Preparation and application of copper-nitrogen-doped porous carbon

Through ultrasonic treatment and heat treatment technology of copper-nitrogen doped porous carbon, copper-nitrogen doped porous carbon is formed, which solves the problems of poor conductivity and insufficient nitrogen doping in the existing technology, and significantly improves the electrochemical performance and energy of the supercapacitor. density.

CN119092312AActive Publication Date: 2024-12-06QUANGANG PETROCHEM RES INST OF FUJIAN NORMAL UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411191988.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-06
Estimated Expiration
2044-08-28

AI Technical Summary

Technical Problem

The existing porous carbon electrode materials have poor electrical conductivity, are prone to falling off with copper doping, and the nitrogen-doped nitrogen content is not high, resulting in insufficient increase in electrochemical stability and energy density of supercapacitors.

Method used

Copper and excess concentrated ammonia water are used to form cupric ions, which are uniformly adhered to the surface of porous carbon by ultrasonic treatment, and heat treatment is carried out in an inert atmosphere to form copper-nitrogen-doped porous carbon, improving its conductivity and energy density.

Benefits of technology

It improves the conductivity and electrochemical stability of copper-nitrogen-doped porous carbon, enhances its energy density and power density in supercapacitors, and is suitable for power substations and electric vehicle batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092312A_ABST
    Figure CN119092312A_ABST
Patent Text Reader

Abstract

The invention discloses preparation and application of copper and nitrogen doped porous carbon. The preparation method of the nitrogen-doped porous carbon comprises the following steps: 1) dissolving a copper source into excessive concentrated ammonia water, then adding porous carbon, and carrying out ultrasonic treatment to obtain a suspension; 2) drying the suspension to obtain powder, transferring the powder into a tubular furnace, and carrying out heat treatment in an inert atmosphere; and 3) washing and drying the product to obtain the copper-nitrogen doped porous carbon. According to the invention, copper ions and a nitrogen-containing ligand have strong complexing ability to generate a stable copper ammonia complex, then the copper ammonia complex is uniformly attached to the surface of the porous carbon through adsorption in an ultrasonic environment, and finally copper and nitrogen are doped to the surface of the porous carbon through heat treatment. The copper-nitrogen-doped porous carbon prepared by the method is excellent in energy density and power density, and is an ideal supercapacitor electrode material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of copper-nitrogen doped porous carbon electrodes, and in particular relates to the preparation and application of copper-nitrogen doped porous carbon. Background Art

[0002] Supercapacitors are a new type of energy storage device between traditional capacitors and batteries, with the advantages of fast charging and discharging speed, long cycle life, and high energy density. Among them, the electrode material is the key factor affecting the electrochemical performance of supercapacitors. Porous carbon is widely used as the electrode material of supercapacitors due to its large specific surface area, good chemical stability, and low cost. However, porous carbon electrode materials have the problem of poor conductivity, which limits the performance improvement of supercapacitors.

[0003] Copper doping in 3d transition metals is a feasible method. Copper has good electrical conductivity, and doping it to the surface of porous carbon can improve its conductivity. The existing technology generally uses a single copper load to the surface of porous carbon to improve its conductivity, or nitrogen doping porous carbon to improve its conductivity and energy density. However, copper loaded on the surface of porous carbon is easy to fall off during the charge and discharge process, resulting in poor electrochemical stability, and nitrogen-doped porous carbon often has a low nitrogen content due to process reasons, and the conductivity improvement is not obvious enough. Therefore, there is an urgent need for a copper-nitrogen doped porous carbon to improve the conductivity and energy density of the electrode. Summary of the invention

[0004] In view of the defects of the prior art, the present invention aims to provide a preparation method and application of copper-nitrogen doped porous carbon.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions: A method for preparing copper-nitrogen doped porous carbon comprises the following steps: (1) Dissolving the copper source in excess concentrated ammonia water to generate copper-ammonia complex ions, then adding porous carbon, placing it in an ultrasonic reactor, and ultrasonically treating it to obtain a suspension; (2) drying the suspension to obtain a powder, transferring the powder to a tube furnace, and subjecting the powder to a heat treatment in an inert atmosphere at a temperature of 400 to 600° C. for a time of 30 to 120 min to obtain a product; (3) The above product is washed with water and dried to obtain copper-nitrogen doped porous carbon.

[0006] In step (1), the copper source is one or both of cupric chloride and cuprous chloride.

[0007] In step (1), the mass ratio of the copper source to the porous carbon is 1:1-1:9, preferably 1:3-1:6. Within this ratio range, the copper ammine complex ions can be more evenly dispersed on the surface of the porous carbon.

[0008] In step (1), the ultrasonic treatment time is 5 to 30 minutes.

[0009] In step (2), the inert atmosphere is one of argon or nitrogen.

[0010] In step (2), the heat treatment heating rate is 5-10°C / min.

[0011] In step (3), the product is washed 1 to 3 times with deionized water and then dried at 60 to 105°C.

[0012] In step (3), the specific surface area of ​​the prepared copper-nitrogen doped porous carbon is 800-3000m 2 / g.

[0013] Furthermore, the heat treatment temperature in step (2) is 400-500° C. Within this temperature range, the effect of the heat treatment on the porous carbon pore structure is lower.

[0014] The application of the copper-nitrogen doped porous carbon in supercapacitors: the copper-nitrogen doped porous carbon is used as an electrode material to assemble into a supercapacitor.

[0015] The invention generates a stable copper-ammine complex by using the strong complexing ability of copper ions and nitrogen-containing ligands, and then uniformly attaches the copper-ammine complex to the surface of porous carbon by adsorption in an ultrasonic environment, and finally dopes the copper-nitrogen complex to the surface of the porous carbon by heat treatment.

[0016] The present invention has the following beneficial effects 1. Copper is used to react with excess concentrated ammonia to generate copper-ammine complex ions. Copper has a very strong complexing ability for nitrogen-containing ligands and can produce stable Cu-N coordination centers, such as Cu-N2 and Cu-N4. This can not only improve the conductivity of porous carbon and is beneficial to electrochemical stability, but also help to dope nitrogen into the carbon skeleton, thereby enhancing the active sites of porous carbon and further improving its conductivity and energy density.

[0017] 2. When copper-nitrogen doped porous carbon is used as supercapacitor electrode material, it has excellent electrochemical properties. The production process of this technology is simple and easy to industrialize, and can bring good economic benefits.

[0018] 3. Compared with the prior art, the copper-nitrogen doped porous carbon prepared by the present invention has excellent energy density and power density, and is an ideal supercapacitor electrode material, and has good application prospects in power substations, electric vehicle batteries, and other fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 Schematic diagram of the synthesis of copper-nitrogen-doped porous carbon prepared in Example 1.

[0020] Figure 2 Elemental analysis and Raman spectra of the copper-nitrogen doped porous carbon prepared in Example 1. (a) is the full XPS spectrum of the copper-nitrogen doped porous carbon; (b) is the Cu 2p 3 / 2 Figure; (c) is the N1s image of copper-nitrogen doped porous carbon; (d) is the Raman spectrum of copper-nitrogen doped porous carbon.

[0021] Figure 3 This is the constant current charge and discharge curve of the copper-nitrogen doped porous carbon prepared in Example 1. DETAILED DESCRIPTION

[0022] The present invention is further described in detail below in conjunction with specific examples. These examples are implemented based on the technical solution of the present invention, and provide detailed implementation methods and specific operation processes, but the protection scope of the present invention is not limited to these examples.

[0023] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs. Example 1

[0024] A method for preparing copper-nitrogen doped porous carbon comprises the following steps: (1) Copper chloride and porous carbon are weighed in a mass ratio of 1:4, firstly the copper chloride is dissolved in excess concentrated ammonia water, then the porous carbon is added, and then placed in an ultrasonic reactor for ultrasonic treatment for 10 minutes to obtain a suspension; (2) drying the suspension to obtain a powder, and then placing the powder in a tube furnace for heat treatment. The heat treatment process is an argon atmosphere, heating to 500°C at a rate of 5°C / min, and heating for 30 min to obtain a product; (3) After the tube furnace was naturally cooled to room temperature, the product was taken out, washed with deionized water three times, and then vacuum dried at 60 °C for 12 h to obtain copper-nitrogen doped porous carbon.

[0025] The specific surface area of ​​the copper-nitrogen doped porous carbon prepared in this example is 2500 m 2 / g. The copper-nitrogen doped porous carbon was assembled as an electrode on a supercapacitor electrode, and a mass specific capacity of 1350F / g was obtained at a current density of 0.5A / g, and the capacity retention rate was 90% after 10,000 cycles.

[0026] Figure 2 Elemental analysis and Raman spectrum of the copper-nitrogen doped porous carbon prepared in Example 1. Figure 2 (a) It can be seen that the appearance of Cu and N characteristic peaks indicates the presence of Cu and N elements in the prepared copper-nitrogen doped porous carbon; Figure 2(b) is for Cu2p 3 / 2 Peak fitting results of the Cu 2p peaks at 932.90 eV and 934.42 eV 3 / 2 The photoelectron peaks correspond to Cu + and Cu 2 + , 952.61 eV and 954.17 eV binding energies are Cu + and Cu 2+ Cu 2p 1 / 2 Photoelectron peak; Figure 2 As can be seen in (c), the characteristic peak at 399.10 eV corresponds to pyridine N, the characteristic peak at 400.37 eV corresponds to pyrrole N, the peak at 401.74 eV corresponds to quaternary amine N, and the peak at 402.80 eV corresponds to pyridine N oxide; Figure 2 (d) is the Raman spectrum of CuN-doped porous carbon at 1358 cm -1 and 1582 cm -1 There are two characteristic peaks nearby, corresponding to the D peak and G peak of carbon materials, which can reflect the structural disorder, defect degree and graphitization degree of carbon materials.

[0027] Figure 3 This is the constant current charge-discharge curve of the copper-nitrogen doped porous carbon prepared in Example 1. From the figure, the first discharge specific capacitance of the copper-nitrogen doped porous carbon at different current densities can be obtained. The results show that the specific capacitance is 1350, 1040.5, 925.9, 888.9, 852.3, 808.1 and 766.3 F / g at current densities of 0.5, 1, 2, 4, 6, 8 and 10 A / g, respectively. Example 2

[0028] A method for preparing copper-nitrogen doped porous carbon comprises the following steps: (1) Copper chloride and porous carbon are weighed in a mass ratio of 1:2, firstly the copper chloride is dissolved in excess concentrated ammonia water, then the porous carbon is added, and then placed in an ultrasonic reactor for ultrasonic treatment for 10 minutes to obtain a suspension; (2) drying the suspension to obtain a powder, and then placing the powder in a tube furnace for heat treatment. The heat treatment process is an argon atmosphere, heating to 400°C at a rate of 5°C / min, and heating for 30 min to obtain a product; (3) After the tube furnace was naturally cooled to room temperature, the product was taken out and washed with deionized water three times, and then vacuum dried at 60 °C for 12 h to obtain copper-nitrogen doped porous carbon.

[0029] The specific surface area of ​​the copper-nitrogen doped porous carbon prepared in this example is 1500 m 2 / g. The copper-nitrogen doped porous carbon was assembled as an electrode on a supercapacitor electrode, and a mass specific capacity of 950F / g was obtained at a current density of 0.5A / g, and the capacity retention rate was 92% after 10,000 cycles. Example 3

[0030] A method for preparing copper-nitrogen doped porous carbon comprises the following steps: (1) Copper chloride and porous carbon are weighed in a mass ratio of 1:1, firstly the copper chloride is dissolved in excess concentrated ammonia water, then the porous carbon is added, and then placed in an ultrasonic reactor for ultrasonic treatment for 10 minutes to obtain a suspension; (2) drying the suspension to obtain a powder, and then placing the powder in a tube furnace for heat treatment. The heat treatment process is an argon atmosphere, heating to 600°C at a rate of 5°C / min, and heating for 30 min to obtain a product; (3) After the tube furnace was naturally cooled to room temperature, the product was taken out, washed with deionized water three times, and then vacuum dried at 60 °C for 12 h to obtain copper-nitrogen doped porous carbon.

[0031] The specific surface area of ​​the copper-nitrogen doped porous carbon prepared in this example is 1200 m 2 / g, and assembled the copper-nitrogen doped porous carbon as an electrode onto the supercapacitor electrode. A mass specific capacity of 430 F / g was obtained at a current density of 0.5 A / g, and the capacity retention rate was 95% after 10,000 cycles.

Claims

1. A method for preparing copper-nitrogen doped porous carbon, characterized in that: The following steps are involved: (1) Dissolving the copper source in excess concentrated ammonia water, then adding porous carbon, placing it in an ultrasonic reactor, and ultrasonically treating it to obtain a suspension; (2) drying the suspension to obtain a powder, transferring the powder to a tube furnace, and subjecting the powder to a heat treatment in an inert atmosphere at a temperature of 400 to 600° C. for a time of 30 to 120 min to obtain a product; (3) The above product is washed with water and dried to obtain copper-nitrogen doped porous carbon.

2. The method for preparing copper-nitrogen doped porous carbon according to claim 1, characterized in that: In step (1), the copper source is one or both of cupric chloride and cuprous chloride.

3. The method for preparing copper-nitrogen doped porous carbon according to claim 1, characterized in that: The specific surface area of ​​the copper-nitrogen doped porous carbon is 800-3000 m 2 / g.

4. The method for preparing copper-nitrogen doped porous carbon according to claim 1, characterized in that: In step (1), the mass ratio of the copper source to the porous carbon is 1:1 to 1:

9.

5. The method for preparing copper-nitrogen doped porous carbon according to claim 1, characterized in that: In step (1), the ultrasonic treatment time is 5 to 30 minutes.

6. The method for preparing copper-nitrogen doped porous carbon according to claim 1, characterized in that: In step (2), the inert atmosphere is one of argon or nitrogen.

7. The method for preparing copper-nitrogen doped porous carbon according to claim 1, characterized in that: In step (2), the heat treatment heating rate is 5-10°C / min.

8. The method for preparing copper-nitrogen doped porous carbon according to claim 1, characterized in that: In step (3), the product is washed 1 to 3 times with deionized water and then dried at 60 to 105°C.

9. The copper-nitrogen doped porous carbon obtained according to the preparation method according to any one of claims 1 to 8.

10. Use of the copper-nitrogen doped porous carbon as claimed in claim 9 in a supercapacitor.

Citation Information

Patent Citations

  • Method for preparing copper-doped activated carbon by utilizing complexing process

    CN103803545A

  • Copper-nitrogen co-doped carbon nanotube catalyst and preparation method and application thereof

    CN108187713A

  • Hierarchical porous carbon material used for flexible supercapacitor and production method thereof

    CN109850866A

  • Preparation method and application of waste wet tissue derived nitrogen-oxygen-sulfur co-doped flexible carbon cloth