Modified metal zinc negative electrode material and preparation method and application thereof
By using zinc hydroxide plating in zinc ion batteries, the problems of zinc dendrites and side reactions are solved, the stability of zinc negative electrodes and the cycle life of the battery are improved, and more efficient electrochemical performance is achieved.
Patent Information
- Application Number
- CN202411197229.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-06
AI Technical Summary
The growth and side reactions of zinc dendrites (such as corrosion, passivation and hydrogen evolution) in the charge and discharge process of metal zinc anode in aqueous zinc ion batteries lead to poor cell circulation performance and low Coulomb efficiency, which seriously restricts its commercialization process.
Zinc hydroxide (ZnOHF) plating is used to form a zinc matrix surface. The zinc hydroxide plating is formed by heating in a hydrofluoric acid solution to adjust the nucleation and deposition process of zinc ions to inhibit side reactions and corrosion of electrolyte.
It improves the interface stability and cycle stability of zinc negative electrode, reduces dendrites' growth, extends the cycle life of the battery, and improves the efficiency of the Coulomb.
Smart Images

Figure CN119092669A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a zinc metal battery, and in particular to a modified metal zinc negative electrode material and a preparation method and application thereof. Background Art
[0002] At present, people are paying more and more attention to the safety of electric vehicles and energy storage devices. The toxicity of organic electrolytes and the fire caused by short circuits in traditional lithium-ion batteries are safety issues. There is an urgent need to develop a safe, non-toxic, and low-cost secondary battery system. Aqueous zinc-ion batteries have high safety and high theoretical discharge capacity (820 mAh g -1 ) has attracted widespread attention. However, the practical application of aqueous zinc-ion batteries is still restricted by many problems, the most serious of which is the growth of zinc dendrites and side reactions (such as corrosion, passivation and hydrogen evolution) during the charge and discharge process of the metal zinc anode, which leads to poor battery cycle performance and low coulombic efficiency, seriously restricting the commercialization of aqueous zinc-ion batteries. Due to the lack of sufficient nucleation sites for zinc ions in repeated deposition / dissolution cycles, under the influence of the "tip advantage", zinc ions are continuously and unevenly deposited to form dendrites, resulting in irreversible "dead zinc". In addition, due to the side effects of the interface, there are chemical corrosion and hydrogen evolution side reactions between the electrolyte and the zinc anode. The zinc anode undergoes electrochemical corrosion in the aqueous electrolyte to produce a series of byproducts such as Zn4SO4(OH)6·xH2O. The continuous generation of insulating byproducts on the surface of the zinc anode continuously consumes electrolyte and active zinc ions, increases interfacial resistance, hinders the transmission of zinc ions, and reduces the reversibility of the zinc anode. In addition, the zinc anode has a low redox potential (-0.76V vs. SHE) and will inevitably spontaneously produce hydrogen in the aqueous battery system, thereby increasing the internal pressure of the sealed battery and accelerating the generation of byproducts due to the increased alkalinity of the electrolyte. These behaviors destroy the surface structure of the zinc anode, causing irreversible consumption of active materials, leading to short cycle life and low Coulombic efficiency in zinc-ion batteries. Improving the interfacial stability of the zinc anode is considered to be an important way to improve the performance of zinc-ion batteries. Suitable surface modification materials should have the following properties: 1) hydrophilicity and stability in aqueous electrolytes; 2) high ionic conductivity; 3) sufficient mechanical strength; 4) physical barriers to inhibit side reactions.
[0003] CN115241408A discloses a method for preparing a zinc negative electrode material, a modified zinc negative electrode and a zinc battery. The method comprises: step 1, dispersing graphite fluoride in a solvent to obtain a dispersion of graphite fluoride, the concentration of which is 0.01-2 mg / mL, and the concentration can ensure that the graphite fluoride is fully and evenly dispersed. Too much solvent will cause a porous structure to appear during the drying process; step 2, uniformly coating the surface of the zinc negative electrode material with the dispersion of graphite fluoride, the coating amount of which is 5-50 ul / cm 2, remove the solvent to obtain a modified zinc negative electrode material. CN117577766A discloses a method for preparing a zinc negative electrode protective coating for an aqueous zinc ion battery, using a metal zinc negative electrode as a base, and using sulfonated polyaniline and acrylic resin to uniformly mix in ethanol to prepare a protective coating with both conductive and anti-corrosion functions. Both are beneficial attempts in the field. Summary of the invention
[0004] The purpose of the present invention is to provide a modified metal zinc negative electrode material and a preparation method and application thereof, so as to solve the problems of dendrites, hydrogen evolution, high interface impedance and side reactions existing in the zinc negative electrode of the existing zinc metal battery, thereby affecting the electrochemical performance of the zinc metal battery.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is as follows: In a first aspect, the present invention provides a modified metal zinc negative electrode material, comprising a zinc substrate and a zinc fluoride hydroxide coating coated on the surface of the zinc substrate.
[0006] In a second aspect, the present invention provides a method for preparing a modified metal zinc negative electrode material, the method comprising: placing a zinc substrate to be treated above a hydrofluoric acid solution, heating the hydrofluoric acid solution and keeping it warm for a preset time, the hydrofluoric acid gas generated by the volatilization of the hydrofluoric acid solution reacts with the surface of the zinc substrate to form a zinc fluoride and hydroxide coating, thereby obtaining a modified metal zinc negative electrode material.
[0007] Furthermore, the concentration of the hydrofluoric acid solution is 0.1-0.3M.
[0008] Furthermore, placing the zinc substrate to be treated above the hydrofluoric acid solution, heating the hydrofluoric acid solution and keeping it warm for a preset time specifically includes: placing the hydrofluoric acid solution in a reaction container, fixing the zinc substrate to be treated by a clamp and arranging it above the hydrofluoric acid solution in the reaction container; placing the reaction container in a heating box, setting the heating temperature and the preset insulation time, and heating the hydrofluoric acid solution and keeping it warm for a preset time.
[0009] Furthermore, the heating temperature of the heating box is set to 145-155° C., and the preset insulation time is set to 30-60 minutes.
[0010] Furthermore, after the preset insulation time, when the temperature of the heating box is naturally cooled to 40° C., the reaction container is taken out, and then the zinc substrate to be treated in the reaction container is taken out.
[0011] Furthermore, the reaction container is a reactor including a polytetrafluoroethylene container, and the zinc substrate to be treated and the hydrofluoric acid solution are placed in the polytetrafluoroethylene container.
[0012] Furthermore, after the hydrofluoric acid gas generated by the volatilization of the hydrofluoric acid solution reacts with the surface of the zinc substrate to form a fluoride zinc hydroxide coating, the modified metal zinc negative electrode material is cleaned and dried with a washing solvent to remove the residual hydrofluoric acid on the modified metal zinc negative electrode material.
[0013] Furthermore, the zinc substrate to be treated is a zinc sheet, and the plane where the zinc sheet is located is arranged parallel to the liquid surface of the hydrofluoric acid solution.
[0014] In a third aspect, the present invention provides a method for preparing the modified metal zinc negative electrode material as described above and an application of the modified metal zinc negative electrode material in an aqueous zinc ion battery.
[0015] The present invention has the following unexpected beneficial effects: 1. The modified metal zinc negative electrode material of the present invention comprises a zinc substrate and a zinc fluoride hydroxide coating layer coated on the surface of the zinc substrate. 2+ ions have a strong adsorption effect, and the Zn 2+ The lateral diffusion and aggregation of ions along the surface can make Zn 2+ The uniform distribution of ions produces various fine-sized nucleation sites. In addition, due to the adsorption of Zn near the ZnOHF modified layer 2+ Ions require additional energy when they transfer laterally, which forces them to deposit near the initial nucleation site rather than move to other favorable growth sites. In addition, the fluorinated zinc hydroxide coating can also prevent coordinated water molecules and oxygen in the electrolyte from directly contacting the electrode surface, thereby inhibiting water decomposition and the generation of byproduct Zn4SO4(OH)6·xH2O, thereby solving the problem of dendrites, high interface impedance and side reactions in the zinc negative electrode of existing zinc metal batteries, which affects the electrochemical performance of zinc metal batteries.
[0016] 2. The present invention adopts a thermal volatilization method to form a modified coating on the surface of the zinc substrate to be treated, that is, by placing the zinc substrate to be treated above a hydrofluoric acid solution, heating the hydrofluoric acid solution and keeping it warm for a preset time, and the hydrofluoric acid gas generated by the hydrofluoric acid solution being heated and volatilized reacts with the surface of the zinc substrate to form a fluoride zinc hydroxide coating. The preparation process is simple and easy, the preparation yield is high, and the prepared fluoride zinc hydroxide coating particles are uniform. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only some embodiments of the present invention.
[0018] Figure 1The surface microscopic morphology of the modified metal zinc negative electrode material prepared in Example 1 of the present invention is shown.
[0019] Figure 2 The XRD diagram of the modified metal zinc negative electrode material prepared in Example 1 of the present invention is shown.
[0020] Figure 3 The symmetric zinc battery assembled from the prepared modified metal zinc negative electrode material has a current density of 10 mA cm -2 and area capacity of 0.5 mAh cm -2 Voltage-time cycle diagram for .
[0021] Figure 4 The symmetric battery assembled from unmodified metal zinc anode material has a current density of 10 mA cm -2 and area capacity of 0.5 mAh cm -2 Voltage-time cycle diagram for .
[0022] Figure 5 The surface microscopic morphology of the modified metal zinc negative electrode material prepared in Example 2 of the present invention is shown.
[0023] Figure 6 The zinc symmetric battery assembled from the modified metal zinc negative electrode material prepared in Example 2 of the present invention has a current density of 10 mA·cm -2 and area capacity of 0.5 mAh cm -2 Voltage-time cycle diagram for .
[0024] Figure 7 The surface microscopic morphology of the modified metal zinc negative electrode material prepared in Example 3 of the present invention is shown.
[0025] Figure 8 The zinc symmetric battery assembled with the modified metal zinc negative electrode material prepared in Example 3 of the present invention has a current density of 10 mA·cm -2 and area capacity of 0.5 mAh cm -2 Voltage-time cycle diagram for . DETAILED DESCRIPTION
[0026] The following will describe the embodiments of the present invention with reference to the accompanying drawings and preferred embodiments. Those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be understood that the preferred embodiments are only for illustrating the present invention, not for limiting the scope of protection of the present invention.
[0027] In one embodiment, the present invention provides a modified metal zinc negative electrode material, comprising a zinc substrate and a zinc hydroxide fluoride (ZnOHF) coating on the surface of the zinc substrate. 2+ ions have a strong adsorption effect, and the Zn 2+ The lateral diffusion and aggregation of ions along the surface can make Zn 2+ The uniform distribution of ions produces various fine-sized nucleation sites. In addition, due to the adsorption of Zn near the ZnOHF modified layer 2+ Ions require additional energy when they transfer laterally, which forces them to deposit near the initial nucleation site rather than move to other favorable growth sites. In addition, the fluorinated zinc hydroxide coating can also prevent coordinated water molecules and oxygen in the electrolyte from directly contacting the electrode surface, thereby inhibiting water decomposition and the generation of byproduct Zn4SO4(OH)6·xH2O, thereby solving the problem of dendrites, high interface impedance and side reactions in the zinc negative electrode of existing zinc metal batteries, which affects the electrochemical performance of zinc metal batteries.
[0028] In one embodiment, the present invention provides a method for preparing a modified metal zinc negative electrode material, the method comprising: placing a zinc substrate to be treated above a hydrofluoric acid solution, heating the hydrofluoric acid solution and keeping it warm for a preset time, and the hydrofluoric acid gas generated by the hydrofluoric acid solution being heated and volatilized reacts with the surface of the zinc substrate to form a fluoride zinc hydroxide coating, thereby obtaining a modified metal zinc negative electrode material. The entire preparation process is simple and easy, the preparation yield is high, and the obtained fluoride zinc hydroxide coating particles are uniform.
[0029] The preparation method of this modified metal zinc negative electrode material is an innovative surface treatment technology that aims to form a layer of zinc fluoride hydroxide coating on the surface of the zinc substrate by chemical vapor deposition, thereby improving its electrochemical performance, especially the negative electrode performance in the battery system. The following are the detailed steps of the preparation method: S1, preparation stage: Select a suitable zinc substrate as the starting material and ensure that its surface is clean and free of impurities.
[0030] Prepare hydrofluoric acid solution and adjust its concentration according to experimental requirements.
[0031] A heating device is provided to ensure that the heating temperature of the hydrofluoric acid solution can be accurately controlled.
[0032] S2, heating and heat preservation: Place the zinc substrate in a closed or well-ventilated container above the hydrofluoric acid solution to avoid direct leakage of hydrofluoric acid gas. Heat the hydrofluoric acid solution to gradually volatilize it to produce hydrofluoric acid gas. The heating temperature must be controlled within a safe range to avoid boiling and splashing of the solution or causing danger. Maintain a certain heating temperature and keep it warm for a preset time to ensure that the hydrofluoric acid gas fully contacts the surface of the zinc substrate and undergoes a chemical reaction.
[0033] S3, reaction and coating formation: hydrofluoric acid gas reacts with the surface of the zinc substrate to form a zinc fluoride hydroxide coating. In this step, the reaction time, temperature and hydrofluoric acid concentration are key factors affecting the quality of the coating. As the reaction proceeds, the coating gradually thickens and eventually covers the entire surface of the zinc substrate.
[0034] S4, subsequent treatment: After the reaction is completed, the zinc substrate is taken out of the container and subjected to necessary cleaning and drying treatments to remove residual hydrofluoric acid and other impurities on the surface.
[0035] The performance of the modified metal zinc negative electrode material is tested, including the evaluation of electrochemical performance, corrosion resistance, cycle stability and other indicators.
[0036] The preparation method of the present invention is used to form a fluoride zinc hydroxide coating on the surface of the zinc substrate, which helps to improve the cycle stability and discharge capacity of the zinc negative electrode and reduce dendrite growth and corrosion. Due to the presence of the fluoride zinc hydroxide coating, the surface properties of the zinc negative electrode are changed, reducing the risk of thermal runaway of the battery during the charging and discharging process. And compared with traditional wet coating or physical vapor deposition methods, this method has the advantages of simple process and easy control. Although hydrofluoric acid is corrosive, the amount of hydrofluoric acid used in this method is relatively small, and the impact on the environment can be reduced through reasonable waste liquid treatment.
[0037] However, it should be noted that hydrofluoric acid is a highly corrosive and toxic chemical. Safety operating procedures must be strictly followed during the preparation process to ensure the safety of personnel and equipment. In addition, the process parameters need to be further optimized to obtain the best coating effect.
[0038] In a preferred embodiment, the concentration of the hydrofluoric acid solution is 0.1-0.3M.
[0039] The concentration of hydrofluoric acid of 0.1~0.3M is enough to provide enough hydrofluoric acid molecules to react with the surface of the zinc substrate, but it will not cause the reaction to be too violent and difficult to control due to excessive concentration. The moderate concentration helps to maintain the stability of the reaction rate, making it easier to obtain a uniform and dense coating.
[0040] A lower concentration may result in a slower coating formation and require a longer reaction time, while a higher concentration may induce undesirable side reactions, affecting the purity and uniformity of the coating. Setting the hydrofluoric acid solution concentration to 0.1-0.3M helps form a high-quality zinc fluoride hydroxide coating.
[0041] Although hydrofluoric acid itself is corrosive and toxic, the concentration of 0.1~0.3M is relatively low, which reduces the safety risk during operation. However, it is still necessary to strictly follow the safe operating procedures, ensure that personnel wear appropriate protective equipment, and operate in a well-ventilated environment.
[0042] In a preferred embodiment, placing the zinc substrate to be treated above the hydrofluoric acid solution, heating the hydrofluoric acid solution and keeping it warm for a preset time specifically includes: placing the hydrofluoric acid solution in a reaction container, fixing the zinc substrate to be treated by a clamp and arranging it above the hydrofluoric acid solution in the reaction container; placing the reaction container in a heating box, setting the heating temperature and the preset insulation time, and heating the hydrofluoric acid solution and keeping it warm for a preset time.
[0043] The specific steps include: Prepare the reaction vessel: Select a suitable reaction vessel to ensure that it can withstand the pressure and temperature that may be generated during the heating process. The reaction vessel should be corrosion-resistant to cope with the strong corrosiveness of hydrofluoric acid.
[0044] Place hydrofluoric acid solution: Pour 0.2M (or other optimized concentration) hydrofluoric acid solution into the reaction vessel carefully to avoid splashing. Make sure the liquid level of the hydrofluoric acid solution is below the preset safety line to prevent the liquid from expanding and overflowing during heating.
[0045] Fixing the zinc substrate: Use a special clamp to firmly fix the zinc substrate to be treated. Place the clamp and the zinc substrate together above the hydrofluoric acid solution in the reaction container, ensuring that a certain distance is maintained between the surface of the zinc substrate and the hydrofluoric acid solution so that the hydrofluoric acid gas can fully contact and react.
[0046] Set up a heating box: Place the reaction vessel in a heating box that has temperature control and insulation functions. Set the appropriate heating temperature and insulation preset time according to the experimental requirements. The choice of temperature should take into account factors such as the volatility of hydrofluoric acid, the thermal stability of the zinc matrix, and the reaction rate.
[0047] Heating and heat preservation: Start the heating box and start heating the hydrofluoric acid solution. As the temperature rises, the hydrofluoric acid gradually evaporates to produce gas, which contacts the surface of the zinc substrate during the rising process and reacts chemically to form a fluoride-hydroxide zinc coating.
[0048] After the preset insulation time is over, turn off the heating box and let the reaction container cool naturally to room temperature.
[0049] In a preferred embodiment, the heating temperature of the heating box is set to 145-155°C, and the preset insulation time is set to 30-60 minutes. The selection of this temperature and time range is based on the comprehensive consideration of the volatility of hydrofluoric acid, the thermal stability of the zinc matrix material, and the formation rate of the zinc fluoride and hydroxide coating.
[0050] The heating temperature is set at 145~155℃, which is enough to make the hydrofluoric acid volatilize quickly and produce enough hydrofluoric acid gas to fully react with the surface of the zinc substrate. At the same time, this temperature also takes into account the thermal stability of the zinc substrate material. Within this temperature range, the zinc substrate will not undergo obvious thermal deformation or melting, thus ensuring the uniformity and quality of the coating.
[0051] The preset holding time is set to 30~60min to ensure that the hydrofluoric acid gas has enough time to react chemically with the surface of the zinc substrate. A shorter time may result in incomplete coating formation or insufficient thickness, while a longer time may waste energy and time, or even cause unnecessary side reactions, affecting the uniformity of the coating composition.
[0052] In a preferred embodiment, after the preset insulation time, when the temperature of the heating box is naturally cooled to 40°C, the reaction container is taken out, and then the zinc substrate to be treated in the reaction container is taken out. On the one hand, the safety risk during the removal process can be significantly reduced to protect the operators and equipment. On the other hand, thermal stress can be avoided. The zinc substrate and the reaction container at high temperature may produce thermal stress when suddenly encountering cold air, causing material deformation or cracking of the coating. Natural cooling to a lower temperature before taking it out can help reduce the impact of such thermal stress and protect the integrity and quality of the coating.
[0053] In a preferred embodiment, the reaction container is a reactor including a polytetrafluoroethylene container, and the zinc substrate to be treated and the hydrofluoric acid solution are placed in the polytetrafluoroethylene container. Selecting polytetrafluoroethylene as the material of the reaction container and designing it in the form of a reactor can ensure that a stable, safe and efficient reaction environment is provided during the preparation of the modified metal zinc negative electrode material.
[0054] PTFE is a material with extremely high corrosion resistance, and can resist the erosion of many strong acids, strong bases and organic solvents including hydrofluoric acid. This makes it an ideal choice for handling corrosive substances such as hydrofluoric acid. PTFE also has excellent high temperature resistance and can maintain stable physical and chemical properties at higher temperatures. This ensures that the reactor will not be deformed or damaged by high temperatures during the heating process. The surface of PTFE has extremely low surface energy, making it almost non-adherent to any substance. This feature helps to reduce friction and wear between the zinc substrate and the container wall during the reaction process, protecting the integrity of the coating.
[0055] Design advantages of reactors: Reactors are usually sealed to prevent hydrofluoric acid gas from leaking into the external environment during heating, thus ensuring the safety of operators. And the reactor can withstand a certain pressure to ensure that it will not break or leak due to increased internal pressure during heating and insulation.
[0056] In a preferred embodiment, after the hydrofluoric acid gas generated by the hydrofluoric acid solution is heated and volatilized and reacts with the surface of the zinc substrate to form a zinc fluoride hydroxide coating, the modified metal zinc negative electrode material is cleaned and dried with a washing solvent to remove the residual hydrofluoric acid on the modified metal zinc negative electrode material. This ensures that after the hydrofluoric acid gas reacts with the surface of the zinc substrate to form a zinc fluoride hydroxide coating, the residual hydrofluoric acid can be effectively removed, while protecting the integrity and quality of the coating.
[0057] The selection of washing solvent is a key step in the post-treatment step. In order to effectively remove residual hydrofluoric acid and avoid damage to the zinc fluoride hydroxide coating, it is necessary to select a solvent that can fully react with hydrofluoric acid without adversely affecting the coating. Common choices include water, alkaline solutions or special chemical cleaning agents. Among them, alkaline solutions (such as sodium hydroxide solutions) can neutralize hydrofluoric acid and quickly remove residues. However, when using alkaline solutions, special attention should be paid to the control of concentration and temperature to avoid excessive corrosion of the coating.
[0058] The cleaning steps are as follows: Preliminary cleaning: First, use deionized water or purified water to preliminarily clean the modified metal zinc negative electrode material to remove the floating dust and most of the soluble residues on the surface. This step can be performed by spraying, soaking or rinsing.
[0059] Deep cleaning: After the initial cleaning, deep cleaning is performed using the selected cleaning solvent. If an alkaline solution is used, the concentration should be moderate, and the cleaning time and temperature should be controlled to avoid adverse effects on the coating. The solution can be gently stirred or shaken during the cleaning process to promote the dissolution and shedding of residues.
[0060] Rinsing: After deep cleaning, rinse the modified metal zinc anode material with a large amount of deionized water or purified water to completely remove the residual washing solvent and hydrofluoric acid. This step should be repeated several times until the rinse solution is neutral and clear without impurities.
[0061] Drying: Place the cleaned modified metal zinc negative electrode material in a dry and ventilated place to dry naturally, or use a low-temperature oven to dry it. During the drying process, avoid contact and friction with hard objects to protect the integrity and gloss of the coating.
[0062] In a preferred embodiment, the zinc substrate to be treated is a zinc sheet, and the plane where the zinc sheet is located is arranged parallel to the surface of the hydrofluoric acid solution. This arrangement has the following advantages: Uniformity: When the plane of the zinc sheet is parallel to the surface of the hydrofluoric acid solution, the hydrofluoric acid gas can contact the surface of the zinc sheet more evenly during the volatilization process. This uniform contact helps ensure the uniform distribution of the zinc fluoride hydroxide coating on the surface of the zinc sheet, thereby improving the quality and consistency of the coating.
[0063] Reaction efficiency: Parallel arrangement also helps to improve reaction efficiency. Since the contact area between the hydrofluoric acid gas and the zinc sheet surface is relatively large and uniform, the reaction rate will be faster, thus shortening the formation time of the coating.
[0064] Operability: In actual operation, it is easier to arrange the zinc sheet parallel to the hydrofluoric acid solution. The operator can use a clamp or other fixing device to hang the zinc sheet firmly in the reaction vessel without worrying about the direct contact between the zinc sheet and the solution or the uneven reaction caused by tilting.
[0065] Safety: In addition, the parallel arrangement also helps to improve safety. Since a certain distance is maintained between the zinc sheet and the hydrofluoric acid solution, even if the hydrofluoric acid solution fluctuates during the heating process, it is unlikely to splash onto the zinc sheet, thereby reducing the risk of splashing injuries to operators.
[0066] Implementation details: When implementing this preferred method, it is necessary to ensure that the surface of the zinc sheet is clean and free of impurities so that the hydrofluoric acid gas can fully contact the surface of the zinc sheet and react with it. At the same time, it is necessary to select a suitable fixture and fixing method according to the size and shape of the zinc sheet to ensure that the zinc sheet remains stable and does not shake during the reaction. During the heating and insulation process, the temperature and pressure changes in the heating box should be closely monitored, and the heating parameters should be adjusted as needed to ensure the smooth progress of the reaction.
[0067] In another embodiment, the present invention provides a method for preparing a modified metal zinc negative electrode material as described in any of the above embodiments, and use of the modified metal zinc negative electrode material in an aqueous zinc ion battery.
[0068] The following is an explanation with reference to specific examples.
[0069] Embodiment 1, a method for preparing a modified metal zinc negative electrode material, the method comprising the following steps: 1) Cut the zinc foil into 2.5cm×2.5cm square zinc sheets, and place the cut zinc sheets under a hydraulic press to flatten them for later use.
[0070] 2) Prepare 30 mL of 0.2 M hydrofluoric acid solution in a beaker.
[0071] 3) Transfer 30 mL of 0.2 M hydrofluoric acid solution to the diameter polytetrafluoroethylene liner.
[0072] 4) Stick double-sided tape on the center of a 2.5 cm x 2.5 cm zinc sheet so that it sticks to a 2.5 cm long, 1.5 cm diameter cylindrical polytetrafluoroethylene cylinder.
[0073] 5) Place the zinc sheet and PTFE cylinder assembly into a PTFE liner containing 30 mL of 0.2 M hydrofluoric acid solution and close the lid.
[0074] 6) Place the PTFE liner into the reactor.
[0075] 7) Heat the reactor in a hot box at 150°C for 40 minutes. When the hot box cools to 40°C, take out the reactor and then the zinc sheet.
[0076] 8) The removed zinc sheet is first washed three times with pure water and then washed three times with 98% by volume alcohol to obtain a modified metal zinc negative electrode material with a uniform ZnOHF coating.
[0077] See also Figure 1 , showing the surface micromorphology of the modified metal zinc negative electrode material, it can be seen that the prepared zinc fluoride hydroxide particles are uniform.
[0078] See also Figure 2 , shows the XRD analysis result of the surface coating, which, compared with the standard PDF card of ZnOHF, has obvious characteristic peaks, indicating that the obtained product is ZnOHF.
[0079] The prepared modified metal zinc negative electrode material was used as the positive and negative electrode sheets to assemble a zinc symmetric battery. The obtained zinc symmetric battery was charged at a current density of 10 mA cm -2 and area capacity of 0.5 mAh cm -2 The cycle performance test was carried out under the conditions of Figure 3 , the ZnOHF-modified zinc symmetric battery maintained high reversibility and cycle stability in a cycle of nearly 1800 hours. Figure 4 As shown in , after less than 6 hours, the battery short-circuited due to the violent growth of irregular dendrites under high current density.
[0080] There is a significant difference in the cycling performance of symmetrical batteries assembled with unmodified zinc anode and zinc anode modified with ZnOHF, which is due to the effect of the ZnOHF modification layer. The cycle life of the symmetrical battery assembled with the zinc anode modified with ZnOHF is about 300 times that of the symmetrical battery with the unmodified zinc anode. The short cycle life of the unmodified zinc symmetrical battery may be due to unstable polarization and local short circuit after cycling at high current density for symmetrical batteries in weakly acidic zinc sulfate electrolyte, which accelerates the formation of zinc dendrites. In contrast, the zinc symmetrical battery modified with ZnOHF still exhibits a stable voltage-time cycling curve at high current density. These results further verify that the designed ZnOHF modified protective layer has a fast Zn 2+ Ion diffusion pathways, directing Zn 2+ Uniform ion deposition ensures the stability of zinc deposition / dissolution.
[0081] Embodiment 2 is different from Embodiment 1 in that the concentration of the hydrofluoric acid solution is changed to 0.1 M, which can also achieve the effect of protecting the zinc negative electrode.
[0082] See also Figure 5 , showing the surface microstructure of the modified metal zinc negative electrode material of Example 2, it can be seen that the prepared zinc fluoride hydroxide coating particles are relatively thin.
[0083] See also Figure 6 , shows the performance test results of zinc symmetric battery assembled by using modified metal zinc negative electrode material prepared in Example 2 as positive and negative electrode sheets. The obtained zinc symmetric battery has a current density of 10 mA·cm -2 and area capacity of 0.5 mAh cm -2 The cycle performance test was carried out under the conditions of , and the ZnOHF-modified zinc symmetric battery maintained high reversibility and cycle stability in a cycle of nearly 320 hours.
[0084] Embodiment 3 is different from Embodiment 1 in that the concentration of the hydrofluoric acid solution is changed to 0.3M, which can also achieve the effect of protecting the zinc negative electrode.
[0085] See also Figure 7 , showing the surface microstructure of the modified metal zinc negative electrode material of Example 3, it can be seen that the prepared zinc fluoride hydroxide coating particles are relatively thick.
[0086] See also Figure 8 , shows the performance test results of a zinc symmetric battery assembled by using the modified metal zinc negative electrode material prepared in Example 3 as the positive and negative electrode sheets. The obtained zinc symmetric battery has a current density of 10 mA·cm -2 and area capacity of 0.5 mAh cm -2The cycle performance test was carried out under the conditions of , and the ZnOHF-modified zinc symmetric battery maintained high reversibility and cycle stability for nearly 400 hours of cycling.
[0087] The above embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Any equivalent substitution or change made by a person skilled in the art based on the present invention is within the protection scope of the present invention.
Claims
1. A modified metal zinc negative electrode material, Features: The invention comprises a zinc substrate and a zinc fluoride hydroxide coating covering the surface of the zinc substrate.
2. A method for preparing a modified metal zinc negative electrode material, It is characterized in that include: The zinc substrate to be treated is placed above the hydrofluoric acid solution, the hydrofluoric acid solution is heated and kept warm for a preset time, and the hydrofluoric acid gas generated by the hydrofluoric acid solution being heated and volatilized reacts with the surface of the zinc substrate to form a fluoride zinc hydroxide coating, thereby obtaining the modified metal zinc negative electrode material as claimed in claim 1.
3. The method for preparing the modified metal zinc negative electrode material according to claim 1, Features: The concentration of the hydrofluoric acid solution is 0.1-0.3M.
4. The method for preparing the modified metal zinc negative electrode material according to claim 2, Features: Placing the zinc substrate to be treated above the hydrofluoric acid solution, heating the hydrofluoric acid solution and keeping it warm for a preset time specifically includes: placing the hydrofluoric acid solution in a reaction container, fixing the zinc substrate to be treated by a clamp and arranging it above the hydrofluoric acid solution in the reaction container; The reaction container is placed in a heating box, the heating temperature and the preset insulation time are set, and the hydrofluoric acid solution is heated and kept warm for the preset time.
5. The method for preparing the modified metal zinc negative electrode material according to claim 4, Features: The heating temperature of the heating box is set to 145-155° C., and the preset insulation time is set to 30-60 minutes.
6. The method for preparing the modified metal zinc negative electrode material according to claim 4, Features: After the preset insulation time, when the temperature of the heating box is naturally cooled to 40° C., the reaction container is taken out, and then the zinc substrate to be treated in the reaction container is taken out.
7. The method for preparing the modified metal zinc negative electrode material according to claim 4, Features: The reaction container is a reaction kettle including a polytetrafluoroethylene container, and the zinc substrate to be treated and the hydrofluoric acid solution are placed in the polytetrafluoroethylene container.
8. The method for preparing the modified metal zinc negative electrode material according to claim 2, Features: After the hydrofluoric acid gas generated by the volatilization of the hydrofluoric acid solution reacts with the surface of the zinc substrate to form a fluoride zinc hydroxide coating, the modified metal zinc negative electrode material is cleaned and dried with a washing solvent to remove the residual hydrofluoric acid on the modified metal zinc negative electrode material.
9. The method for preparing the modified metal zinc negative electrode material according to claim 2, Features: The zinc substrate to be treated is a zinc sheet, and the plane where the zinc sheet is located is arranged parallel to the liquid surface of the hydrofluoric acid solution.
10. Use of the modified metal zinc negative electrode material as claimed in claim 1 or the modified metal zinc negative electrode material as claimed in any one of claims 2 to 9 in aqueous zinc ion batteries.
Citation Information
Patent Citations
Preparation method of zinc negative electrode material, modified zinc negative electrode and zinc battery
CN115241408A
Preparation method of zinc negative electrode protective coating for aqueous zinc ion battery
CN117577766A