Battery composite diaphragm and preparation method thereof
By using polymers with lithium sulfonate groups and pore-forming agents to prepare composite separators in lithium batteries, the capacity attenuation problems caused by manganese ion deposition and SEI film destruction in the cycle of LFMP batteries was solved, and the circulation performance of the battery was significantly improved.
Patent Information
- Application Number
- CN202411181003.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-06
AI Technical Summary
LFMP batteries have a problem of accelerated capacity attenuation in the later cycle, mainly due to the deposition of manganese ions on the negative electrode surface and the destruction of SEI film.
A polymer containing lithium sulfonate group is mixed with a pore-forming agent in an organic solvent, and a composite battery separator is prepared through a coating process to supplement lithium ions and adsorb manganese ions to alleviate capacity attenuation.
The adsorption of metal ions and supplementation of lithium ions through the compounds of lithium sulfonate groups significantly delays the attenuation of battery capacity and improves the cycling performance of the battery.
Smart Images

Figure CN119092935A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium ion battery diaphragms, and in particular to a battery composite diaphragm and a preparation method thereof. Background Art
[0002] With the development of society and economic progress, the people have stronger requirements for living environment and quality of life. Green energy has gradually attracted attention, and the lithium battery industry, as an important part of green energy, plays a pivotal role.
[0003] Lithium-ion batteries are composed of a positive electrode, a negative electrode, a separator and an electrolyte. Among them, LiFePO4 (LFP) has been widely used in the field of lithium batteries due to its excellent cycle performance, structural stability, safety and low cost. However, the low operating voltage (3.4V) and energy density (580Wh / kg) of LFP have severely restricted the development of LFP. Compared with LFP, LiFeMnPO4 (LFMP), which also has an olivine structure, has a higher operating voltage (4.1V) and energy density (701Wh / kg), and is a very promising new positive electrode material. However, during the battery charge and discharge cycle, manganese ions dissolved in the positive electrode material of LFMP are deposited on the surface of the negative electrode, and the SEI film (solid electrolyte interface film) is destroyed and regenerated, and a large amount of active lithium is consumed, which leads to the accelerated decay of the battery capacity in the middle and late stages of the cycle. Summary of the invention
[0004] The purpose of the present invention is to provide a battery composite diaphragm and a preparation method thereof, which are used to solve the technical problem in the prior art that the battery capacity of the LFMP battery system decays rapidly in the cycle.
[0005] To achieve the above object, one embodiment of the present invention provides a method for preparing a battery composite separator, comprising the following steps:
[0006] Adding a polymer containing lithium sulfonate salt groups and a pore-forming agent into an organic solvent to prepare a coating liquid;
[0007] Applying the coating liquid to the surface of the base film;
[0008] The coated base film is placed in a coagulation bath and dried to obtain a composite diaphragm.
[0009] In one of the preferred embodiments of the present invention, the polymer includes any one of a polyacrylate lithium sulfonate polymer and a polyvinylidene fluoride lithium sulfonate polymer.
[0010] In one of the preferred embodiments of the present invention, the polymer is at least one of a homopolymer or a copolymer of a polyacrylate lithium sulfonate polymer.
[0011] In one of the preferred embodiments of the present invention, the mass ratio of the polymer to the pore-forming agent is 0.1-5:1.
[0012] In one of the preferred solutions of the present invention, the solid content of the mixed solution formed by adding the polymer and the pore-forming agent into the organic solvent is 2%-50%.
[0013] In one preferred embodiment of the present invention, the pore-forming agent is at least one of polyethylene glycol, terpineol, ammonium carbonate, ammonium bicarbonate and oxalic acid ammonium.
[0014] In one preferred embodiment of the present invention, the organic solvent comprises any one of N-methyl-2-pyrrolidone, dimethylacetamide and acetone.
[0015] In one of the preferred solutions of the present invention, the coating thickness is 0.5 μm-5 μm.
[0016] In one of the preferred solutions of the present invention, the coating thickness is 3 μm.
[0017] In one of the preferred embodiments of the present invention, the coagulation bath comprises water and an organic solvent, and the mass ratio of water to the organic solvent is 1-9:10.
[0018] Based on the preparation method of a battery composite diaphragm disclosed in the present invention, the present invention also discloses a battery composite diaphragm, which is prepared by the above preparation method.
[0019] 1. The battery composite diaphragm and its preparation method of the present invention combine the compound with functional groups capable of supplementing lithium ions and metal ion adsorption with the lithium battery diaphragm through a coating process, which plays a role in supplementing lithium ions and adsorbing manganese ions during battery use, and alleviates the capacity decay, solving the problem of manganese ions dissolving and depositing on the negative electrode surface of LFMP batteries (lithium iron manganese phosphate batteries) during circulation.
[0020] 2. The sulfonic acid functional group can ionize to form negatively charged -SO3 - The group can act as a chelating agent to adsorb metal ions in the solution, and lithium sulfonate can also act as a lithium supplement to replenish the consumption of active lithium caused by the formation of SEI film, etc. Therefore, it is meaningful to synthesize some special compounds that have excellent adsorption properties for metals and can replenish lithium ions by introducing lithium sulfonate groups. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 The present invention is a flowchart of a method for preparing a composite battery separator according to an embodiment of the present invention. DETAILED DESCRIPTION
[0022] In order to make the purpose, technical solution and advantages of the embodiments of the present disclosure clearer, the technical solution in the embodiments of the present disclosure will be clearly and completely described below in conjunction with the drawings in the embodiments of the present disclosure. Obviously, the described embodiments are part of the embodiments of the present disclosure, not all of the embodiments. Based on the embodiments in the present disclosure, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present disclosure.
[0023] The present invention provides a method for preparing a battery composite diaphragm, such as Figure 1 As shown, the following steps are included:
[0024] Step (1): adding a polymer containing lithium sulfonate groups and a pore-forming agent into an organic solvent to prepare a coating liquid;
[0025] Step (2): applying the coating liquid to the surface of the base film;
[0026] Step (3): The coated base film is placed in a coagulation bath and dried to obtain a composite membrane; specifically, the coated base film is immersed in a coagulation bath to coagulate and form pores, taken out, extracted with pure water, and dried after extraction to obtain a composite membrane.
[0027] The battery composite diaphragm and its preparation method of the present invention combine the compound with functional groups capable of supplementing lithium ions and metal ion adsorption with the lithium battery diaphragm through a coating process, which plays a role in supplementing lithium ions and adsorbing manganese ions and alleviating capacity decay during battery use.
[0028] Furthermore, the polymer in step (1) includes any one of polyacrylate lithium sulfonate polymer and polyvinylidene fluoride lithium sulfonate polymer. Preferably, the polymer is at least one of the homopolymer or copolymer of polyacrylate lithium sulfonate polymer. Polymethacrylate and polyvinylidene fluoride polymers refer to polymer main chain substances, which are generally used as coating materials of glue in the diaphragm. The use of the above-mentioned types of polymers can enhance the lithium supplementation and manganese capture effects of the battery composite diaphragm.
[0029] Furthermore, the mass ratio of the polymer to the pore-forming agent is 0.1-5: 1. The mass ratio of the polymer to the pore-forming agent is limited to ensure the performance of the prepared battery composite diaphragm. When the mass ratio of the polymer to the pore-forming agent is too low, the coating of the battery composite diaphragm will be unstable; when the mass ratio of the polymer to the pore-forming agent is too high, the coating has too few pores, the air permeability of the battery composite diaphragm is too large, and the resistance is easily increased.
[0030] Furthermore, the solid content of the mixed solution formed by adding the polymer and the pore-forming agent to the organic solvent is 2%-50%. The solid content of the mixed solution formed by adding the polymer and the pore-forming agent to the organic solvent is limited to ensure the normal subsequent base film coating. When the solid content is too low, the coating thickness will not meet the standard during coating; when the solid content is too high, the viscosity of the coating liquid is too high and it is not easy to coat.
[0031] Furthermore, the pore-forming agent is at least one of polyethylene glycol, terpineol, ammonium carbonate, ammonium bicarbonate and ammonium oxalate. The above-mentioned pore-forming agents are easily dissolved in organic solvents and water, and are easily extracted to form pore structures when passing through a water bath.
[0032] Further, the organic solvent includes any one of N-methyl-2-pyrrolidone (NMP), dimethylacetamide (DMAC) and acetone. The above-mentioned organic solvents are used to ensure the dissolution of the coating material and the pore-forming agent.
[0033] Furthermore, the coagulation bath in step (3) comprises water and an organic solvent, and the mass ratio of water to the organic solvent is 1-9:10, wherein the organic solvent is any one of N-methyl-2-pyrrolidone (NMP), dimethylacetamide (DMAC) and acetone. The gradient coagulation bath can gradually extract the solvent and pore-forming agent in the coating liquid, while the functional material can be retained and gradually form a solid and remain on the base film. The role of selecting a specific ratio is that the gradient extraction can ensure the integrity of the material coating and the integrity of the pores.
[0034] Preferably, the base film in step (2) comprises any one of polypropylene (PP), polyethylene (PE) and PP1 / PE2 / PP1. The coating method is any one of micro-concave transfer, gravure transfer and blade coating. The coating thickness is 0.5 μm-5 μm, and further, the coating thickness is 3 μm. The currently used coating membrane type is selected, and the coating thickness ratio is relatively high.
[0035] The present invention also discloses a battery composite diaphragm, which is prepared by the above-mentioned preparation method. The battery composite diaphragm prepared by the present invention plays a role in replenishing lithium ions and adsorbing manganese ions during the use of the battery, alleviating the capacity decay, and solving the problem of manganese ions dissolved and deposited on the negative electrode surface of the LFMP battery during the cycle.
[0036] Example 1
[0037] The preparation of a polymer containing a lithium sulfonate group comprises the following steps: dissolving p-bromophenol, triethylamine and methacryloyl chloride in dichloromethane, reacting in a single-necked flask to generate p-bromophenol methacrylate; dissolving 2-(2-iodo-tetrafluoroethoxy)tetrafluoroethylsulfonyl lithium salt and p-bromophenol methacrylate in DMSO (dimethyl sulfoxide), adding copper powder, reacting under nitrogen protection at a temperature of 110°C to generate a methacrylate perfluorosulfonic acid lithium salt monomer, and finally generating a methacrylate perfluorosulfonic acid lithium salt polymer (PMMA-PSF-Li) through a polymerization reaction.
[0038] A preparation method for a battery composite diaphragm comprises the following steps: adding PMMA-PSF-Li and a pore-forming agent PEG (polyethylene glycol) to a DMAC solvent at a mass ratio of 1:1, adjusting the proportion so that the solid content of the mixed solution reaches 20%, mechanically stirring for 2 hours, and uniformly dispersing the mixed slurry; uniformly coating the mixed slurry on one side of a 9μm base film by micro-gravure coating, with the coating thickness controlled at 3μm, immersing the coated diaphragm in a coagulation bath formed by mixing 80wt% DMAC and water to coagulate and form pores, taking it out after 1 hour, and finally extracting it with pure water for 5 minutes, and drying the diaphragm at 60°C to remove residual water, so as to obtain a composite coated diaphragm.
[0039] Example 2
[0040] The preparation of a polymer containing lithium sulfonate salt groups comprises the following steps: adding PVDF (polyvinylidene fluoride) to a three-necked flask containing chlorosulfonic acid, and stirring the mixture at 60°C for 45 minutes; cooling the mixture to room temperature and then dropping it into 1,2-dichloroethane to separate the polymer precipitation, and then washing it with 1,2-dichloroethane for two times, and drying to obtain a vinylidene fluoride sulfonic acid polymer (PVDF-S), and then soaking the PVDF-S powder in a 1 mol / L LiOH (lithium hydroxide) aqueous solution at 60°C for 24 hours, separating the polymer and washing it with deionized water until it is neutral, and drying to obtain a vinylidene fluoride sulfonate polymer (PVDF-S-Li).
[0041] A preparation method for a battery composite diaphragm comprises the following steps: adding PVDF-S-Li and pore-forming agent PEG to NMP solvent at a mass ratio of 1:1, adjusting the proportion so that the solid content of the mixed solution reaches 20%, mechanically stirring for 2 hours, and uniformly dispersing the mixed slurry. The mixed slurry is uniformly coated on one side of a 9μm base film by micro-gravure coating, and the coating thickness is controlled to be 3μm. The coated diaphragm is immersed in a coagulation bath formed by mixing 80wt% NMP and water to coagulate and form pores, and is taken out after 1 hour. Finally, after extraction with pure water for 5 minutes, the diaphragm is dried at 60°C to remove the residual water, and a composite coated diaphragm is obtained.
[0042] Comparative Example 1
[0043] A preparation method for a battery composite diaphragm comprises the following steps: adding polyvinylidene fluoride (PVDF) and pore-forming agent PEG to NMP solvent at a mass ratio of 1:1, adjusting the proportion so that the solid content of the mixed solution reaches 20%, mechanically stirring for 2 hours, and uniformly dispersing the mixed slurry. The mixed slurry is uniformly coated on one side of a 9μm base film by micro-gravure coating, and the coating thickness is controlled to be 3μm. The coated diaphragm is immersed in a coagulation bath formed by mixing 80wt% NMP and water to coagulate and form pores, and is taken out after 1 hour. Finally, the diaphragm is extracted with pure water for 5 minutes, and the residual water is dried at 60°C to obtain a composite coated diaphragm.
[0044] Comparative Example 2
[0045] A method for preparing a battery composite diaphragm comprises the following steps: coating a ceramic slurry with a solid content of 35% on one side of a 9μm base film to a coating thickness of 3μm, and curing to obtain a ceramic coated diaphragm.
[0046] Test and Inspection
[0047] The diaphragms prepared in the above examples 1-2 and comparative examples 1-2 were respectively subjected to thickness tests and air permeability tests, and the diaphragms prepared in the above examples 1-2 and comparative examples 1-2 were assembled into 2.4Ah soft-pack battery LFMP batteries, and the four prepared batteries were subjected to room temperature cycle tests (500 cycles, capacity retention rate). The test results are shown in Table 1.
[0048] Table 1: Physical property test results of the diaphragms prepared in Examples 1-2 and Comparative Examples 1-2
[0049]
[0050] It can be seen from Table 1 that the thickness and permeability of the diaphragms prepared in Example 1-2 and Comparative Example 1-2 are not much different. The diaphragm containing lithium sulfonate in Example 1-2 has excellent cycle performance, which is related to the adsorption of manganese ions and the supplementation of lithium ions. After disassembly, the negative electrode before and after the cycle was subjected to ICP test (inductively coupled plasma test). The battery negative electrode with the diaphragm containing lithium sulfonate has the least manganese content, which also shows that the sulfonic acid group has a good adsorption capacity for manganese ions generated during the cycle, inhibiting its precipitation at the negative electrode.
[0051] The embodiments described above are merely descriptions of preferred implementations of the present invention and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary engineering and technical personnel in the field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for preparing a battery composite diaphragm, characterized in that: The following steps are involved: Adding a polymer containing lithium sulfonate salt groups and a pore-forming agent into an organic solvent to prepare a coating liquid; Applying the coating liquid to the surface of the base film; The coated base film is placed in a coagulation bath and dried to obtain a composite diaphragm.
2. The method for preparing a battery composite separator according to claim 1, characterized in that: The polymer includes any one of a polyacrylate lithium sulfonate polymer and a polyvinylidene fluoride lithium sulfonate polymer.
3. The method for preparing a battery composite separator according to claim 2, characterized in that: The polymer is at least one of a homopolymer or a copolymer of a polyacrylate lithium sulfonate polymer.
4. A method for preparing a battery composite separator according to any one of claims 1 to 3, characterized in that: The mass ratio of the polymer to the pore-forming agent is 0.1-5:
1.
5. The method for preparing a battery composite separator according to claim 1, characterized in that: The solid content of the mixed solution formed by adding the polymer and the pore-forming agent into the organic solvent is 2%-50%.
6. The method for preparing a battery composite separator according to claim 1, characterized in that: The pore-forming agent is at least one of polyethylene glycol, terpineol, ammonium carbonate, ammonium bicarbonate and oxalic acid ammonium.
7. The method for preparing a battery composite separator according to claim 1, characterized in that: The organic solvent includes any one of N-methyl-2-pyrrolidone, dimethylacetamide and acetone.
8. The method for preparing a battery composite separator according to claim 1, characterized in that: The coating has a thickness of 0.5 μm to 5 μm.
9. The method for preparing a battery composite separator according to claim 8, characterized in that: The coating thickness was 3 μm.
10. The method for preparing a battery composite separator according to claim 1, characterized in that: The coagulation bath comprises water and an organic solvent, and the mass ratio of the water to the organic solvent is 1-9:
10.
11. A battery composite separator, characterized in that: The preparation method is described in any one of claims 1 to 10.
Citation Information
Patent Citations
Preparation method of interpenetrating network structure P(LiAMPS)-based single-ion transport gel polymer electrolyte film
CN102276860A
Solvent-resistant microporous film, microporous composite film and preparation method and application of microporous composite film
CN106601970A
Isolating layer used for lithium-sulfur battery
CN106935773A
Modified separator, preparation method thereof and lithium ion battery
CN109560238A
Coating composition for lithium battery diaphragm and preparation method thereof
CN111100523A