Metal foil with resin, method for manufacturing printed wiring board and method for manufacturing semiconductor package

By using a resin composition of a liquid reactive group compound and an inorganic filler material at 25°C, the fluidity and volatility of the resin metal foil during heating curing is solved, and the quality of the printed circuit board and semiconductor package is improved. .

CN119095724APending Publication Date: 2024-12-06RESONAC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380036969.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-12-28
Filing Date
2023-12-25
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In the prior art, the resin-containing metal foil is heat-cured due to the volatility of the organic solvent, and it is difficult to obtain sufficient fluidity, which affects the quality of the printed circuit board and the semiconductor package.

Method used

A resin composition containing a compound having a reactive group at 25°C and a molecular weight of 1,000 or less was used to form a resin layer to improve fluidity and inhibit the generation of volatile components.

Benefits of technology

Excellent flowability of the resin layer and suppression of volatile components during heating curing are achieved, and the reliability and performance of printed circuit boards and semiconductor packages are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005105451380000081
    Figure BDA0005105451380000081
  • Figure BDA0005105451380000101
    Figure BDA0005105451380000101
  • Figure BDA0005105451380000102
    Figure BDA0005105451380000102
Patent Text Reader

Abstract

The present invention relates to a metal foil with a resin, a method for manufacturing a printed wiring board using the metal foil with a resin, and a method for manufacturing a semiconductor package, the metal foil with a resin having a metal foil and a resin layer provided on one surface of the metal foil and containing a resin composition, the resin composition containing: (A) a thermosetting resin; (B) a compound that is liquid at 25 DEG C, has a reactive group, and has a molecular weight of 1,000 or less; and (C) an inorganic filler.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present embodiment relates to a metal foil with resin, a method for manufacturing a printed wiring board, and a method for manufacturing a semiconductor package. Background Art

[0002] In recent years, due to the miniaturization and performance improvement of electronic devices, the wiring density and integration have been increasing in the field of printed wiring boards and semiconductor packages.

[0003] In these electronic devices, insulating materials such as thermosetting resins are used as sealing materials for semiconductor chips and substrate materials for printed circuit boards. However, when mounting components, stress caused by the difference in thermal expansion coefficients between the insulating material and the semiconductor chip can sometimes become a problem. The stress generated here can cause warping of the semiconductor package, which is a major cause of reduced reliability.

[0004] Therefore, as a method of making the thermal expansion coefficient of the insulating material close to the thermal expansion coefficient of the semiconductor chip, a method of mixing an inorganic filler into the insulating material has been developed.

[0005] Patent document 1 discloses the following technology with the aim of providing a thermosetting resin composition having low dielectric loss tangent, low thermal expansion, excellent embedding properties and flatness of wiring: a polybutadiene-based elastomer modified with an acid anhydride is added to a thermosetting resin composition containing an inorganic filler and a polyimide compound, wherein the polyimide compound has a structural unit derived from a maleimide resin having at least two N-substituted maleimide groups and a structural unit derived from a diamine compound.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2018-012747 Summary of the invention

[0009] Problems to be solved by the invention

[0010] However, as an insulating material, a metal foil with resin having a resin layer formed using a resin composition on the metal foil is sometimes used. The resin layer of the metal foil with resin is sometimes formed into an insulating layer by curing while embedding a circuit of a circuit substrate, or is used as a sealing material for a semiconductor chip.

[0011] In order to embed the circuit well using the resin layer of the metal foil with resin, the resin layer needs to have sufficient fluidity when melted. However, for example, when using a thermosetting resin that is easy to obtain high heat resistance, or when using an inorganic filler that contributes to low thermal expansion, etc., sometimes it is impossible to obtain sufficient fluidity of the resin layer.

[0012] As a method for improving the fluidity of the resin layer, a method of making the resin layer contain a small amount of organic solvent to the extent that the solid is maintained can be considered. However, when the resin layer containing a small amount of organic solvent is heated and cured, voids may be generated in the cured product due to the volatilized organic solvent, or unevenness may appear on the surface of the cured product. In addition, since the organic solvent volatilizes during the heat curing, it is also necessary to provide a safer working environment.

[0013] In view of such a situation, the subject of this embodiment is to provide a metal foil with resin having excellent fluidity of the resin layer and capable of suppressing the generation of volatile components during heat curing, a method for manufacturing a printed wiring board using the metal foil with resin, and a method for manufacturing a semiconductor package.

[0014] Means for solving problems

[0015] The present inventors have studied to solve the above-mentioned problems, and as a result, have found that the problems can be solved by the following present embodiment.

[0016] That is, this embodiment relates to the following [1] to

[11] .

[0017] [1] A metal foil with a resin, comprising a metal foil and a resin layer containing a resin composition provided on one surface of the metal foil,

[0018] The resin composition contains: (A) a thermosetting resin; (B) a compound which is liquid at 25°C, has a reactive group and has a molecular weight of 1,000 or less; and (C) an inorganic filler.

[0019] [2] The resin-coated metal foil according to [1] above, wherein the component (A) is one or more selected from a maleimide resin having one or more N-substituted maleimide groups and a derivative of the maleimide resin.

[0020] [3] The metal foil with resin according to the above [2], wherein the maleimide resin having one or more N-substituted maleimide groups is a maleimide resin having a condensed ring of an aromatic ring and an aliphatic ring in its molecular structure and having two or more N-substituted maleimide groups.

[0021] [4] The resin-coated metal foil according to any one of [1] to [3] above, wherein the component (B) has one or more selected from a functional group containing an ethylenically unsaturated bond, an epoxy group, a hydroxyl group, a carboxyl group and an amino group as the reactive group.

[0022] [5] The resin-coated metal foil according to any one of [1] to [4], wherein the component (B) has two or more of the reactive groups in one molecule.

[0023] [6] The metal foil with resin according to any one of [1] to [5], wherein the component (B) is a di(meth)acrylate.

[0024] [7] The resin-coated metal foil according to any one of [1] to [6] above, wherein the content of the component (B) is 0.5 to 20% by mass relative to the total solid content (100% by mass) of the resin composition.

[0025] [8] The resin-coated metal foil according to any one of [1] to [7], wherein the metal foil is copper foil.

[0026] [9] The metal foil with resin according to any one of [1] to [8], wherein the mass reduction rate of the resin layer when heated and dried at 170° C. for 30 minutes in an air atmosphere is 2.0 mass % or less.

[0027]

[10] A method for producing a printed wiring board, comprising forming an insulating material using the metal foil with resin as described in any one of [1] to [9] above.

[0028]

[11] A method for manufacturing a semiconductor package, wherein an insulating material is formed using the metal foil with resin described in any one of [1] to [9] above.

[0029] Effects of the Invention

[0030] According to the present embodiment, it is possible to provide a metal foil with resin having excellent fluidity of the resin layer and capable of suppressing generation of volatile components during heat curing, a method for manufacturing a printed wiring board using the metal foil with resin, and a method for manufacturing a semiconductor package. DETAILED DESCRIPTION

[0031] In the present specification, a numerical range expressed using "to" means a range including the numerical values ​​described before and after "to" as the minimum value and the maximum value, respectively.

[0032] For example, a numerical range such as "X to Y" (X, Y are real numbers) refers to a numerical range greater than X and less than Y. Also, a description such as "greater than X" in this specification refers to X and a numerical value greater than X. In addition, a description such as "less than Y" in this specification refers to Y and a numerical value less than Y.

[0033] The lower limit and the upper limit of the numerical range described in the present specification can be arbitrarily combined with the lower limit or the upper limit of other numerical ranges, respectively.

[0034] In the numerical range described in the present specification, the lower limit value or the upper limit value of the numerical range may be replaced with the value shown in the Examples.

[0035] Unless otherwise specified, each component and material exemplified in the present specification may be used alone or in combination of two or more.

[0036] In the present specification, when there are plural substances corresponding to each component in the resin composition, the content of each component in the resin composition refers to the total amount of the plural substances present in the resin composition unless otherwise specified.

[0037] In this specification, "resin composition" refers to a mixture containing at least two or more components of resins, and when the resin is a thermosetting resin, it also includes a material in which the mixture is in a B-stage state. The types and contents of each component in the resin composition in a B-stage state refer to the types and contents of each component before the resin composition is in a B-stage state, that is, the types and amounts of the components added when the resin composition is manufactured.

[0038] In this specification, when a "layer" is expressed, in addition to a solid layer, a layer that is not a solid layer but has a portion in an island shape, a layer with holes, and a layer in which the interface with the adjacent layer is unclear are also included in the "layer".

[0039] In this specification, "solid content" refers to components other than the solvent, and also includes substances that are liquid, syrupy, and waxy at room temperature. Here, in this specification, room temperature means 25°C.

[0040] In this specification, "(meth)acrylate" refers to "acrylate" and its corresponding "methacrylate". Similarly, "(meth)acrylic acid" refers to "acrylic acid" and its corresponding "methacrylic acid", and "(meth)acryloyl" refers to "acryloyl" and its corresponding "methacryloyl".

[0041] The "molecular weight" of a compound in this specification refers to a molecular weight that can be calculated from the structural formula when the compound is not a polymer but the structural formula of the compound can be determined, and refers to a number average molecular weight when the compound is a polymer.

[0042] The number average molecular weight in this specification refers to a value measured by gel permeation chromatography (GPC) and converted to polystyrene. Specifically, the number average molecular weight in this specification can be measured by the method described in the Examples.

[0043] The mechanism of action described in this specification is a guess, and does not limit the mechanism by which the effect of the resin composition of the present embodiment is exerted.

[0044] A mode in which the matters described in this specification are arbitrarily combined is also included in this embodiment.

[0045] [Metal foil with resin]

[0046] The metal foil with resin according to the present embodiment includes a metal foil and a resin layer containing a resin composition provided on one surface of the metal foil.

[0047] The resin composition contains (A) a thermosetting resin; (B) a compound which is liquid at 25°C, has a reactive group and has a molecular weight of less than 1,000; and (C) an inorganic filler.

[0048] In addition, in this specification, each component may be abbreviated as (A) component, (B) component, etc., respectively, and the same abbreviation method may be used for other components.

[0049] In addition, (B) a compound that is liquid at 25°C, has a reactive group, and has a molecular weight of 1,000 or less may be referred to as "(B) reactive liquid compound".

[0050] In the present embodiment, being liquid at 25° C. means that the viscosity calculated by the following measurement method is 100,000 mPa·s or less.

[0051] <Method for measuring viscosity>

[0052] Device: E-type viscometer

[0053] Conical rotor: 1°34'×R24

[0054] Temperature: 25℃

[0055] Sample volume: 1.0 mL

[0056] Speed: 20rpm

[0057] Hereinafter, in this specification, the viscosity at 25° C. means the viscosity measured by the above-mentioned method.

[0058] The reason why the resin layer of the metal foil with resin according to the present embodiment is excellent in fluidity and can suppress generation of volatile components during heat curing is presumed as follows.

[0059] The resin composition contained in the resin layer of the resin-attached metal foil of the present embodiment contains (B) a compound that is liquid at 25° C. and has a molecular weight of 1,000 or less as a component that improves the fluidity of the resin layer. The (B) reactive liquid compound is a liquid component with a relatively low molecular weight, and thus can improve the fluidity of the resin layer when it is heated and melted.

[0060] In addition, the (B) reactive liquid compound has a reactive group, so during the heat curing of the (A) thermosetting resin, the (B) reactive liquid compound can react with each other or with other components. That is, the (B) reactive liquid compound helps to improve fluidity and suppresses volatilization through the curing reaction. Therefore, it can be considered that the metal foil with resin of this embodiment can suppress the generation of volatile components and improve fluidity compared to the case where an organic solvent or the like is used as a component for improving fluidity.

[0061] Resin layer

[0062] The resin layer of the metal foil with resin according to the present embodiment contains a resin composition [hereinafter, sometimes simply referred to as “the resin composition according to the present embodiment”], and is preferably a resin layer obtained by forming a layer of the resin composition according to the present embodiment.

[0063] The resin composition of the present embodiment contains: (A) a thermosetting resin; (B) a compound which is liquid at 25° C., has a reactive group, and has a molecular weight of 1,000 or less; and (C) an inorganic filler.

[0064] Hereinafter, each component which the resin composition of this embodiment may contain is demonstrated sequentially.

[0065] <(A) Thermosetting resin>

[0066] The resin composition of the present embodiment contains (A) a thermosetting resin.

[0067] (A) Thermosetting resins may be used alone or in combination of two or more.

[0068] (A) Thermosetting resins include, for example, epoxy resins, phenolic resins, maleimide resins, cyanate resins, isocyanate resins, benzoxazine resins, oxetane resins, amino resins, unsaturated polyester resins, allyl resins, dicyclopentadiene resins, silicone resins, triazine resins, and melamine resins.

[0069] Among them, the (A) thermosetting resin is preferably a maleimide resin from the viewpoint of heat resistance, and more preferably at least one selected from a maleimide resin having one or more N-substituted maleimide groups and a derivative of the maleimide resin.

[0070] In the following description, “one or more selected from a maleimide resin having one or more N-substituted maleimide groups and a derivative of the maleimide resin” may be referred to as “maleimide-based resin”.

[0071] In the following description, a maleimide resin having one or more N-substituted maleimide groups may be referred to as a "maleimide resin (AX)" or a "component (AX)".

[0072] In addition, a derivative of a maleimide resin having one or more N-substituted maleimide groups may be referred to as a "maleimide resin derivative (AY)" or a "(AY) component".

[0073] (Maleimide resin (AX))

[0074] The maleimide resin (AX) is not particularly limited as long as it is a maleimide resin having one or more N-substituted maleimide groups.

[0075] From the viewpoint of conductor adhesion and heat resistance, the maleimide resin (AX) is preferably an aromatic maleimide resin having two or more N-substituted maleimide groups, and more preferably an aromatic bismaleimide resin having two N-substituted maleimide groups.

[0076] It should be noted that, in this specification, "aromatic maleimide resin" refers to a compound having an N-substituted maleimide group directly bonded to an aromatic ring. In addition, in this specification, "aromatic bismaleimide resin" refers to a compound having two N-substituted maleimide groups directly bonded to an aromatic ring. In addition, in this specification, "aromatic polymaleimide resin" refers to a compound having three or more N-substituted maleimide groups directly bonded to an aromatic ring.

[0077] In addition, in this specification, "aliphatic maleimide resin" means a compound having an N-substituted maleimide group directly bonded to an aliphatic hydrocarbon.

[0078] As the maleimide resin (AX), from the viewpoints of dielectric properties, conductor adhesion and heat resistance, a maleimide resin having a condensed ring of an aromatic ring and an aliphatic ring in its molecular structure and having two or more N-substituted maleimide groups (hereinafter, sometimes referred to as "maleimide resin (A1)" or "(A1) component"). ] is preferred.

[0079] [Maleimide resin (A1)]

[0080] The maleimide resin (A1) is preferably an aromatic maleimide resin having a condensed ring of an aromatic ring and an aliphatic ring in its molecular structure and having two or more N-substituted maleimide groups from the viewpoint of dielectric properties, conductor adhesion and heat resistance.

[0081] The maleimide resin (A1) is more preferably an aromatic bismaleimide resin having a condensed ring of an aromatic ring and an aliphatic ring in its molecular structure and having two N-substituted maleimide groups.

[0082] From the viewpoints of dielectric properties, conductor adhesion and ease of production, the condensed ring contained in the maleimide resin (A1) preferably has a condensed bicyclic structure, and more preferably an indane ring.

[0083] As the maleimide resin (A1) containing an indane ring, an aromatic bismaleimide resin containing an indane ring is preferred.

[0084] It should be noted that, in this specification, the indane ring refers to a fused bicyclic structure of an aromatic 6-membered ring and a saturated aliphatic 5-membered ring. At least one of the ring-forming carbon atoms forming the indane ring has a bonding group for bonding to other groups constituting the maleimide resin (A1). The ring-forming carbon atom having the bonding group and other ring-forming carbon atoms may not have a bonding group, a substituent, etc. in addition to the above-mentioned bonding group, but preferably a divalent group is formed by having a bonding group other than the above-mentioned.

[0085] In the maleimide resin (A1), the indane ring is preferably contained in the form of a divalent group represented by the following general formula (A1-1).

[0086] [Chemical formula 1]

[0087]

[0088] (Where R a1It is an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, an aryloxy group having 6 to 10 carbon atoms, an arylthio group having 6 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, a halogen atom, a hydroxyl group or a mercapto group. a1 is an integer from 0 to 3. a2 ~R a4 Each independently represents an alkyl group having 1 to 10 carbon atoms. * represents a bonding site. )

[0089] As R in the above general formula (A1-1) a1 Examples of the alkyl group having 1 to 10 carbon atoms include methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, etc. These alkyl groups may be linear or branched.

[0090] As R a1 Examples of the alkyl group contained in the alkoxy group having 1 to 10 carbon atoms and the alkylthio group having 1 to 10 carbon atoms shown in the foregoing examples include the same groups as those for the alkyl group having 1 to 10 carbon atoms.

[0091] As R a1 Examples of the aryl group having 6 to 10 carbon atoms include phenyl and naphthyl.

[0092] As R a1 Examples of the aryl group contained in the aryloxy group having 6 to 10 carbon atoms and the arylthio group having 6 to 10 carbon atoms shown in the above-mentioned example include the same groups as those mentioned above for the aryl group having 6 to 10 carbon atoms.

[0093] As R a1 Examples of the cycloalkyl group having 3 to 10 carbon atoms include cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, cyclononyl and cyclodecyl.

[0094] In the above general formula (A1.1), n a1 When R is an integer of 1 to 3, from the viewpoint of solvent solubility and reactivity, a1 An alkyl group having 1 to 4 carbon atoms, a cycloalkyl group having 3 to 6 carbon atoms, or an aryl group having 6 to 10 carbon atoms is preferred, and an alkyl group having 1 to 4 carbon atoms is more preferred.

[0095] As R a2 ~R a4 The alkyl group having 1 to 10 carbon atoms represented by a1 The same alkyl group. a2 ~R a4 An alkyl group having 1 to 4 carbon atoms is preferred, a methyl group and an ethyl group are more preferred, and a methyl group is further preferred.

[0096] In the above general formula (A1-1), n a1 is an integer from 0 to 3, n a1 If the value is 2 or 3, multiple R a1 They can be the same or different from each other.

[0097] Among the above, from the viewpoint of ease of production, the divalent group represented by the general formula (A1-1) is preferably n a1 0, R a2 ~R a4 The divalent group represented by the following formula (A1-1a) which is a methyl group is more preferably a divalent group represented by the following formula (A1-1a′) or a divalent group represented by the following formula (A1-1a″).

[0098] [Chemical formula 2]

[0099]

[0100] (Wherein, * indicates the bonding site.)

[0101] As the maleimide resin (A1) containing a divalent group represented by the general formula (A1-1), a maleimide resin represented by the following general formula (A1-2) is preferred from the viewpoints of dielectric properties, conductor adhesion, heat resistance and ease of production.

[0102] [Chemical formula 3]

[0103]

[0104] (Where R a1 ~R a4 and n a1 and R in the above general formula (A1-1) a1 ~R a4 and n a1 Same. a5 Each is independently an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, an aryloxy group having 6 to 10 carbon atoms, an arylthio group having 6 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, a halogen atom, a nitro group, a hydroxyl group or a mercapto group. a2 Each independently represents an integer from 0 to 4. a3 A number between 0.95 and 10.0.)

[0105] In the above general formula (A1-2), a plurality of R a1 Each other, multiple n a1 Each other, multiple R a5 Each other, multiple n a2 They may be the same as or different from each other.

[0106] In n a3 If more than 1, multiple R a2 Each other, multiple R a3 Each other and multiple R a4 They may be the same as or different from each other.

[0107] As R in the above general formula (A1-2) a5 The alkyl group having 1 to 10 carbon atoms, the alkoxy group having 1 to 10 carbon atoms, the alkylthio group having 1 to 10 carbon atoms, the aryl group having 6 to 10 carbon atoms, the aryloxy group having 6 to 10 carbon atoms, the arylthio group having 6 to 10 carbon atoms and the cycloalkyl group having 3 to 10 carbon atoms can be exemplified by the same group as R a1 The same groups are preferred.

[0108] In the above general formula (A1-2), n a2 It is an integer of 0 to 4, and is preferably an integer of 1 to 3, more preferably 2 or 3, and even more preferably 2, from the viewpoint of compatibility with other resins, dielectric properties, conductor adhesion, and ease of production.

[0109] It should be noted that by making n a2 When n is 1 or more, the benzene ring and the N-substituted maleimide group have a distorted conformation, and the solvent solubility tends to be further improved because the stacking between molecules is suppressed. a2 When R is greater than 1, a5 The substitution position is preferably the ortho position relative to the N-substituted maleimide group.

[0110] From the viewpoints of dielectric properties, conductor adhesion, solvent solubility, handling properties, and heat resistance, n in the general formula (A1-2) is a3 It is preferably a number of 0.98 to 8.0, more preferably a number of 1.0 to 7.0, and still more preferably a number of 1.1 to 6.0. a3 The average value of the number of structural units containing an indane ring is shown.

[0111] From the viewpoints of dielectric properties, conductor adhesion, solvent solubility and ease of production, the maleimide resin (A1) represented by the general formula (A1-2) is more preferably a maleimide resin represented by the following general formula (A1.3) or a maleimide resin represented by the following general formula (A1-4).

[0112] [Chemical formula 4]

[0113]

[0114] (Where R a1 ~Ra5 and n a1 and n a3 and R in the above general formula (A1-2) a1 ~R a5 and n a1 and n a3 same.)

[0115]

[0116] (Where R a1 ~R a4 and n a1 and n a3 and R in the above general formula (A1-2) a1 ~R a4 and n a1 and n a3 same.)

[0117] Examples of the maleimide resin (A1) represented by the general formula (A1-3) include a maleimide resin represented by the following general formula (A1-3-1), a maleimide resin represented by the following general formula (A1-3-2), and a maleimide resin represented by the following general formula (A1-3-3).

[0118] [Chemical formula 5]

[0119]

[0120] (where n a3 With the above general formula (A1-2) in n a3 same.)

[0121] The maleimide resin (A1) represented by the general formula (A1-4) is more preferably a maleimide resin represented by the following general formula (A1-4-1) from the viewpoints of dielectric properties, conductor adhesion, solvent solubility, and ease of production.

[0122] [Chemical formula 6]

[0123]

[0124] (where n a3 With the above general formula (A1-2) in n a3 same.)

[0125] The number average molecular weight of the maleimide resin (A1) is not particularly limited, but is preferably 600 to 3,000, more preferably 800 to 2,000, and even more preferably 1,000 to 1,500 from the viewpoint of compatibility with other resins, conductor adhesion, and heat resistance.

[0126] The maleimide resin (AX) may be a maleimide resin (A2) other than the maleimide resin (A1) [hereinafter, sometimes referred to as "maleimide resin (A2)" or "component (A2)".].

[0127] [Maleimide resin (A2)]

[0128] As the maleimide resin (A2), a maleimide resin represented by the following general formula (A2-1) is preferred.

[0129] [Chemical formula 7]

[0130]

[0131] (Where X a11 It is a divalent organic group that does not contain a condensed ring of an aromatic ring and an aliphatic ring.)

[0132] X in the above general formula (A2-1) a11 It is a divalent organic group not including a condensed ring of an aromatic ring and an aliphatic ring.

[0133] As X in the above general formula (A2-1) a11 The divalent organic group represented by the following general formula (A2-2) includes a divalent group, a divalent group represented by the following general formula (A2-3), a divalent group represented by the following general formula (A2-4), a divalent group represented by the following general formula (A2-5), a divalent group represented by the following general formula (A2-6), etc.

[0134] [Chemical formula 8]

[0135]

[0136] (Where R a11 It is an aliphatic hydrocarbon group having 1 to 5 carbon atoms or a halogen atom. a11 is an integer from 0 to 4. * indicates a bonding site. )

[0137] As R in the above general formula (A2-2) a11 The aliphatic hydrocarbon group having 1 to 5 carbon atoms represented by , for example, includes alkyl groups having 1 to 5 carbon atoms such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, and n-pentyl; alkenyl groups having 2 to 5 carbon atoms; alkynyl groups having 2 to 5 carbon atoms; and the like. The aliphatic hydrocarbon group having 1 to 5 carbon atoms may be either linear or branched. As the aliphatic hydrocarbon group having 1 to 5 carbon atoms, an aliphatic hydrocarbon group having 1 to 3 carbon atoms is preferred, an alkyl group having 1 to 3 carbon atoms is more preferred, and a methyl group is further preferred.

[0138] Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom.

[0139] In the above general formula (A2-2), n a11 It is an integer of 0 to 4, preferably an integer of 0 to 2, more preferably 0 or 1, and even more preferably 0, from the viewpoint of easy availability.

[0140] In n a11 When the integer is 2 or more, multiple R a11 They can be the same or different from each other.

[0141] [Chemical formula 9]

[0142]

[0143] (Where R a12 and R a13 Each independently represents an aliphatic hydrocarbon group having 1 to 5 carbon atoms or a halogen atom. a12 It is an alkylene group having 1 to 5 carbon atoms, an alkylidene group having 2 to 5 carbon atoms, an ether group, a thioether group, a sulfonyl group, a carbonyloxy group, a keto group, a single bond, or a divalent group represented by the following general formula (A2-3-1). a12 and n a13 Each independently represents an integer of 0 to 4. * represents a bonding site. )

[0144] As R in the above general formula (A2-3) a12 and R a13 The aliphatic hydrocarbon group having 1 to 5 carbon atoms and the halogen atom represented by the above R a11 Same group.

[0145] As X in the above general formula (A2-3) a12 Examples of the alkylene group having 1 to 5 carbon atoms include methylene, 1,2-ethylene, 1,3-propylene, 1,4-butylene and 1,5-pentylene.

[0146] As X in the above general formula (A2-3) a12 Examples of the alkylidene group having 2 to 5 carbon atoms include ethylidene, propylidene, isopropylidene, butylidene, isobutylidene, pentylidene and isopentylidene.

[0147] In the above general formula (A2-3), n a12 and n a13 Each independently represents an integer of 0 to 4, and is preferably an integer of 1 to 3, more preferably 1 or 2, and even more preferably 2, from the viewpoint of easy availability, compatibility with other resins, and suppression of gelation of the product during the reaction.

[0148] In n a12 or a13When the integer is 2 or more, multiple R a12 Each other or multiple R a13 They may be the same as or different from each other.

[0149] X in the above general formula (A2-3) a12 The divalent group represented by the general formula (A2-3-1) is as follows.

[0150] [Chemical formula 10]

[0151]

[0152] (Where R a14 and R a15 Each independently represents an aliphatic hydrocarbon group having 1 to 5 carbon atoms or a halogen atom. a13 It is an alkylene group having 1 to 5 carbon atoms, an alkylidene group having 2 to 5 carbon atoms, an ether group, a thioether group, a sulfonyl group, a carbonyloxy group, a keto group or a single bond. a14 and n a15 Each independently represents an integer of 0 to 4. * represents a bonding site. )

[0153] As R in the above general formula (A2-3-1) a14 and R a15 The aliphatic hydrocarbon group having 1 to 5 carbon atoms and the halogen atom represented by the above R a11 Same group.

[0154] As X in the above general formula (A2-3-1) a13 The alkylene group having 1 to 5 carbon atoms and the alkylidene group having 2 to 5 carbon atoms represented by X include, for example, a12 Same group.

[0155] In the above general formula (A2-3-1), n a14 and n a15 Each independently represents an integer of 0 to 4, and is preferably an integer of 0 to 2, more preferably 0 or 1, and even more preferably 0, from the viewpoint of easy availability.

[0156] In n a14 or a15 When the integer is 2 or more, multiple R a14 Each other or multiple R a15 They may be the same as or different from each other.

[0157] [Chemical formula 11]

[0158]

[0159] (where n a16is an integer from 0 to 10. * indicates a bonding site. )

[0160] From the viewpoint of easy availability, n in the above general formula (A2-4) is a16 An integer of 0-5 is preferable, an integer of 0-4 is more preferable, and an integer of 0-3 is further preferable.

[0161] [Chemical formula 12]

[0162]

[0163] (where n a17 It is a number from 0 to 5. * indicates a bonding site. )

[0164] [Chemical formula 13]

[0165]

[0166] (Where R a16 and R a17 Each independently represents a hydrogen atom or an aliphatic hydrocarbon group having 1 to 5 carbon atoms. a18 is an integer from 1 to 8. * represents a bonding site. )

[0167] As R in the above general formula (A2-6) a16 and R a17 The aliphatic hydrocarbon group having 1 to 5 carbon atoms represented by a11 Same group.

[0168] In the above general formula (A2-6), n a18 is an integer of 1 to 8, preferably an integer of 1 to 5, more preferably an integer of 1 to 3, and further preferably 1. a18 When the integer is 2 or more, multiple R a16 Each other or multiple R a17 They may be the same as or different from each other.

[0169] Moreover, as maleimide resin (A2), polymaleimide resin represented by the following general formula (A2-7) is preferable.

[0170] [Chemical formula 14]

[0171]

[0172] (Where X a14 are each independently a divalent hydrocarbon group having 1 to 20 carbon atoms, n a19 is an integer from 2 to 5.)

[0173] As X in the above general formula (A2-7) a14Examples of the divalent hydrocarbon group having 1 to 20 carbon atoms include divalent aliphatic hydrocarbon groups such as alkylene groups having 1 to 5 carbon atoms and alkylidene groups having 2 to 5 carbon atoms; and divalent hydrocarbon groups including aromatic hydrocarbon groups represented by the following general formula (A2-8).

[0174] Examples of the alkylene group having 1 to 5 carbon atoms include methylene, 1,2-ethylene, 1,3-propylene, 1,4-butylene, 1,5-pentylene, etc. As the alkylene group having 1 to 5 carbon atoms, an alkylene group having 1 to 3 carbon atoms is preferred, an alkylene group having 1 or 2 carbon atoms is more preferred, and a methylene group is further preferred.

[0175] The alkylidene group having 2 to 5 carbon atoms is preferably an alkylidene group having 2 to 4 carbon atoms, more preferably an alkylidene group having 2 or 3 carbon atoms, and further preferably an isopropylidene group.

[0176] [Chemical formula 15]

[0177] *-X a15 -Ar a1 -X a16 -* (A2-8)

[0178] (Where Ar a1 is a divalent aromatic hydrocarbon group, X a15 and X a16 Each independently represents a divalent aliphatic hydrocarbon group having 1 to 5 carbon atoms. * represents a bonding site. )

[0179] As X in the above general formula (A2-8) a15 and X a16 The divalent aliphatic hydrocarbon group having 1 to 5 carbon atoms represented by a14 The alkylene group having 1 to 5 carbon atoms and the alkylidene group having 2 to 5 carbon atoms are the same groups as mentioned above. Among them, the methylene group is preferred.

[0180] As Ar in the above general formula (A2-8) a1 The divalent aromatic hydrocarbon group represented by , for example, phenylene, naphthylene, biphenylene, anthrylene, etc. can be mentioned. Among them, biphenylene is preferred. As biphenylene, 4,2'-biphenylene, 4,3'-biphenylene, 4,4'-biphenylene, 3,3'-biphenylene, etc. can be mentioned, among which 4,4'-biphenylene is preferred.

[0181] In the above options, X in the above general formula (A2-7) a14 Preferably, it is a divalent hydrocarbon group containing an aromatic hydrocarbon group represented by the above general formula (A2-8), and more preferably, X in the above general formula (A2-8) is a15 and X a16 is a methylene group and Ara1 It is a divalent hydrocarbon group of 4,4'-biphenylene.

[0182] In the above general formula (A2-7), n a19 It is an integer of 2-5, preferably an integer of 2-4, and more preferably 2 or 3.

[0183] As maleimide resin (A2), aromatic bismaleimide resin, aromatic polymaleimide resin, aliphatic maleimide resin etc. are mentioned, for example.

[0184] Specific examples of the maleimide resin (A2) include bis(4-maleimidephenyl)methane, m-phenylene bismaleimide, 2,2-bis[4-(4-maleimidephenoxy)phenyl]propane, 4-methyl-1,3-phenylene bismaleimide, 3,3'-dimethyl-5,5'.diethyl-4,4'-diphenylmethane bismaleimide, polyphenylmethane maleimide, biphenyl aralkyl maleimide, etc. Among them, biphenyl aralkyl maleimide is preferred.

[0185] (Maleimide resin derivative (AY))

[0186] As the maleimide resin derivative (AY), an aminomaleimide resin having a structural unit derived from the maleimide resin (AX) and a structural unit derived from a diamine compound is preferred.

[0187] The aminomaleimide resin has a structural unit derived from the maleimide resin (AX) and a structural unit derived from a diamine compound.

[0188] The aminomaleimide resin is obtained by, for example, subjecting a maleimide resin (AX) to Michael addition of a diamine compound.

[0189] As the diamine compound, for example, the same diamine compound as the amine compound having at least two primary amino groups in one molecule listed in Japanese Patent Application Laid-Open No. 2020-200406 can be used. Among them, 4,4'-diaminodiphenylmethane, 3,3'-dimethyl-4,4'-diaminodiphenylmethane, 3,3'-diethyl-4,4'-diaminodiphenylmethane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 4,4'-[1,3-phenylenebis(1-methylethylidene)]dianiline, 4,4'-[1,4-phenylenebis(1-methylethylidene)]dianiline, 3,3'-diethyl-4,4'-diaminodiphenylmethane are preferred.

[0190] Among the thermosetting resins (A) described above, from the viewpoints of dielectric properties, conductor adhesion and heat resistance, the thermosetting resin (A) is preferably a maleimide resin having a condensed ring of an aromatic ring and an aliphatic ring in its molecular structure and having two or more N-substituted maleimide groups.

[0191] The (A) thermosetting resin preferably has a viscosity at 25°C measured by the above method exceeding 100,000 mPa·s, and is more preferably solid at 25°C.

[0192] ((A) Content of thermosetting resin)

[0193] In the resin composition of the present embodiment, the content of (A) thermosetting resin is not particularly limited, and is preferably 5 to 60 mass %, more preferably 8 to 40 mass %, further preferably 10 to 30 mass %, and particularly preferably 15 to 25 mass %, relative to the total amount (100 mass %) of the resin components in the resin composition of the present embodiment.

[0194] When the content of the thermosetting resin (A) is above the above lower limit, the heat resistance, formability, processability and conductor adhesion tend to be better. In addition, when the content of the thermosetting resin (A) is below the above upper limit, the dielectric properties tend to be better.

[0195] In addition, the upper limit of the content of the thermosetting resin (A) may be 80% by mass or less, 70% by mass or less, or 60% by mass or less, relative to the total amount (100% by mass) of the thermosetting resin (A) and the reactive liquid compound (B). In addition, the lower limit of the content of the thermosetting resin (A) may be 5% by mass or more, 10% by mass or more, or 15% by mass or more, relative to the total amount (100% by mass) of the thermosetting resin (A) and the reactive liquid compound (B).

[0196] Here, in this specification, the "resin component" refers to a resin and a compound that forms a resin by a curing reaction.

[0197] For example, in the resin composition of the present embodiment, the component (A), the component (B), and the component (C) correspond to the resin component.

[0198] When the resin composition of the present embodiment contains a resin or a compound that forms a resin by a curing reaction as an optional component in addition to the above components, these optional components are also included in the resin component. As an optional component equivalent to the resin component, there can be mentioned the component (E) and the component (F) described later.

[0199] On the other hand, the component (D) is not contained in the resin component.

[0200] The content of the resin component in the resin composition of the present embodiment is not particularly limited, and is preferably 5 to 80% by mass, more preferably 10 to 60% by mass, and further preferably 20 to 40% by mass, relative to the total solid content (100% by mass) of the resin composition of the present embodiment from the viewpoint of low thermal expansion, heat resistance, flame retardancy and conductor adhesion.

[0201] The content of the maleimide resin in the (A) thermosetting resin is not particularly limited, but is preferably 80 to 100% by mass, more preferably 90 to 100% by mass, and even more preferably 95 to 100% by mass, relative to the total amount (100% by mass) of the (A) thermosetting resin.

[0202] If the content of the maleimide resin is above the above lower limit, the heat resistance, formability, processability and conductor adhesion tend to become better. In addition, if the content of the maleimide resin is below the above upper limit, the dielectric properties tend to become better.

[0203] <(B) Reactive liquid compound>

[0204] The resin composition contained in the resin layer of the metal foil with resin of the present embodiment can improve the fluidity of the resin layer when heated and melted by containing the reactive liquid compound (B). In addition, the reactive liquid compound (B) can penetrate well into the molecules of the resin component, and can also improve the flexibility of the resin layer by effectively weakening the intermolecular interaction of the resin component. Therefore, even if the thickness of the resin layer is increased, when the metal foil with resin is processed, it is possible to suppress the generation of cracks in the resin layer.

[0205] (B) The reactive liquid compound is not particularly limited as long as it is a compound that is liquid at 25° C., has a reactive group, and has a molecular weight of 1,000 or less.

[0206] (B) The reactive liquid compound may be used alone or in combination of two or more.

[0207] The reactive liquid compound (B) preferably has two or more reactive groups in one molecule, more preferably has 2 to 5 reactive groups, further preferably has 2 to 4 reactive groups, and particularly preferably has 2 or 3 reactive groups.

[0208] When the number of reactive groups is within the above range, volatilization during heat curing is more effectively suppressed, and excellent fluidity and flexibility tend to be easily obtained.

[0209] The molecular weight of the reactive liquid compound (B) is 1,000 or less, preferably 100 to 800, more preferably 150 to 600, and even more preferably 200 to 400.

[0210] If the molecular weight of the reactive liquid compound (B) is above the lower limit, the volatilization of the reactive liquid compound (B) before the resin composition is heated and cured tends to be suppressed. In addition, if the molecular weight of the reactive liquid compound (B) is below the upper limit, it tends to be easy to obtain more excellent fluidity and flexibility.

[0211] The viscosity of the reactive liquid compound (B) at 25° C. is preferably 1 to 5,000 mPa.s, more preferably 2 to 1,000 mPa.s, and even more preferably 4 to 500 mPa.s.

[0212] When the viscosity of the reactive liquid compound (B) at 25°C is at least the above lower limit, volatilization of the reactive liquid compound (B) tends to be easily suppressed. On the other hand, when the viscosity of the reactive liquid compound (B) at 25°C is at most the above upper limit, more excellent fluidity and flexibility tend to be easily obtained.

[0213] (B) The viscosity of the reactive liquid compound at 25°C can be measured by the above-mentioned measurement method.

[0214] The (B) reactive liquid compound preferably has, as the reactive group, one or more selected from the group consisting of a functional group containing an ethylenically unsaturated bond, an epoxy group, a hydroxyl group, a carboxyl group, and an amino group.

[0215] It should be noted that, in the present specification, the "ethylenically unsaturated bond" refers to a carbon-carbon double bond capable of an addition reaction, and does not include a double bond of an aromatic ring.

[0216] Examples of the functional group containing an ethylenically unsaturated bond include a vinyl group, an allyl group, a 1-methallyl group, an isopropenyl group, a 2-butenyl group, a 3-butenyl group, a styryl group, an N-substituted maleimide group, and a (meth)acryloyl group.

[0217] Among them, the reactive group is more preferably a functional group containing an ethylenically unsaturated bond or an epoxy group. From the viewpoint of easily obtaining more excellent dielectric properties, a functional group containing an ethylenically unsaturated bond is further preferred, and a (meth)acryloyl group is particularly preferred.

[0218] Specific examples of the (B) reactive liquid compound having a (meth)acryloyl group as a reactive group include (meth)acrylates such as mono(meth)acrylate, di(meth)acrylate, and tri- or higher-functional (meth)acrylate.

[0219] Examples of the mono(meth)acrylate include methyl(meth)acrylate, ethyl(meth)acrylate, propyl(meth)acrylate, butyl(meth)acrylate, pentyl(meth)acrylate, hexyl(meth)acrylate, heptyl(meth)acrylate, 2-ethylhexyl(meth)acrylate, octyl(meth)acrylate, isooctyl(meth)acrylate, nonyl(meth)acrylate, decyl(meth)acrylate, dodecyl(meth)acrylate, lauryl(meth)acrylate, tridecyl(meth)acrylate, stearyl(meth)acrylate, cyclohexyl(meth)acrylate, cyclopentyl(meth)acrylate, benzyl(meth)acrylate, dicyclopentenyl(meth)acrylate, dicyclopentenyloxyethyl(meth)acrylate, methoxyethyl(meth)acrylate, ethoxyethyl(meth)acrylate, butoxyethyl(meth)acrylate, phenoxyethyl(meth)acrylate, 2-hydroxyethyl(meth)acrylate, 2-hydroxypropyl(meth)acrylate, and 4-hydroxybutyl(meth)acrylate.

[0220] Examples of the di(meth)acrylate include 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, tricyclodecane di(meth)acrylate, 1,12-dodecanediol di(meth)acrylate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, ethoxylated bisphenol A di(meth)acrylate, ethoxylated bisphenol F di(meth)acrylate, and dioxanediol di(meth)acrylate.

[0221] Examples of the dioxanediol di(meth)acrylate include 2-[5-ethyl-5-[(acryloyloxy)methyl]-1,3-dioxan-2-yl]-2,2-dimethylethyl acrylate and the like.

[0222] Examples of trifunctional or higher-functional (meth)acrylates include trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, and dipentaerythritol hexa(meth)acrylate.

[0223] Among the above options, as the (meth)acrylate, di(meth)acrylate is preferred.

[0224] As the di(meth)acrylate, a diacrylate represented by the following general formula (B-1) or a dimethacrylate represented by the following general formula (B-2) is preferred, and a dimethacrylate represented by the following general formula (B-2) is more preferred.

[0225] [Chemical formula 16]

[0226]

[0227] (Where R b1 is an alkylene group having 1 to 20 carbon atoms. )

[0228] From the viewpoint of fluidity, flexibility and suppression of volatilization, R in the above general formulas (B-1) and (B-2) b1 The alkylene group having 1 to 20 carbon atoms preferably has 4 to 18 carbon atoms, more preferably 6 to 15 carbon atoms, and further preferably 8 to 12 carbon atoms.

[0229] Examples of the alkylene group having 1 to 20 carbon atoms include methylene, ethylene, propylene, butylene, pentylene, hexylene, heptylene, octylene, nonylene, decylene, undecylene, dodecylene, tetradecylene, pentadecylene, etc. The alkylene group may be linear, branched or cyclic, and is preferably linear.

[0230] ((B) Content of reactive liquid compound)

[0231] In the resin composition of the present embodiment, the content of the reactive liquid compound (B) is not particularly limited, and is preferably 5 to 60% by mass, more preferably 8 to 40% by mass, further preferably 10 to 30% by mass, and particularly preferably 15 to 25% by mass, relative to the total amount (100% by mass) of the resin components in the resin composition of the present embodiment.

[0232] In the resin composition of the present embodiment, the content of the reactive liquid compound (B) is not particularly limited, but is preferably 0.5 to 20% by mass, more preferably 1.0 to 15% by mass, and even more preferably 1.5 to 10% by mass, relative to the total solid content (100% by mass) of the resin composition.

[0233] If the content of the reactive liquid compound (B) is above the lower limit, there is a tendency to easily obtain more excellent fluidity and flexibility. In addition, if the content of the reactive liquid compound (B) is below the upper limit, there is a tendency to easily suppress the generation of volatile components during heat curing.

[0234] <(C) Inorganic filler>

[0235] The resin composition of the present embodiment tends to easily obtain more excellent low thermal expansion property, heat resistance, and flame retardancy by containing the (C) inorganic filler.

[0236] In particular, since the resin composition of the present embodiment is excellent in fluidity and flexibility, the content of the (C) inorganic filler can be increased to further improve the low thermal expansion property.

[0237] (C) The inorganic filler may be used alone or in combination of two or more.

[0238] (C) Inorganic fillers include, for example, silica, alumina, titanium oxide, mica, beryllium oxide, barium titanate, potassium titanate, strontium titanate, calcium titanate, aluminum carbonate, magnesium hydroxide, aluminum hydroxide, aluminum silicate, calcium carbonate, calcium silicate, magnesium silicate, silicon nitride, boron nitride, clay, talc, aluminum borate, silicon carbide, etc. Among them, from the viewpoint of low thermal expansion, heat resistance and flame retardancy, silica, alumina, mica and talc are preferred, and silica and alumina are more preferred.

[0239] Examples of silica include precipitated silica with a high water content produced by a wet process, dry-process silica that contains almost no bound water, etc. Examples of dry-process silica include crushed silica, fumed silica, and fused silica, depending on the production method.

[0240] The (C) inorganic filler may be surface-treated with a surface treatment agent such as a silane coupling agent, for example, from the viewpoint of improving dispersibility and adhesion with an organic component.

[0241] The average particle size of the inorganic filler (C) is not particularly limited, but is preferably 0.01 to 20 μm, more preferably 0.1 to 10 μm, further preferably 0.2 to 1 μm, and particularly preferably 0.3 to 0.8 μm from the viewpoint of dispersibility and fine wiring properties of the inorganic filler (C).

[0242] It should be noted that, in this specification, the average particle size of the inorganic filler (C) refers to the particle size corresponding to the point of 50% volume when the total volume of the particles is set to 100% and the cumulative frequency distribution curve based on the particle size is obtained. The average particle size of the inorganic filler (C) can be measured, for example, by a particle size distribution measuring device using a laser diffraction scattering method.

[0243] Examples of the shape of the (C) inorganic filler include spherical shapes and crushed shapes, and a spherical shape is preferred.

[0244] ((C) Content of inorganic filler)

[0245] In the resin composition of the present embodiment, the content of the (C) inorganic filler is not particularly limited, but is preferably 20 to 95% by mass, more preferably 40 to 90% by mass, and even more preferably 60 to 80% by mass, relative to the total solid content (100% by mass) of the resin composition.

[0246] If the content of (C) inorganic filler is above the above lower limit, low thermal expansion, heat resistance and flame retardancy tend to become better. In addition, if the content of (C) inorganic filler is below the above upper limit, formability and conductor adhesion tend to become better.

[0247] <(D) Elastomers having a molecular weight exceeding 1,000>

[0248] The resin composition of the present embodiment preferably further contains (D) an elastomer having a molecular weight exceeding 1,000 [hereinafter, sometimes referred to as "(D) elastomer"].].

[0249] The resin composition of the present embodiment tends to easily obtain more excellent dielectric properties by containing the (D) elastomer.

[0250] In addition, the "elastomer" herein refers to a polymer having a glass transition temperature of 25° C. or less as measured by differential scanning calorimetry in accordance with JIS K 6240:2011.

[0251] (D) The elastomer may be used alone or in combination of two or more.

[0252] The molecular weight of the elastomer (D) exceeds 1,000, preferably 1,050 to 500,000, more preferably 1,100 to 350,000, and even more preferably 1,150 to 200,000.

[0253] If the molecular weight of the elastomer (D) is above the lower limit, the heat resistance of the resin composition tends to be better maintained. If the molecular weight of the elastomer (D) is below the upper limit, the dielectric properties and conductor adhesion of the resin composition tend to be better.

[0254] Preferred examples of the elastomer (D) include a conjugated diene polymer (D1), a modified conjugated diene polymer (D2), and a styrene-based elastomer (D3).

[0255] Preferred embodiments of these components are described below.

[0256] (Conjugated diene polymer (D1))

[0257] In this specification, the "conjugated diene polymer" refers to a polymer of a conjugated diene compound.

[0258] The resin composition of the present embodiment tends to easily obtain more excellent dielectric properties by containing the conjugated diene polymer (D1).

[0259] The conjugated diene polymer (D1) may be used alone or in combination of two or more.

[0260] Examples of the conjugated diene compound include 1,3-butadiene, isoprene, 1,3-pentadiene, 2,3-dimethyl-1,3-butadiene, 2-phenyl-1,3-butadiene, and 1,3-hexadiene.

[0261] The conjugated diene polymer (D1) may be a polymer of one conjugated diene compound or a copolymer of two or more conjugated diene compounds.

[0262] Furthermore, the conjugated diene polymer (D1) may be a copolymer of one or more conjugated diene compounds and one or more monomers other than the conjugated diene compound.

[0263] When the conjugated diene polymer (D1) is a copolymer, the polymerization method is not particularly limited, and any of random polymerization, block polymerization, and graft polymerization may be used.

[0264] As the conjugated diene polymer (D1), a conjugated diene polymer having a plurality of vinyl groups in a side chain is preferred from the viewpoint of compatibility with other resins and dielectric properties.

[0265] The number of vinyl groups in one molecule of the conjugated diene polymer (D1) is not particularly limited, but is preferably 3 or more, more preferably 5 or more, and even more preferably 10 or more, from the viewpoint of compatibility with other resins and dielectric properties.

[0266] The upper limit of the number of vinyl groups in the conjugated diene polymer (D1) per molecule is not particularly limited, and may be 100 or less, 80 or less, or 60 or less.

[0267] As the conjugated diene polymer (D1), for example: polybutadiene with 1,2-vinyl group, butadiene-styrene copolymer with 1,2-vinyl group, polyisoprene with 1,2-vinyl group, etc. can be cited. Among them, from the viewpoint of dielectric properties and heat resistance, polybutadiene with 1,2-vinyl group and butadiene-styrene copolymer with 1,2-vinyl group are preferred, and polybutadiene with 1,2-vinyl group is more preferred. In addition, as the polybutadiene with 1,2-vinyl group, polybutadiene homopolymer with 1,2-vinyl group is preferred.

[0268] The 1,2-vinyl group derived from butadiene in the conjugated diene polymer (D1) means a vinyl group contained in the structural unit derived from butadiene represented by the following formula (D1-1).

[0269] [Chemical formula 17]

[0270]

[0271] In the case where the conjugated diene polymer (D1) is a polybutadiene with 1,2-vinyl, relative to the total structural units of the butadiene constituting the polybutadiene, there is a content of 1,2-vinyl structural units [hereinafter, sometimes referred to as "vinyl content".] Not particularly limited, from the viewpoint of compatibility with other resins, dielectric properties and heat resistance, preferably more than 50 mol%, more preferably more than 70 mol%, further preferably more than 85 mol%. In addition, the upper limit of vinyl content is not particularly limited, can be less than 100 mol%, can also be less than 95 mol%, can also be less than 90 mol%. As the structural unit with 1,2-vinyl, the structural unit from butadiene shown in the preferred above-mentioned formula (D1-1).

[0272] From the same viewpoint, the polybutadiene having a 1,2-vinyl group is preferably a 1,2-polybutadiene homopolymer.

[0273] The number average molecular weight of the conjugated diene polymer (D1) is not particularly limited, but is preferably 1,050 to 3,000, more preferably 1,100 to 2,000, and even more preferably 1,150 to 1,500 from the viewpoint of compatibility with other resins, dielectric properties, and heat resistance.

[0274] (Modified conjugated diene polymer (D2))

[0275] The modified conjugated diene polymer (D2) is a polymer obtained by modifying a conjugated diene polymer.

[0276] The resin composition of the present embodiment has good heat resistance and low thermal expansion due to the inclusion of the modified conjugated diene polymer (D2), and tends to easily obtain more excellent dielectric properties.

[0277] The modified conjugated diene polymer (D2) may be used alone or in combination of two or more.

[0278] For example, when the (A) thermosetting resin includes a maleimide-based resin, the modified conjugated diene polymer (D2) is preferably a modified conjugated diene polymer obtained by modifying (d1) a conjugated diene polymer having a vinyl group in a side chain [hereinafter, sometimes referred to as "conjugated diene polymer (d1)"]. with (d2) a maleimide resin having two or more N-substituted maleimide groups [hereinafter, sometimes referred to as "maleimide resin (d2)".]. from the viewpoint of compatibility with other resins, dielectric properties and conductor adhesion.

[0279] As the conjugated diene polymer (d1), for example, the conjugated diene polymer having a vinyl group in a side chain described as the above conjugated diene polymer (D1) can be used, and the preferred embodiments are also the same.

[0280] The conjugated diene polymer (d1) may be used alone or in combination of two or more.

[0281] As the maleimide resin (d2), for example, the maleimide resin having two or more N-substituted maleimide groups described as the maleimide resin (AX) can be used, and the preferred embodiments are also the same.

[0282] The maleimide resin (d2) may be used alone or in combination of two or more.

[0283] The modified conjugated diene polymer (D2) preferably has a substituent (hereinafter sometimes referred to as "substituent (x)") formed by reaction of a vinyl group of the conjugated diene polymer (d1) with an N-substituted maleimide group of the maleimide resin (d2) in a side chain.

[0284] From the viewpoint of compatibility with other resins, dielectric properties, low thermal expansion and heat resistance, the substituent (x) is preferably a group containing a structure represented by the following general formula (D2-1) or (D2-2) as a structure derived from the maleimide resin (d2).

[0285] [Chemical formula 18]

[0286]

[0287] (Where X d1 A divalent group formed by removing two N-substituted maleimide groups from the maleimide resin (d2), * d1 This is a site bonded to a carbon atom derived from a vinyl group in a side chain of the conjugated diene polymer (d1).* d2 The site where atoms bond to other atoms.)

[0288] The modified conjugated diene polymer (D2) preferably has a substituent (x) and a vinyl group (y) in a side chain.

[0289] The extent to which the substituent (x) exists in the modified conjugated diene polymer (D2) can be determined by the extent to which the vinyl groups of the conjugated diene polymer (d1) are modified by the maleimide resin (d2) (hereinafter, sometimes referred to as “vinyl modification ratio”).

[0290] The vinyl modification rate is not particularly limited, but is preferably 20 to 70%, more preferably 30 to 60%, and further preferably 35 to 50%, from the viewpoint of compatibility with other resins, dielectric properties, low thermal expansion and heat resistance. Here, the vinyl modification rate is a value obtained by the method described in the Examples.

[0291] The vinyl group (y) is preferably a 1,2-vinyl group contained in the structural unit derived from butadiene.

[0292] The number average molecular weight of the modified conjugated diene polymer (D2) is not particularly limited, but is preferably 1,100 to 6,000, more preferably 1,300 to 4,000, and even more preferably 1,500 to 2,000 from the viewpoint of compatibility with other resins, dielectric properties, low thermal expansion and heat resistance.

[0293] The modified conjugated diene polymer (D2) can be produced by reacting the conjugated diene polymer (d1) with the maleimide resin (d2).

[0294] The method for reacting the conjugated diene polymer (d1) and the maleimide resin (d2) is not particularly limited. For example, the modified conjugated diene polymer (D2) can be obtained by placing the conjugated diene polymer (d1), the maleimide resin (d2), a reaction catalyst and an organic solvent in a reaction vessel and reacting them while heating, keeping warm, stirring, etc. as required.

[0295] The reaction temperature of the above reaction is preferably 70 to 120°C, more preferably 80 to 110°C, and even more preferably 85 to 105°C, from the viewpoint of workability and suppression of gelation of the product during the reaction.

[0296] From the viewpoint of productivity and sufficient progress of the reaction, the reaction time of the above reaction is preferably 0.5 to 15 hours, more preferably 1 to 10 hours, and even more preferably 3 to 7 hours.

[0297] However, these reaction conditions can be appropriately adjusted according to the types of raw materials used, and are not particularly limited.

[0298] When the above reaction is carried out, the molar number (M m ) relative to the molar number (M) of the side chain vinyl groups possessed by the conjugated diene polymer (d1) v ) ratio (M m / M v ) is not particularly limited, but is preferably 0.001 to 0.5, more preferably 0.005 to 0.1, and further preferably 0.008 to 0.05, from the viewpoint of compatibility of the obtained modified conjugated diene polymer (D2) with other resins and suppression of gelation of the product in the reaction.

[0299] <Styrene elastomer (D3)>

[0300] The styrene-based elastomer (D3) is not particularly limited as long as it is an elastomer having a structural unit derived from a styrene-based compound.

[0301] The resin composition of the present embodiment tends to easily obtain more excellent dielectric properties by containing the styrene-based elastomer (D3).

[0302] The styrene-based elastomer (D3) may be used alone or in combination of two or more.

[0303] The styrene-based elastomer (D3) preferably has a structural unit derived from a styrene-based compound represented by the following general formula (D3-1).

[0304] [Chemical formula 19]

[0305]

[0306] (Where R d1 is a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, R d2 It is an alkyl group having 1 to 5 carbon atoms. n d1 is an integer from 0 to 5.)

[0307] As R in the above general formula (D3-1) d1 and R d2 The alkyl group having 1 to 5 carbon atoms represented by , for example, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-pentyl, etc. can be mentioned. The alkyl group having 1 to 5 carbon atoms can be any of linear or branched. Among them, the alkyl group having 1 to 3 carbon atoms is preferred, the alkyl group having 1 or 2 carbon atoms is more preferred, and the methyl group is further preferred.

[0308] In the above general formula (D3-1), n d1It is an integer of 0 to 5, preferably an integer of 0 to 2, more preferably 0 or 1, and further preferably 0.

[0309] The styrene-based elastomer (D3) may contain a structural unit other than the structural unit derived from a styrene-based compound.

[0310] Examples of the structural unit other than the structural unit derived from the styrene-based compound which the styrene-based elastomer (D3) may contain include a structural unit derived from butadiene, a structural unit derived from isoprene, a structural unit derived from maleic acid, and a structural unit derived from maleic anhydride.

[0311] The structural unit derived from butadiene and the structural unit derived from isoprene may be hydrogenated. When hydrogenated, the structural unit derived from butadiene becomes a structural unit in which ethylene units and butene units are mixed, and the structural unit derived from isoprene becomes a structural unit in which ethylene units and propylene units are mixed.

[0312] Examples of the styrene-based elastomer (D3) include hydrogenated products of styrene-butadiene-styrene block copolymers, hydrogenated products of styrene-isoprene-styrene block copolymers, and styrene-maleic anhydride copolymers.

[0313] The hydrogenated products of styrene-butadiene-styrene block copolymers include SEBS formed by completely hydrogenating the carbon-carbon double bonds in the butadiene block, and SBBS formed by partially hydrogenating the carbon-carbon double bonds in the 1,2-bonding portion of the butadiene block. It should be noted that the complete hydrogenation in SEBS means that the carbon-carbon double bonds are usually 90% or more relative to the whole, and can be 95% or more, or 99% or more, or 100%. In addition, the partial hydrogenation rate in SBBS is, for example, 60 to 85% relative to the whole carbon-carbon double bonds. The hydrogenated product of styrene-isoprene-styrene block copolymer is obtained as SEPS by hydrogenating the polyisoprene part.

[0314] Among them, SEBS and SEPS are preferred, and SEBS is more preferred, from the viewpoint of dielectric properties, conductor adhesion, heat resistance, glass transition temperature, and low thermal expansion.

[0315] The content of the structural unit derived from the styrene compound in the styrene elastomer (D3) [hereinafter sometimes referred to as "styrene content"] is not particularly limited, but is preferably 5 to 60% by mass, more preferably 7 to 40% by mass, and further preferably 10 to 20% by mass.

[0316] The melt flow rate (MFR) of the styrene elastomer (D3) is not particularly limited, but is preferably 0.1 to 20 g / 10 min, more preferably 1 to 10 g / 10 min, and further preferably 3 to 7 g / 10 min under the measurement conditions of 230°C and a load of 2.16 kgf (21.2 N).

[0317] The number average molecular weight of the styrene elastomer (D3) is not particularly limited, but is preferably 10,000 to 500,000, more preferably 50,000 to 350,000, and further preferably 100,000 to 200,000.

[0318] Examples of the (D) elastomer other than the conjugated diene polymer (D1), the modified conjugated diene polymer (D2) and the styrene elastomer (D3) include polyolefin resins, polyphenylene ether resins, polyester resins, polyamide resins and polyacrylic resins.

[0319] ((D) Elastomer content)

[0320] When the resin composition of the present embodiment contains (D) elastomer, the content of the (D) elastomer is not particularly limited, but is preferably 10 to 80% by mass, more preferably 30 to 70% by mass, and further preferably 50 to 60% by mass, relative to the total amount (100% by mass) of the resin components in the resin composition of the present embodiment.

[0321] When the content of the elastomer (D) is at least the above lower limit, more excellent dielectric properties tend to be easily obtained. On the other hand, when the content of the elastomer (D) is at most the above upper limit, more excellent heat resistance tends to be easily obtained.

[0322] The total content of one or more selected from the conjugated diene polymer (D1), the modified conjugated diene polymer (D2) and the styrene-based elastomer (D3) is not particularly limited, but is preferably 60 to 100 mass %, more preferably 80 to 100 mass %, and even more preferably 90 to 100 mass % relative to the total amount (100 mass %) of the elastomer (D), from the viewpoint of dielectric properties and conductor adhesion.

[0323] From the viewpoint of dielectric properties and compatibility, the elastomer (D) preferably contains at least one selected from the group consisting of a conjugated diene polymer (D1) and a modified conjugated diene polymer (D2), and a styrene-based elastomer (D3).

[0324] When the elastomer (D) contains one or more selected from a conjugated diene polymer (D1) and a modified conjugated diene polymer (D2), and a styrene-based elastomer (D3), the ratio of the total content of the conjugated diene polymer (D1) and the modified conjugated diene polymer (D2) to the content of the styrene-based elastomer (D3) [[(D1) + (D2)] / (D3)] is not particularly limited, but is preferably 0.1 to 5, more preferably 0.2 to 1, and even more preferably 0.3 to 0.7 from the viewpoint of dielectric properties and compatibility.

[0325] <(E) Curing accelerator>

[0326] The resin composition of the present embodiment further contains (E) a curing accelerator.

[0327] The resin composition of the present embodiment contains the (E) curing accelerator, whereby the curability is improved, and there is a tendency that more excellent dielectric properties, heat resistance, and conductor adhesion are easily obtained.

[0328] (E) The curing accelerator may be used alone or in combination of two or more.

[0329] From the viewpoint of efficiently forming the chemical bond of the resin component during heating, as (E) curing accelerator, it is preferred to include a radical polymerization initiator. The radical polymerization initiator plays a role as a polymerization initiator for free radical polymerization, and when exposed to energy such as light and heat, it decomposes into a substance with unpaired electrons. As the radical polymerization initiator, organic peroxides, inorganic peroxides, azo compounds, etc. described later can be cited, preferably organic peroxides.

[0330] Examples of the curing accelerator (E) include acidic catalysts such as p-toluenesulfonic acid; amine compounds such as triethylamine, pyridine, tributylamine, and dicyandiamide; imidazole compounds such as methylimidazole, phenylimidazole, and 1-cyanoethyl-2-phenylimidazole; isocyanate-masked imidazole compounds such as an addition reaction product of hexamethylene diisocyanate resin and 2-ethyl-4-methylimidazole; tertiary amine compounds; quaternary ammonium compounds; phosphorus compounds such as triphenylphosphine; diisopropyl peroxide, 2,5-dimethyl-2,5-bis(tert-butyl)pyrrolidone; Organic peroxides such as tert-butylperoxy)hex-3-yne, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, tert-butylperoxyisopropyl monocarbonate, 1,3-di(tert-butylperoxyisopropyl)benzene; inorganic peroxides such as potassium persulfate, sodium persulfate, ammonium persulfate; azo compounds such as 2,2'-azobisisobutyronitrile, 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(4-methoxy-2'-dimethylvaleronitrile); carboxylates of manganese, cobalt, zinc, etc.

[0331] Among them, from the viewpoint of the curing accelerating effect and storage stability, imidazole compounds, isocyanate-masked imidazole compounds, organic peroxides, and carboxylates are preferred, and isocyanate-masked imidazole compounds and organic peroxides are more preferred.

[0332] When the resin composition of the present embodiment contains (E) a curing accelerator, the content of the (E) curing accelerator is not particularly limited, and is preferably 0.1 to 15 parts by mass, more preferably 1 to 10 parts by mass, and further preferably 4 to 8 parts by mass, relative to the total amount (100 parts by mass) of the (A) thermosetting resin and the (B) reactive liquid compound.

[0333] When the content of the curing accelerator (E) is at least the above lower limit, a sufficient curing acceleration effect tends to be easily obtained. On the other hand, when the content of the curing accelerator (E) is at most the above upper limit, storage stability tends to be further improved.

[0334] When the resin composition of the present embodiment contains a free radical polymerization initiator as the (E) curing accelerator, the content of the free radical polymerization initiator is not particularly limited, and is preferably 0.05 to 7 parts by mass, more preferably 0.5 to 5 parts by mass, and further preferably 2 to 4 parts by mass, relative to the total amount (100 parts by mass) of the (A) thermosetting resin and the (B) reactive liquid compound.

[0335] If the content of the radical polymerization initiator is above the lower limit, sufficient curing acceleration effect is easily obtained and the generation of volatile components is more easily suppressed. In addition, if the content of the radical polymerization initiator is below the upper limit, storage stability tends to be better.

[0336] <Other ingredients>

[0337] The resin composition of the present embodiment may further contain one or more arbitrary components selected from resin materials other than the above-mentioned components, flame retardants, antioxidants, heat stabilizers, antistatic agents, ultraviolet absorbers, pigments, colorants, lubricants, organic solvents and additives other than these, as needed.

[0338] The above-mentioned optional components may be used alone or in combination of two or more.

[0339] The content of the above-mentioned optional components in the resin composition of the present embodiment is not particularly limited, and may be used as needed within a range that does not inhibit the effects of the present embodiment.

[0340] In addition, the resin composition of the present embodiment may not contain the above-mentioned arbitrary components depending on the desired performance.

[0341] <Thickness of Resin Layer>

[0342] The thickness of the resin layer is not particularly limited, but is preferably 5 to 1,000 μm, more preferably 10 to 500 μm, further preferably 20 to 200 μm, further preferably 30 to 100 μm, and particularly preferably 40 to 70 μm.

[0343] When the thickness of the resin layer is greater than or equal to the above lower limit, the embedding property of the circuit tends to be more favorable. In addition, when the thickness of the resin layer is less than or equal to the above upper limit, the wiring density tends to be more appropriately increased.

[0344] <Solvent Content of Resin Layer>

[0345] The content of the organic solvent in the resin layer is preferably 2 mass % or less, more preferably 1 mass % or less, further preferably 0.5 mass % or less, and may be 0 mass % relative to the total amount of the resin layer (100 mass %).

[0346] When the content of the organic solvent in the resin layer is within the above range, the amount of the organic solvent volatilized during heat curing tends to be easily suppressed sufficiently.

[0347] <Mass reduction rate of resin layer at 170°C>

[0348] The mass reduction rate of the resin layer when heated and dried at 170° C. for 30 minutes in an air atmosphere [hereinafter sometimes referred to as “170° C. mass reduction rate”] is preferably 2.0 mass % or less, more preferably 1.5 mass % or less, further preferably 1.0 mass % or less, and may be 0 mass %.

[0349] When the mass reduction rate at 170° C. is within the above range, the amount of volatile components during heat curing tends to be easily suppressed.

[0350] The mass reduction rate at 170° C. can be measured by the method described in Examples.

[0351] <Dielectric Properties of Cured Resin Layer>

[0352] The relative dielectric constant (Dk) of the cured product of the resin layer at 10 GHz may be less than 3.0, less than 2.9, or less than 2.8. The smaller the relative dielectric constant (Dk), the better. The lower limit is not particularly limited. Considering the balance with other physical properties, it may be, for example, 2.4 or more, or 2.5 or more.

[0353] The dielectric loss tangent (Df) of the cured product of the resin layer at 10 GHz may be less than 0.0030, less than 0.0025, or less than 0.0015. The smaller the dielectric loss tangent (Df), the better. The lower limit is not particularly limited. Considering the balance with other physical properties, it may be, for example, 0.0010 or more, or 0.0015 or more.

[0354] It should be noted that the relative dielectric constant (Dk) and the dielectric loss tangent (Df) are values ​​based on the cavity resonator perturbation method, and more specifically, are values ​​measured by the method described in the Examples.

[0355] "Metal Foil"

[0356] Examples of the metal foil include copper foil, tin foil, tin-lead alloy foil, and nickel foil. Among them, copper foil is preferred. The copper foil preferably has a copper content of 95% by mass or more.

[0357] From the viewpoint of use in semiconductor packages, the metal foil is preferably based on the JIS standard (electrolytic copper foil for printed wiring boards: JIS C6512, rolled copper foil for printed wiring boards: JIS C6513) or the IPC standard (IPC 4562 standard Grade 1, 2, 3).

[0358] From the viewpoint of adhesion, the surface of the resin layer forming the metal foil may be roughened.

[0359] The roughening treatment can be performed by forming roughening particles on the surface of the metal foil.

[0360] As the roughening particles, for example, preferably, are electrodeposited particles composed of a single substance selected from copper, nickel, phosphorus, tungsten, arsenic, molybdenum, chromium, cobalt, and zinc, or electrodeposited particles composed of an alloy containing any one or more of these.

[0361] The roughening particles may be used alone or in combination of two or more.

[0362] In addition to the above-mentioned roughening treatment, the metal foil may be formed into secondary particles, tertiary particles, a rust-proof layer, a heat-resistant layer, etc., using, for example, a single substance selected from nickel, cobalt, copper and zinc, or an alloy containing any one or more of them.

[0363] In addition to the above-mentioned layers, the surface may be further subjected to a surface treatment such as a chromate treatment or a silane coupling treatment.

[0364] The thickness of the metal foil may be appropriately adjusted depending on the application of the metal foil with resin, etc., and is not particularly limited, but is preferably 0.1 to 40 μm, more preferably 1 to 30 μm, and further preferably 1.5 to 20 μm.

[0365] If the thickness of the metal foil is greater than the lower limit, the handleability of the metal foil with resin tends to be further improved. On the other hand, if the thickness of the metal foil is greater than the lower limit, it tends to be more suitable for increasing the wiring density.

[0366] The metal foil with resin of the present embodiment is suitable as, for example, a metal foil with resin for forming an insulating layer of a printed wiring board such as a multilayer printed wiring board or a metal foil with resin for semiconductor sealing of a semiconductor package.

[0367] <Method for producing metal foil with resin>

[0368] The metal foil with resin according to the present embodiment can be produced, for example, by applying a resin composition containing an organic solvent [hereinafter, the resin composition containing an organic solvent may be referred to as “resin varnish”] to a metal foil and then heating and drying the coating.

[0369] As the coating device for coating the resin varnish, for example, a coating device known to those skilled in the art such as a comma coater, a bar coater, a kiss coater, a roll coater, a gravure coater, a die coater, etc. These coating devices may be appropriately selected according to the film thickness to be formed.

[0370] The drying conditions after applying the resin varnish may be appropriately determined according to the content, boiling point, etc. of the organic solvent, and are not particularly limited.

[0371] For example, in the case of a resin varnish containing 40 to 60% by mass of an aromatic hydrocarbon solvent, the drying temperature is not particularly limited, but is preferably 50 to 200° C., more preferably 80 to 150° C., and even more preferably 100 to 130° C. from the viewpoint of productivity and making the resin composition appropriately B-staged.

[0372] In the case of the resin varnish, the drying time is not particularly limited, but is preferably 1 to 30 minutes, more preferably 2 to 15 minutes, and even more preferably 3 to 10 minutes from the viewpoint of productivity and making the resin composition appropriately B-staged.

[0373] [Manufacturing method of printed wiring board]

[0374] The method for producing a printed wiring board according to the present embodiment is a method for producing a printed wiring board using the metal foil with resin according to the present embodiment as an insulating material.

[0375] Hereinafter, one aspect of the method for manufacturing a printed wiring board according to the present embodiment will be described.

[0376] When manufacturing a printed wiring board using the resin-coated metal foil of the present embodiment, first, the resin-coated metal foil of the present embodiment is laminated on one or both surfaces of a circuit board so that the resin layer faces the circuit board side.

[0377] Examples of the circuit board include a glass epoxy substrate, a metal substrate, a polyester substrate, a polyimide substrate, a BT resin substrate, a thermosetting polyphenylene ether substrate, etc., on one or both sides of which a patterned conductor layer is formed.

[0378] Next, the circuit board on which the metal foil with the resin is laminated is heated to cure the resin layer, thereby forming an insulating layer including a cured product of the resin layer.

[0379] The heating temperature during heat curing is not particularly limited, but is preferably 100 to 300°C, more preferably 120 to 280°C, and further preferably 150 to 250°C.

[0380] The heating time during heat curing is not particularly limited, but is preferably 2 to 300 minutes, more preferably 5 to 200 minutes, and even more preferably 10 to 150 minutes.

[0381] By the above method, a printed wiring board is formed in which a circuit substrate, an insulating layer in which a circuit of the circuit substrate is embedded, and a metal foil are sequentially stacked.

[0382] The outermost metal foil can be removed by etching or can be used directly to form circuits.

[0383] After forming the insulating layer, holes can be opened as needed. Opening holes is a process of opening holes in the circuit substrate and the formed insulating layer by methods such as drilling, laser, plasma, or a combination thereof to form via holes (Japanese: via hole), through hole (Japanese: sur-hole), etc. Examples of lasers used for opening holes include carbon dioxide lasers, YAG lasers, UV lasers, excimer lasers, etc.

[0384] When the metal foil from the metal foil with resin is etched away, the exposed insulating layer can be roughened by an oxidant. In addition, when vias, through holes, etc. are formed between the insulating layer and the circuit substrate, the so-called "drill smear (Japanese: smear)" generated when forming them can be removed by an oxidant. Roughening and removal of drill smear can be performed at the same time.

[0385] When the outermost layer is a metal foil, a circuit may be formed on the metal foil, or the metal foil itself may be patterned to form a circuit, depending on the form of the metal foil.

[0386] In addition, when the outermost layer is an insulating layer, the circuit can be formed on the insulating layer after the above-mentioned roughening treatment is performed as needed.

[0387] When forming a conductor for forming a circuit, the conductor is preferably formed by a plating method such as an electroless plating method or an electrolytic plating method. Examples of metals for plating include copper, gold, silver, nickel, platinum, molybdenum, ruthenium, aluminum, tungsten, iron, titanium, chromium, and alloys containing at least one of these metal elements. Among them, copper and nickel are preferred, and copper is more preferred.

[0388] As a method for patterning the conductor layer and forming a circuit, for example, a subtractive method, a full additive method, a semi-additive process (SAP: SemiAdditive Process), a modified semi-additive process (m-SAP: modified Semi Additive Process) and the like can be used.

[0389] Furthermore, a multilayer printed wiring board can be manufactured by appropriately repeating necessary steps.

[0390] [Method for manufacturing semiconductor package]

[0391] The method for manufacturing a semiconductor package according to the present embodiment is a method for manufacturing a semiconductor package using the metal foil with resin according to the present embodiment as an insulating material.

[0392] The method for manufacturing a semiconductor package of the present embodiment may be, for example, a method for manufacturing a semiconductor package by mounting a semiconductor chip on a printed wiring board manufactured by the method for manufacturing a printed wiring board of the present embodiment. In this case, the semiconductor package manufactured by the manufacturing method of the present embodiment has a printed wiring board having an insulating material formed using a metal foil with a resin of the present embodiment. The mounting of the semiconductor chip on the printed wiring board may be performed by a known method.

[0393] In addition, the method for manufacturing a semiconductor package of the present embodiment may be, for example, a method for manufacturing a semiconductor package by sealing a semiconductor chip with a cured product of a resin layer of the metal foil with resin of the present embodiment. In this case, the semiconductor package manufactured by the manufacturing method of the present embodiment has an insulating sealing material formed using the metal foil with resin of the present embodiment.

[0394] Sealing of a semiconductor chip with a metal foil with resin can be performed, for example, by placing a resin layer of the metal foil with resin on the semiconductor chip, heating and melting the resin layer to embed the semiconductor chip, and then heating and curing the resin composition to seal the semiconductor chip.

[0395] Example

[0396] Hereinafter, the present embodiment will be described in detail with reference to examples, but the present embodiment is not limited to the following examples.

[0397] (Method for determining number average molecular weight)

[0398] The number average molecular weight is converted by gel permeation chromatography (GPC) based on a calibration curve using standard polystyrene. The calibration curve uses standard polystyrene: TSKstandard POLYSTYRENE (model: A-2500, A-5000, F-1, F-2, F-4, F-10, F-20, F-40) (manufactured by Tosoh Corporation, trade name), and is approximated by a cubic formula. The measurement conditions of GPC are shown below.

[0399] [GPC measurement conditions]

[0400] Device: High-speed GPC device HLC-8320GPC

[0401] Detector: UV-8320 ultraviolet absorption detector [manufactured by Tosoh Corporation]

[0402] Column: Guard column; TSK Guardcolumn SuperHZ-L + column; TSKgelSuperHZM-N + TSKgelSuperHZM-M + TSKgel SuperH-RC (all manufactured by Tosoh Corporation, trade names)

[0403] Column size: 4.6×20mm (guard column), 4.6×150mm (column), 6.0×150mm (reference column)

[0404] Eluent: Tetrahydrofuran

[0405] Sample concentration: 10mg / 5mL

[0406] Injection volume: 25μLL

[0407] Flow rate: 1.00mL / min

[0408] Measuring temperature: 40℃

[0409] [Manufacturing of modified conjugated diene polymer]

[0410] Production Example 1

[0411] Into a 2L glass flask container equipped with a thermometer, a reflux condenser and a stirring device, which can be heated and cooled, 33.8 parts by mass of 1,2-polybutadiene homopolymer (number average molecular weight = 1,200, vinyl content = 85% or more), 1.43 parts by mass of an aromatic bismaleimide resin containing an indane ring (a compound represented by the above general formula (A 1-4-1), number average molecular weight = 1,300), 0.0035 parts by mass of tert-butyl peroxyisopropyl carbonate and toluene as an organic solvent were added. Next, under a nitrogen atmosphere, the mixture was reacted at 90 to 100° C. while stirring for 5 hours, thereby obtaining a solution of a modified conjugated diene polymer (solid content concentration: 35% by mass). The number average molecular weight of the obtained modified conjugated diene polymer was 1,700.

[0412] In addition, for comprising 1,2-polybutadiene homopolymer before reaction start and the solution of the aromatic bismaleimide resin comprising indane ring and the solution after reaction, GPC is measured by the above method, the peak area from the aromatic bismaleimide resin comprising indane ring before and after reaction is obtained. Next, the vinyl modification rate of the aromatic bismaleimide resin comprising indane ring is calculated by following formula. It should be noted that the vinyl modification rate is equivalent to the reduction rate of the peak area from the aromatic bismaleimide resin comprising indane ring based on reaction.

[0413] Vinyl modification rate (%) = [(peak area derived from the aromatic bismaleimide resin containing an indane ring before the reaction) - (peak area derived from the aromatic bismaleimide resin containing an indane ring after the reaction)] × 100 / (peak area derived from the aromatic bismaleimide resin containing an indane ring before the reaction)

[0414] The vinyl modification ratio determined from the above formula was 40%.

[0415] [Manufacturing of resin composition]

[0416] Examples 1 to 12, Comparative Examples 1 to 2

[0417] The components listed in Table 1 were mixed with toluene in the amounts listed in Table 1, and then stirred and mixed while heating at 25° C. or 50 to 80° C., thereby preparing a resin composition having a solid content concentration of about 50% by mass. It should be noted that in Table 1, the unit of the amount of each component is part by mass, and in the case of a solution, it refers to part by mass in terms of solid content.

[0418] [Manufacture of copper foil with resin]

[0419] The resin composition obtained in each example was applied to one side of a low-profile copper foil (Mitsui Mining & Smelting Co., Ltd., trade name "3EC-VLP-18") having a thickness of 18 μm so that the thickness of the resin layer after drying was 50 μm. It should be noted that the resin composition was applied to the M surface of the low-profile copper foil. Then, the resin composition was heated and dried at 105° C. for 5 minutes, thereby making the resin composition in a B-stage state, and a copper foil with resin was produced.

[0420] [Manufacturing of resin sheets with copper foil on both sides]

[0421] The copper foil with resin obtained above was cut into a size of 250 mm in length and 250 mm in width, and two sheets were stacked with the resin layer sides facing each other, and then heated and pressed under the conditions of temperature 180°C, pressure 2.0 MPa, and time 60 minutes to solidify the resin layer, thereby producing a resin board with copper foil on both sides. The thickness of the resin board portion of the obtained resin board with copper foil on both sides was about 0.1 mm.

[0422] [Measurement and evaluation methods]

[0423] The resin compositions, copper foils with resin, and resin plates with copper foils on both sides obtained in the above Examples and Comparative Examples were used to perform various measurements and evaluations according to the following methods.

[0424] (1. Determination and evaluation method of melt viscosity)

[0425] The resin layer of the copper foil with resin obtained in each example was scraped off and press-formed at room temperature to produce a resin plate with a diameter of 10 mm and a thickness of 1 mm. Next, a rheometer (manufactured by TA Instruments, product name "DHR-20") was used to measure the melt viscosity under the conditions of a temperature range of 40 to 200°C, a heating rate of 5°C / min, and a weight of 0.5N, and the minimum melt viscosity of 80 to 130°C was obtained, and the evaluation was performed according to the following criteria. In the following criteria, A represents the best.

[0426] <Criteria for Determining Melt Viscosity>

[0427] A: Less than 5,000 Pa·s

[0428] B: 5,000 Pa·s or more and less than 7,500 Pa·s

[0429] C: 7,500 Pa·s or more and less than 10,000 Pa·s

[0430] D: 10,000 Pa·s or more

[0431] (2. Evaluation method of flexibility of resin layer)

[0432] The resin composition obtained in each example was coated on one side surface of a low-profile copper foil (manufactured by Mitsui Mining & Smelting Co., Ltd., trade name "3EC-VLP-18") having a thickness of 18 μm so that the thickness of the resin layer after drying became 150 μm. It should be noted that the resin composition is applied to the M surface of the low-profile copper foil. Then, the resin composition was heated and dried at 105 for 5 minutes, thereby making the resin composition in a B-stage state, and a copper foil with resin was prepared. The copper foil with resin was wound around a resin cylinder with a diameter of 85 mm at 25°C with the resin layer on the outside. The appearance of the wound resin layer was visually observed and evaluated according to the following criteria. Among the following criteria, A represents the best.

[0433] <Flexibility Criteria>

[0434] A: No cracks in the resin layer or peeling from the copper foil were observed.

[0435] B: Cracks in the resin layer or peeling from the copper foil were observed.

[0436] (3. Determination and evaluation method of linear expansion coefficient and glass transition temperature)

[0437] The resin plate with copper foil on both sides obtained in each example was immersed in a 10% by mass solution of ammonium persulfate (Mitsubishi Gas Chemical Company, Inc.) as a copper etching solution to remove the copper foil. The obtained resin plate was cut into a width of 0.4 mm and a length of 20 mm, and then dried at 105 for 1 hour to serve as a test piece. The test piece was clamped at both ends of the long side direction of the test piece with upper and lower clamps in a manner that the interval between the clamps was 10 mm. Next, a thermomechanical measuring device (TMA) (Seiko Instruments Co., Ltd., trade name "SS6100") was used to measure the dimensional change under the conditions of tensile mode, temperature range of 30 to 300, heating rate of 5°C / min, and load of 4g. The inflection point of the dimensional change relative to temperature was taken as the glass transition temperature, and the average value of the dimensional change per unit temperature of 30 to 150°C was taken as the linear expansion coefficient, and evaluated according to the following criteria. In the following criteria, A represents the best.

[0438] <Determination criteria of linear expansion coefficient>

[0439] A: less than 20ppm / K

[0440] B: 20ppm / K or more and less than 40ppm / K

[0441] C: 40ppm / K or more and less than 60ppm / K

[0442] D: 60ppm / K or more

[0443] <Criteria for Determining Glass Transition Temperature>

[0444] A: Above 180℃

[0445] B: less than 180

[0446] (Measurement and evaluation method of tensile elastic modulus at 4.25°C)

[0447] The resin plate with copper foil on both sides obtained in each example was immersed in a 10% by mass solution of ammonium persulfate (Mitsubishi Gas Chemical Company, Inc.) as a copper etching solution to remove the copper foil. The obtained resin plate was cut into a width of 10 mm and a length of 40 mm, and then dried at 105°C for 1 hour to serve as a test piece. The test piece was clamped at both ends of the long side direction of the test piece with upper and lower clamps in a manner that the interval between the clamps was 20 mm. Next, a small desktop testing machine (manufactured by Shimadzu Corporation, trade name "EZ-TEST") was used to obtain the tensile modulus of the above test piece under an environment of 25°C and a tensile speed of 2 mm / min. Five identical samples were made, and the tensile modulus was obtained under the same conditions as above, and the average value was used as the 25°C tensile modulus. Other detailed conditions and the calculation method of the tensile modulus were carried out in accordance with the international standard ISO5271 (1993). The obtained 25°C tensile modulus was evaluated according to the following judgment criteria. In the following criteria, A indicates the best.

[0448] <25℃ tensile modulus of elasticity determination criteria>

[0449] A: less than 1.5GPa

[0450] B: 1.5GPa or above

[0451] (5. Determination and evaluation method of peel strength)

[0452] After the copper foil of the resin plate with copper foil on both sides obtained in each example is processed into a straight line with a width of 5 mm by etching, it is dried at 105°C for 1 hour and used as a test piece. The formed straight copper foil is installed in a small desktop testing machine (manufactured by Shimadzu Corporation, trade name "EZ-TEST"), peeled in a 90° direction, and the peel strength of the copper foil is measured. The tensile speed when peeling the copper foil is set to 50 mm / min. The peel strength obtained is evaluated according to the following judgment criteria. In the following criteria, A represents the best.

[0453] <Determination Criteria of Peel Strength>

[0454] A: 0.5kN / m or more

[0455] B: 0.4kN / m or more and less than 0.5kN / m

[0456] (6. Measurement and evaluation method of relative dielectric constant (Dk) and dielectric loss tangent (Df))

[0457] The resin plate with copper foil on both sides obtained in each example was immersed in a 10 mass % solution of ammonium persulfate (Mitsubishi Gas Chemical Company, Inc.) as a copper etching solution to remove the copper foil. The obtained resin plate was cut into 2mm × 50mm, dried at 105°C for 1 hour, and used as a test piece. Next, according to the cavity resonator perturbation method, at an atmosphere temperature of 25°C, using a 10GHz band, the relative dielectric constant (Dk) and dielectric loss tangent (Df) of the above test piece were measured and evaluated according to the following criteria. In the following criteria, A represents the best.

[0458] <Criteria for determining relative dielectric constant (Dk)>

[0459] A: less than 2.8

[0460] B: 2.8 or above

[0461] <Criteria for determining dielectric loss tangent (Df)>

[0462] A: less than 0.0015

[0463] B: 0.0015 or more and less than 0.0025

[0464] C: 0.0025 or more and less than 0.0030

[0465] D: 0.0030 or more

[0466] (7.170℃ mass reduction rate determination method)

[0467] The resin layer of the copper foil with resin obtained in each example was scraped off, and the powder in the B-stage state obtained was used as an evaluation sample. Using the evaluation sample, the mass reduction rate when heated and dried at 170°C for 30 minutes in an atmospheric atmosphere [{(mass before heating - mass after heating at 170°C for 30 minutes) / (mass before heating)}×100] was taken as the mass reduction rate at 170°C. The results are shown in Table 1. It should be noted that in Table 1, "≤1.0" means that the mass reduction rate at 170°C is less than 1.0% by mass.

[0468] [Table 1]

[0469] Table 1

[0470]

[0471] It should be noted that the details of the components shown in Table 1 are as follows.

[0472] [(A) ingredient]

[0473] Maleimide resin A: an aromatic bismaleimide resin containing an indane ring represented by the general formula (A1-4-1): number average molecular weight = 1,300, solid at 25°C

[0474] Maleimide resin B: manufactured by Nippon Kayaku Co., Ltd., trade name "MIR-3000", a compound represented by the above general formula (A2-7), X a14 X in the above general formula (A2-8) a15 and X a16 is a methylene group and Ar a1 It is a divalent hydrocarbon group of 4,4'-biphenylene: number average molecular weight = 500, solid at 25°C

[0475] [(B) ingredient]

[0476] Bisphenol F epoxy resin: Epoxy equivalent: 155-165 g / eq, liquid at 25°C (viscosity at 25°C = 393 mPa·s), number average molecular weight: 300

[0477] 1,9-nonanediol diacrylate: liquid at 25°C (viscosity at 25°C = 8 mPa.s), molecular weight: 268.35

[0478] 1,10-Decanediol diacrylate: liquid at 25°C (viscosity at 25°C = 12 mPa·s), molecular weight: 282.38

[0479] Dioxanediol diacrylate: 2-[5-ethyl-5-[(acryloyloxy)methyl]-1,3-dioxane-2-yl]-2,2-dimethylethyl acrylate, liquid at 25°C (viscosity at 25°C = 310 mPa·s), molecular weight: 326.38

[0480] 1,9-nonanediol dimethacrylate: liquid at 25°C (viscosity at 25°C = 8 mPa·s), molecular weight: 296.4

[0481] 1,12-Dodecanediol dimethacrylate: liquid at 25°C (viscosity at 25°C = 11 mPa·s), molecular weight: 338.5

[0482] [(C) ingredient]

[0483] Silica: Spherical silica treated with aminosilane coupling agent, average particle size 0.5 μm

[0484] [(D) ingredient]

[0485] Modified conjugated diene polymer: the modified conjugated diene polymer obtained in Production Example 1, number average molecular weight 1,700

[0486] Styrene elastomer: hydrogenated styrene thermoplastic elastomer (styrene-ethylene-butylene-styrene copolymer), trade name "Tuftec H1221", styrene content = 12% by mass, MFR under the measurement conditions of 230, load 2.16 kgf = 4.5 g / 10 min, number average molecular weight = 170,000

[0487] Conjugated diene polymer: 1,2-polybutadiene homopolymer (number average molecular weight = 1,200, vinyl content = 85% or more)

[0488] [(E) ingredient]

[0489] Organic peroxide: 1,3-di(tert-butylperoxyisopropyl)benzene

[0490] Imidazole curing accelerator: Isocyanate-masked imidazole, manufactured by Daiichi Kogyo Seiyaku Co., Ltd., trade name "G-8009L"

[0491] According to the above results, the resin layer of the copper foil with resin of Examples 1 to 12 of the present embodiment has a low melt viscosity and high fluidity. In addition, it can be seen that the mass reduction rate of the resin layer of the copper foil with resin of Examples 1 to 12 at 170°C is less than 1.0 mass%, and the generation of volatile components during heat curing is suppressed. On the other hand, the resin layer of the copper foil with resin of Comparative Examples 1 and 2 has a high melt viscosity and poor fluidity.

[0492] Industrial Applicability

[0493] The resin layer of the copper foil with resin of the present embodiment is excellent in fluidity and can suppress the generation of volatile components during heat curing. Therefore, the copper foil with resin of the present embodiment is useful for printed wiring boards, semiconductor packages, and the like.

Claims

1. A metal foil with resin, comprising a metal foil and a resin layer containing a resin composition provided on one surface of the metal foil, wherein: The resin composition contains: (A) a thermosetting resin; (B) a compound which is liquid at 25° C., has a reactive group, and has a molecular weight of 1,000 or less; and (C) an inorganic filler.

2. The metal foil with resin according to claim 1, wherein The component (A) is one or more selected from the group consisting of a maleimide resin having one or more N-substituted maleimide groups and a derivative of the maleimide resin.

3. The metal foil with resin according to claim 2, wherein The maleimide resin having one or more N-substituted maleimide groups is a maleimide resin having two or more N-substituted maleimide groups and containing a condensed ring of an aromatic ring and an aliphatic ring in its molecular structure.

4. The metal foil with resin according to any one of claims 1 to 3, wherein The component (B) has, as the reactive group, one or more selected from the group consisting of an ethylenically unsaturated bond-containing functional group, an epoxy group, a hydroxyl group, a carboxyl group, and an amino group.

5. The metal foil with resin according to any one of claims 1 to 3, wherein The component (B) contains two or more of the reactive groups in one molecule.

6. The metal foil with resin according to any one of claims 1 to 3, wherein The component (B) is di(meth)acrylate.

7. The metal foil with resin according to any one of claims 1 to 3, wherein The content of the component (B) is 0.5% by mass to 20% by mass relative to 100% by mass of the total solid content of the resin composition.

8. The metal foil with resin according to any one of claims 1 to 3, wherein The metal foil is copper foil.

9. The metal foil with resin according to any one of claims 1 to 3, wherein The resin layer has a mass reduction rate of 2.0 mass % or less when heat-dried at 170° C. for 30 minutes in an air atmosphere.

10. A method for manufacturing a printed circuit board, wherein: An insulating material is formed using the metal foil with resin according to any one of claims 1 to 3.

11. A method for manufacturing a semiconductor package, wherein: An insulating material is formed using the metal foil with resin according to any one of claims 1 to 3.