0544] Time: 35 seconds
[0545] Transfer conditions of the resist intermediate film pattern to the resist underlayer film.
[0546] Chamber pressure: 80mT
[0547] RF power (upper): 500W
[0548] RF power (lower): 300W
[0549] CO2 gas flow rate: 320sccm
[0550] N2 gas flow rate: 80sccm
[0551] Time: 900 sec
[0552] Transfer conditions of resist underlayer film pattern to SiO2 film.
[0553] Chamber pressure: 10mT
[0554] RF power (upper): 100W
[0555] RF power (lower): 800W
[0556] CF4 gas flow rate: 25sccm
[0557] CHF3 gas flow rate: 15sccm
[0558] O2 gas flow rate: 5sccm
[0559] Time: 900 sec
[0560] As comparative example 4-4, a comparative example KrF photoresist material (KrF single-layer resist) was coated on a SiO2 substrate on which a BARC (DUV-42 / 61nm) film had been formed, and fired at 130°C for 90 seconds in the atmosphere to form a resist film with a thickness of 3,000nm. Then, it was exposed with a KrF exposure device (manufactured by NIKON; NSR-S203B (NA=0.55, σ0.75, conventional type, binary mask)), baked at 100°C for 60 seconds (PEB), and developed with a 2.38% by mass tetramethylammonium hydroxide (TMAH) aqueous solution to obtain a 0.5μm and 1:5 positive line and space pattern (resist pattern).
[0561] The comparative example uses a KrF photoresist material (single-layer resist for KrF), and the same method as described above is used.
[0562] Next, the SiO2 film was etched by dry etching using a Telius etching apparatus manufactured by Tokyo Electron Corporation, using the resist pattern as a mask. The etching conditions were as follows.
[0563] Transfer conditions of resist pattern to SiO2 film.
[0564] Chamber pressure: 10mT
[0565] RF power (upper): 100W
[0566] RF power (lower): 800W
[0567] CF4 gas flow rate: 25sccm
[0568] CHF3 gas flow rate: 15sccm
[0569] O2 gas flow rate: 5sccm
[0570] Time: 900 sec
[0571] Table 13 shows the results of observing the pattern cross section using an electron microscope (S-4700) manufactured by Hitachi, Ltd.
[0572] [Table 13]
[0573]
[0574]
[0575] As shown in Table 13, it can be seen that Examples 4-1 to 4-1 using the resist underlayer film-forming compositions UL-1 to 10 used in the pattern forming method of the present invention all transfer the resist upper layer film pattern to the processed substrate well.
[0576] On the other hand, in Comparative Examples 4-1 to 4-3 using Comparative Examples UL-1 to 3 and Comparative Example 4-4 using a single-layer resist for KrF, the pattern transferred to the processed substrate was confirmed to be tapered. This is presumably because the dry etching resistance evaluation showed insufficient resistance to dry etching using CF4 / CHF3 gas.
[0577] The above evaluation is conducted to compare the pattern transfer performance of the mask material used for processing the processed substrate to the processed substrate. It can be seen that the pattern forming method of the present invention (Examples 4-1 to 4-10) has excellent pattern transfer performance to the processed substrate. In other words, it can be said that it has sufficient resistance to complex etching processes such as the formation of step-shaped patterns on the processed substrate represented by 3D-NAND memory, which repeats the etching of the processed substrate and the trimming of the mask material.
[0578] [Pattern Formation Method (Examples 5-1 to 5-10, Comparative Examples 5-1 to 5-3)]
[0579] The compositions for forming thick film-forming resist underlayer films (TUL-1 to 10 and comparative examples TUL-1 to 3) prepared as shown in Table 14 were coated on SiO2 substrates treated with HMDS (90°C x 60 seconds) and fired at 250°C for 60 seconds in the atmosphere to form resist underlayer films with a film thickness of 10,000 nm. A resist intermediate film material (SOG-2) containing silicon atoms was coated thereon and baked at 220°C for 60 seconds to form a resist intermediate film with a film thickness of 150 nm. A single-layer resist for ArF of a resist upper film material was coated thereon and baked at 105°C for 60 seconds to form a photoresist film with a film thickness of 200 nm.
[0580] [Table 14]
[0581]
[0582] As for the anti-etching intermediate film material (SOG-2) containing silicon atoms, the polymer represented by the ArF silicon-containing intermediate film polymer (SiP1) and the thermal cross-linking catalyst (CAT1) are dissolved in an organic solvent containing 0.1 mass% FC-4430 (produced by Sumitomo 3M Co., Ltd.) in the proportions shown in Table 15, and filtered with a fluororesin filter with a pore size of 0.1μm to prepare the anti-etching intermediate film material (SOG-2) containing silicon atoms.
[0583] [Table 15]
[0584]
[0585] The ArF silicon-containing intermediate film polymer (SiP1) and thermal cross-linking catalyst (CAT1) used are the same as described above.
[0586] As for the resist upper layer film material (single-layer resist for ArF), a polymer (RP1), an acid generator (PAG1), and a basic compound (Amine1) are dissolved in a solvent containing 0.1 mass % of a surfactant FC-4430 (manufactured by Sumitomo 3M Co., Ltd.) according to the proportions shown in Table 16, and the mixture is filtered through a 0.1 μm fluororesin filter to prepare the material.
[0587] [Table 16]
[0588]
[0589] The polymer (RP1), acid generator (PAG1), and basic compound (Amine1) used in the resist upper layer film material (single-layer resist for ArF) are the same as described above.
[0590] Next, the film was exposed using an ArF immersion exposure device (manufactured by Nikon Co., Ltd.; NSR-S610C, NA0.85, σ0.75, conventional type, 6% half-step phase shift mask), baked at 100°C for 60 seconds (PEB), and developed with a 2.38% by mass tetramethylammonium hydroxide (TMAH) aqueous solution to obtain a positive spacing and line pattern (resist pattern) of 5 μm and 1:1.
[0591] Next, using a Tokyo Electron etching apparatus Telius, dry etching was performed to etch the resist intermediate film using the resist pattern as a mask to form a resist intermediate film pattern, the resist lower film was etched using the obtained resist intermediate film pattern as a mask to form a resist lower film pattern, and the SiO2 film was etched using the obtained resist lower film pattern as a mask. The etching conditions are as follows.
[0592] Transfer conditions of the resist pattern to the resist intermediate film.
[0593] Chamber pressure: 80mT
[0594] RF power (upper): 500W
[0595] RF power (lower): 300W
[0596] CF4 gas flow rate: 150sccm
[0597] CHF3 gas flow rate: 50sccm
[0598] Time: 70 seconds
[0599] Transfer conditions of the resist intermediate film pattern to the resist underlayer film.
[0600] Chamber pressure: 80mT
[0601] RF power (upper): 500W
[0602] RF power (lower): 300W
[0603] CO2 gas flow rate: 320sccm
[0604] N2 gas flow rate: 80sccm
[0605] Time: 2,100 seconds
[0606] Transfer conditions of resist underlayer film pattern to SiO2 film.
[0607] Chamber pressure: 10mT
[0608] RF power (upper): 100W
[0609] RF power (lower): 800W
[0610] CF4 gas flow rate: 25sccm
[0611] CHF3 gas flow rate: 15sccm
[0612] O2 gas flow rate: 5sccm
[0613] Time: 900 sec
[0614] The pattern cross section was observed using an electron microscope (S-4700) manufactured by Hitachi, Ltd. The results are shown in Table 17.
[0615] [Table 17]
[0616]
[0617]
[0618] As shown in Table 17, in Examples 5-1 to 5-10 using the resist underlayer film forming compositions TUL-1 to 10 for thick film formation used in the pattern forming method of the present invention, the resist upper layer film patterns were all well transferred to the processed substrate. In addition, it was confirmed that there was no abnormality such as peeling at the interface between the resist underlayer film and the substrate.
[0619] On the other hand, in Comparative Examples 5-1 to 5-3 using Comparative Examples TUL-1 to 3, it was confirmed that the shape of the resist underlayer film pattern was tapered. The reason is presumed to be insufficient resistance to dry etching using CF4 / CHF3 gas in the above dry etching resistance evaluation. In addition, it was confirmed that in Comparative Examples 5-2 to 5-3, the resist underlayer film pattern peeled off from the substrate interface. It is presumed that this is due to insufficient hydroxyl content in the resin.
[0620] As shown in the above results, the pattern forming method of the present invention is a method that uses a resist underlayer film forming composition that can form a thick film that takes into account both high-level filling characteristics and substrate adhesion. Compared with the pattern forming method using a single layer of KrF photoresist material, it shows better resist pattern transfer performance, so it can provide an ideal pattern forming method when forming a step-shaped pattern on a processed substrate represented by a 3D-NAND memory.
[0621] This specification includes the following aspects.
[0622] [1]: A pattern forming method is a method for forming a pattern on a processed substrate, characterized by:
[0623] The following steps are involved:
[0624] (I-1) after applying a resist underlayer film forming composition on a substrate to be processed, forming a resist underlayer film by heat treatment,
[0625] (I-2) forming a silicon-containing resist intermediate film on the resist underlayer film,
[0626] (I-3) forming a resist upper layer film on the aforementioned silicon-containing resist intermediate film using a photoresist material,
[0627] (I-4) after pattern exposure of the resist upper layer film, developing with a developer to form a pattern on the resist upper layer film,
[0628] (I-5) using the patterned resist upper layer film as a mask, dry etching is performed to transfer a pattern to the silicon-containing resist intermediate film,
[0629] (I-6) using the silicon-containing resist intermediate film to which the pattern has been transferred as a mask, dry etching is performed to transfer the pattern to the resist lower layer film,
[0630] (I-7) using the resist underlayer film to which the pattern has been transferred as a mask, processing the substrate to be processed to form a pattern on the substrate to be processed,
[0631] (I-8) trimming the resist underlayer film to which the pattern has been transferred,
[0632] (I-9) using the trimmed resist underlayer film pattern as a mask, processing the substrate to be processed to form a step-shaped pattern on the substrate to be processed,
[0633] The resist underlayer film-forming composition comprises (A) a resin and (B) an organic solvent.
[0634] The resin (A) is a resin having a structural unit represented by the following general formula (1), and when the ratio of the phenolic hydroxyl groups contained in the resin (A) is a and the ratio of the groups modified by the phenolic hydroxyl groups is b, the following relations are satisfied: a+b=1, 0.1≤a≤0.5, 0.5≤b≤0.9:
[0635] [Chemistry 57]
[0636]
[0637] In the general formula (1), R 01 is a saturated or unsaturated monovalent organic group having 1 to 30 carbon atoms which may be substituted, R 02 is a hydrogen atom or a saturated or unsaturated monovalent organic group having 1 to 30 carbon atoms which may be substituted, X is a divalent organic group having 1 to 30 carbon atoms, and p is 0 or 1. When p is 0, m2 is an integer of 0 to 3, n2 is an integer of 1 to 4, and m2+n2 is an integer of 1 to 4. When p is 1, m2 is an integer of 0 to 5, n2 is an integer of 1 to 6, and m2+n2 is an integer of 1 to 6.
[0638] [2]: A pattern forming method as described in [1], wherein the steps (I-8) to (I-9) are repeated to form a plurality of step-shaped patterns on the processed substrate.
[0639] [3]: A pattern forming method as in [1] or [2], wherein, for the substrate to be processed, a multilayer film in which polysilicon layers are stacked, or a multilayer film in which SiN layers and SiO layers are alternately stacked is used.
[0640] [4]: A pattern forming method as in [1] or [2], wherein, for the substrate to be processed, a multilayer film in which polysilicon layers and SiO layers are alternately stacked, or a multilayer film in which SiN layers and SiO layers are alternately stacked is used.
[0641] [5]: The pattern forming method according to any one of [1] to [4], wherein the resist underlayer film has a thickness of at least 3 μm.
[0642] [6]: In the pattern forming method of [5], in the step (I-1), the resist underlayer film is applied to a thickness of at least 3 μm in a single coating.
[0643] [7]: The pattern forming method according to any one of [1] to [6], wherein the resin (A) has a weight average molecular weight of 3,000 to 20,000.
[0644] [8]: The pattern forming method according to any one of [1] to [7], wherein the resist underlayer film forming composition contains (C) a base generator.
[0645] [9]: The pattern forming method according to [8], wherein the base generator (C) is any of the following general formulae (2), (3) and (4):
[0646] [Chemistry 58]
[0647]
[0648] In the formula, R 1 ~R 3 Each independently represents a linear, branched or cyclic alkyl group having 1 to 10 carbon atoms or an alkenyl group having 2 to 10 carbon atoms, which may be substituted by a heteroatom or have an intervening heteroatom, or an aryl group having 6 to 18 carbon atoms or an aralkyl group having 7 to 18 carbon atoms, which may be substituted by a heteroatom or have an intervening heteroatom. 1 , R 2 and R 3 Any two of X may also be bonded to each other and form a ring together with the sulfur atom in the formula. - represents an organic or inorganic anion that is a counter ion. - OH not included - . R 4 and R 5 Each independently represents an aryl group having 6 to 20 carbon atoms which may be substituted with or interposed with a hetero atom, and a part or all of the hydrogen atoms thereof may be substituted with a linear, branched or cyclic alkyl or alkoxy group having 1 to 10 carbon atoms. 4 and R 5 They may also bond to each other and to form a ring together with the iodine atom in the formula. 6 , R 7 , R 8 and R 9 Each independently represents a hydrogen atom, or a linear, branched, or cyclic alkyl group having 1 to 20 carbon atoms or an alkenyl group having 2 to 20 carbon atoms, which may be substituted by a heteroatom or have an intervening heteroatom, or an aryl group having 6 to 18 carbon atoms or an aralkyl group having 7 to 18 carbon atoms, which may be substituted by a heteroatom or have an intervening heteroatom. 6 , R 7 , R 8 and R 9 Any two or more of the may be bonded to each other and form a ring together with the nitrogen atom in the formula.
[0649]
[10] : The pattern forming method according to [9], wherein X in the general formulae (2), (3) and (4) is - For example, any anion selected from the group consisting of a structure represented by any one of the following general formulae (5), (6) and (7), and chloride ion, bromide ion, iodide ion, fluoride ion, cyanide ion, nitrate ion, and nitrite ion is used.
[0650] [Chemistry 59]
[0651]
[0652] In the formula, R 10 It represents a linear, branched, or cyclic alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms, which may contain one or more selected from an ether group, an ester group, and a carbonyl group, and some or all of the hydrogen atoms in these groups may be substituted with one or more selected from a halogen atom, a hydroxyl group, a carboxyl group, an amino group, and a cyano group. 11 R represents an aryl group having 6 to 20 carbon atoms, wherein a part or all of the hydrogen atoms of the aryl group may be substituted with one or more selected from a halogen atom, a hydroxyl group, a carboxyl group, an amino group, and a cyano group. 12 , R 13 , and R 14 Each independently represents a hydrogen atom, a halogen atom other than a fluorine atom, or a linear, branched, or cyclic alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms, which may contain one or more selected from an ether group, an ester group, and a carbonyl group, and a part or all of the hydrogen atoms in these groups may be substituted by one or more selected from a halogen atom, a hydroxyl group, a carboxyl group, an amino group, and a cyano group. 12 , R 13 , and R 14 Two or more of them may be bonded to each other to form a ring.
[0653]
[11] : The pattern forming method according to any one of [1] to
[10] , wherein in the general formula (1), R 02 is any of a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, and a structure represented by the following general formula (8),
[0654] [Chemistry 60]
[0655]
[0656] In the general formula (8), * represents the bonding site to the oxygen atom, R A is a divalent organic group having 1 to 10 carbon atoms which may be substituted, RB It is a hydrogen atom or an optionally substituted monovalent organic group having 1 to 10 carbon atoms.
[0657]
[12] : A pattern forming method as described in any one of [1] to
[11] , wherein the resist underlayer film forming composition further comprises one or more selected from (D) a cross-linking agent, (E) a fluidity promoter and (F) a surfactant.
[0658]
[13] : A pattern forming method as described in any one of [1] to
[12] , wherein, in the method for forming a circuit pattern on the upper film of the resist, optical lithography with a wavelength of 5 nm to 300 nm, direct drawing using an electron beam, nanoimprinting, or a combination thereof is used.
[0659]
[14] : The pattern forming method according to any one of [1] to
[13] , wherein as the developing method, alkali development or organic solvent development is used.
[0660]
[15] : A pattern forming method as described in any one of [1] to
[14] , wherein, as the substrate to be processed, a structure or a height difference substrate having an aspect ratio of 5 or more is used.
[0661] The present invention is not limited to the above-mentioned embodiments. The above-mentioned embodiments are illustrative only, and any device having substantially the same configuration and exhibiting the same function and effect as the technical concept described in the claims of the present invention is included in the technical scope of the present invention.
[0662] Description of Reference Numerals
[0663] 1: Processed substrate (nitride film)
[0664] 1a: Pattern (pattern formed on the processed substrate 1)
[0665] 1b: Pattern (pattern formed on pattern 1a)
[0666] 2: Processed layer (oxide film)
[0667] 2a: Pattern (pattern formed on the processed layer 2)
[0668] 2b: Pattern (pattern formed on pattern 2a)
[0669] 3: Resist lower layer film
[0670] 3a: Resist lower film pattern
[0671] 3b: Resist underlayer film pattern (pattern formed on the resist underlayer film pattern 3a)
[0672] 4: Silicon-containing resist interlayer
[0673] 4a: Silicon-containing resist interlayer pattern
[0674] 5: Resist upper film
[0675] 5a: Resist upper film pattern
[0676] 6: Exposure part
[0677] 7: SiO2 wafer substrate with dense hole pattern
[0678] 8: Resist lower layer film
Claims
1. A pattern forming method is a method for forming a pattern on a processed substrate, characterized by: The following steps are involved: (I-1) after applying a resist underlayer film forming composition on a substrate to be processed, forming a resist underlayer film by heat treatment, (I-2) forming a silicon-containing resist intermediate film on the resist underlayer film, (I-3) forming a resist upper layer film on the silicon-containing resist intermediate film using a photoresist material, (I-4) after pattern exposure of the resist upper layer film, developing with a developer to form a pattern on the resist upper layer film, (I-5) using the patterned resist upper layer film as a mask to dry-etch and transfer the pattern to the silicon-containing resist intermediate film, (I-6) using the silicon-containing resist intermediate film having the transferred pattern as a mask, dry etching is performed to transfer the pattern to the resist lower layer film, (I-7) using the resist underlayer film to which the pattern has been transferred as a mask, processing the substrate to be processed to form a pattern on the substrate to be processed, (I-8) trimming the resist underlayer film of the transferred pattern, (I-9) using the trimmed resist underlayer film pattern as a mask, processing the substrate to be processed to form a step-shaped pattern on the substrate to be processed, The resist underlayer film-forming composition comprises (A) a resin and (B) an organic solvent. The resin (A) is a resin having a structural unit represented by the following general formula (1), and when the ratio of the phenolic hydroxyl groups contained in the resin (A) is a and the ratio of the groups modified by the phenolic hydroxyl groups is b, the following relations are satisfied: a+b=1, 0.1≤a≤0.5, 0.5≤b≤0.
9. In the general formula (1), R 01 is a saturated or unsaturated monovalent organic group having 1 to 30 carbon atoms which may be substituted, R 02 is a hydrogen atom or a saturated or unsaturated monovalent organic group having 1 to 30 carbon atoms which may be substituted, X is a divalent organic group having 1 to 30 carbon atoms, p is 0 or 1, when p is 0, m2 is an integer of 0 to 3, n2 is an integer of 1 to 4, m2+n2 is an integer of 1 to 4, when p is 1, m2 is an integer of 0 to 5, n2 is an integer of 1 to 6, and m2+n2 is an integer of 1 to 6.
2. The pattern forming method according to claim 1, wherein: The steps (I-8) to (I-9) are repeated to form a plurality of step-shaped patterns on the substrate to be processed.
3. The pattern forming method according to claim 1, wherein: For the substrate to be processed, a multilayer film in which polysilicon layers are stacked, or a multilayer film in which SiN layers and SiO layers are alternately stacked is used.
4. The pattern forming method according to claim 1, wherein: For the substrate to be processed, a multilayer film in which polysilicon layers and SiO layers are alternately stacked, or a multilayer film in which SiN layers and SiO layers are alternately stacked is used.
5. The pattern forming method according to claim 1, wherein: The resist underlayer film is formed to have a thickness of at least 3 μm.
6. The pattern forming method according to claim 5, wherein: In the step (I-1), the resist underlayer film is applied to a thickness of at least 3 μm by one coating.
7. The pattern forming method according to claim 1, wherein: The resin (A) has a weight average molecular weight of 3,000 to 20,000.
8. The pattern forming method according to claim 1, wherein: The resist underlayer film forming composition contains (C) a base generator.
9. The pattern forming method according to claim 8, wherein: As the base generator (C), any of the following general formulas (2), (3) and (4) can be used: In the formula, R 1 ~R 3 Each independently represents a linear, branched or cyclic alkyl group having 1 to 10 carbon atoms or an alkenyl group having 2 to 10 carbon atoms, which may be substituted by a heteroatom or have an intervening heteroatom, or an aryl group having 6 to 18 carbon atoms or an aralkyl group having 7 to 18 carbon atoms, which may be substituted by a heteroatom or have an intervening heteroatom, and R 1 , R 2 and R 3 Any two of X may also be bonded to each other and form a ring together with the sulfur atom in the formula. - represents an organic or inorganic anion that is a counter ion, but X - OH not included - , R 4 and R 5 Each independently represents an aryl group having 6 to 20 carbon atoms which may be substituted with or inserted with a heteroatom, and a part or all of the hydrogen atoms thereof may be substituted with a linear, branched or cyclic alkyl or alkoxy group having 1 to 10 carbon atoms, and R 4 and R 5 They can also bond with each other and form a ring with the iodine atom in the formula. 6 , R 7 , R 8 and R 9 each independently represents a hydrogen atom, or a linear, branched, or cyclic alkyl group having 1 to 20 carbon atoms or an alkenyl group having 2 to 20 carbon atoms, which may be substituted by a heteroatom or have an intervening heteroatom, or an aryl group having 6 to 18 carbon atoms or an aralkyl group having 7 to 18 carbon atoms, which may be substituted by a heteroatom or have an intervening heteroatom, and R 6 , R 7 , R 8 and R 9 Any two or more of the may be bonded to each other and form a ring together with the nitrogen atom in the formula.
10. The pattern forming method according to claim 9, wherein: In the general formulas (2), (3) and (4), X - For example, any anion selected from the group consisting of a structure represented by any one of the following general formulae (5), (6) and (7), and chloride ion, bromide ion, iodide ion, fluoride ion, cyanide ion, nitrate ion, and nitrite ion is used. In the formula, R 10 represents a linear, branched, or cyclic alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms, which may contain at least one selected from an ether group, an ester group, and a carbonyl group, and some or all of the hydrogen atoms in these groups may be substituted with at least one selected from a halogen atom, a hydroxyl group, a carboxyl group, an amino group, and a cyano group, R 11 represents an aryl group having 6 to 20 carbon atoms, wherein a part or all of the hydrogen atoms of the aryl group may be substituted by one or more selected from halogen atoms, hydroxyl groups, carboxyl groups, amino groups, and cyano groups, and R 12 , R 13 , and R 14 Each independently represents a hydrogen atom, a halogen atom other than a fluorine atom, or a linear, branched, or cyclic alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms, which may contain one or more selected from an ether group, an ester group, and a carbonyl group, and a part or all of the hydrogen atoms in these groups may be substituted by one or more selected from a halogen atom, a hydroxyl group, a carboxyl group, an amino group, and a cyano group. In addition, R 12 , R 13 , and R 14 Two or more of them may be bonded to each other to form a ring.
11. The pattern forming method according to claim 1, wherein: In the general formula (1), the R 02 is any of a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, and a structure represented by the following general formula (8), In the general formula (8), * represents the bonding site to the oxygen atom, R A is a divalent organic group having 1 to 10 carbon atoms which may be substituted, R B It is a hydrogen atom or an optionally substituted monovalent organic group having 1 to 10 carbon atoms.
12. The pattern forming method according to claim 1, wherein: The resist underlayer film-forming composition further contains one or more selected from the group consisting of (D) a crosslinking agent, (E) a fluidity promoter, and (F) a surfactant.
13. The pattern forming method according to claim 1, wherein: The method of forming a circuit pattern on the resist upper layer film uses optical lithography with a wavelength of 5 nm to 300 nm, direct drawing using an electron beam, nanoimprinting, or a combination thereof.
14. The pattern forming method according to claim 1, wherein: As for the developing method, alkali development or organic solvent development is used.
15. The pattern forming method according to any one of claims 1 to 14, wherein: As the substrate to be processed, a substrate having a structure with an aspect ratio of 5 or more or a height difference is used.