Polyolefin copolymer, resin pellets, modifier for engineering plastic, engineering plastic composition, and resin molded article

By using polyolefin-based copolymers of olefin monomers with 2 to 8 carbon atoms and glycidyl-based monomers, the problem of insufficient dielectric properties of engineering plastics in the prior art was solved, and low dielectric constant and low dielectric loss were prepared Tangent polyolefin-based copolymers used in modifiers and are suitable for components of various components.

CN119095888APending Publication Date: 2024-12-06SUMITOMO CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380036598.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-05-19
Filing Date
2023-05-10
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The prior art is difficult to obtain polyolefin-based copolymers with low dielectric constant and low dielectric loss tangent in engineering plastics, and there is a problem of insufficient dielectric performance in the application of modifiers.

Method used

Polyolefin-based copolymers composed of olefin monomers with 2 to 8 carbon atoms and monomers with glycidyl groups were prepared by free radical initiator polymerization or emulsion polymerization, and the monomer ratio was controlled to achieve low dielectric constant and Engineering plastic composition with low dielectric loss tangent.

Benefits of technology

The engineering plastic composition with low dielectric constant and low dielectric loss tangent is successfully provided, suitable for modifiers, improved dielectric properties, suitable for components of automotive and electrical/electronic components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005102658680000041
    Figure BDA0005102658680000041
  • Figure BDA0005102658680000042
    Figure BDA0005102658680000042
  • Figure BDA0005102658680000181
    Figure BDA0005102658680000181
Patent Text Reader

Abstract

The polyolefin copolymer has a main chain containing a monomer unit A derived from an olefin monomer having 2-8 carbon atoms and a monomer unit B having a glycidyl group, the main chain may further contain a monomer unit C derived from a (meth) acrylate or a vinyl ether, and the proportion of the monomer unit A is 94 mass% or more based on the mass of the olefin copolymer. The total proportion of the monomer units B and C is less than 6 mass%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a polyolefin copolymer, a resin particle, a modifier for engineering plastics, an engineering plastic composition and a resin molded body. Background Art

[0002] Modifiers that are used in combination with engineering plastics to improve or change various properties of engineering plastics have been known. For example, Patent Document 1 describes a resin composition comprising: (A) 5 to 95 parts by mass of a polyphenylene ether resin or a mixture of the polyphenylene ether resin and a polystyrene resin, (B) 95 to 5 parts by mass of a saturated polyester, and (C) 1 to 100 parts of a graft-modified polyolefin resin relative to 100 parts of (A) and (B), wherein the graft-modified polyolefin resin is prepared by preparing an aqueous suspension containing (a) 100 parts of a polyolefin resin, (b) 0.1 to 30 parts of a modifier containing a compound represented by a predetermined formula, or containing the compound and glycidyl methacrylate, or containing glycidyl methacrylate, (c) 0.1 to 500 parts of a vinyl monomer, and (d) 0.001 to 10 parts of a radical polymerization initiator relative to 100 parts of the total amount of (b) and (c), and impregnating (b) and (c) in the aqueous suspension into (a) and polymerizing.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Laid-Open No. 8-259798 Summary of the invention

[0006] Problems to be solved by the invention

[0007] One aspect of the present application relates to a polyolefin-based copolymer that, when used as a modifier for engineering plastics, can provide an engineering plastic composition having a low dielectric constant and a low dielectric loss tangent.

[0008] Means for solving problems

[0009] In several aspects of the present application, the following [1] to

[14] are provided.

[0010] [1] A polyolefin-based copolymer having a main chain comprising a monomer unit A derived from an olefin monomer having 2 to 8 carbon atoms and a monomer unit B having a glycidyl group,

[0011] The main chain may further contain monomer units C derived from (meth)acrylate or vinyl ether,

[0012] The ratio of the monomer unit A is 94% by mass or more, and the total ratio of the monomer unit B and the monomer unit C is less than 6% by mass, based on the mass of the polyolefin-based copolymer.

[0013] [2] The polyolefin copolymer according to [1], wherein

[0014] The monomer unit A is a monomer unit derived from ethylene, a monomer unit derived from an α-olefin, or a combination thereof.

[0015] [3] The polyolefin copolymer according to [1], wherein

[0016] The monomer unit A is a monomer unit derived from ethylene.

[0017] [4] The polyolefin copolymer according to any one of [1] to [3], wherein

[0018] The monomer unit B is a monomer unit derived from an unsaturated carboxylic acid glycidyl ester, a monomer unit derived from a glycidyl ether having an unsaturated group, or a combination thereof.

[0019] [5] The polyolefin copolymer according to any one of [1] to [3], wherein

[0020] The monomer unit B is a monomer unit derived from glycidyl (meth)acrylate.

[0021] [6] The polyolefin copolymer according to any one of [1] to [5], wherein

[0022] The ratio of the monomer unit B is 1% by mass or more based on the mass of the polyolefin-based copolymer.

[0023] [7] The polyolefin copolymer according to any one of [1] to [5], wherein

[0024] The proportion of the monomer unit C is less than 1% by mass based on the mass of the polyolefin-based copolymer.

[0025] [8] Resin pellets comprising the polyolefin copolymer described in any one of [1] to [7].

[0026] [9] A modifier for engineering plastics, comprising the polyolefin copolymer described in any one of [1] to [7].

[0027]

[10] An engineering plastic composition comprising the polyolefin copolymer according to any one of [1] to [7] and an engineering plastic.

[0028]

[11] The engineering plastic composition according to

[10] , which does not substantially contain polyethylene terephthalate resin.

[0029]

[12] A resin molded article comprising the engineering plastic composition according to

[10] or

[11] .

[0030]

[13] The resin molded article according to

[12] , which is a member of an automobile part.

[0031]

[14] The resin molded article according to

[12] , which is a member of an electric or electronic component.

[0032] Effects of the Invention

[0033] According to the present application, it is possible to provide a polyolefin-based copolymer that can provide an engineering plastic composition having a low dielectric constant and a low dielectric loss tangent when used as a modifier for engineering plastics. DETAILED DESCRIPTION

[0034] Several examples of the present application are described in detail below, but the present application is not limited to the following examples.

[0035] An example of a polyolefin copolymer is a copolymer having a main chain containing a monomer unit A derived from an olefin monomer having 2 to 8 carbon atoms and a monomer unit B having a glycidyl group. The polyolefin copolymer can be used as a resin pellet (resin composition) containing the polyolefin copolymer, or as a modifier for engineering plastics and the like.

[0036] The monomer unit A derived from an olefin monomer having 2 to 8 carbon atoms may be a monomer unit derived from ethylene, a monomer unit derived from an α-olefin, or a combination thereof, and may be a monomer unit derived from ethylene. Examples of α-olefins include linear olefins such as 1-butene, 1-pentene, 1-hexene, 1-heptene, and 1-octene; cyclic olefins such as norbornene, 5-methylnorbornene, and 1-methylnorbornene; and aromatic olefins such as styrene, methylstyrene, and divinylbenzene.

[0037] Based on the mass of the polyolefin copolymer, the proportion of monomer unit A (or the total proportion of monomer units derived from ethylene and monomer units derived from α-olefins) is 94% by mass or more, and can be 95% by mass or more, 96% by mass or more, 97% by mass or more, or 97.5% by mass or more. Based on the mass of the polyolefin copolymer, the proportion of monomer unit A (or the total proportion of monomer units derived from ethylene and monomer units derived from α-olefins) can be 99.9% by mass or less, 99% by mass or less, 98.5% by mass or less, or 98% by mass or less. Based on the mass of the polyolefin copolymer, the proportion of monomer unit A (or the total proportion of monomer units derived from ethylene and monomer units derived from α-olefins) can be 94 to 99.9% by mass or 95 to 99% by mass.

[0038] The monomer unit B derived from the monomer having a glycidyl group may be: a monomer unit derived from an unsaturated carboxylic acid glycidyl ester, a monomer unit derived from a glycidyl ether having an unsaturated group, or a combination thereof, or a monomer unit derived from an unsaturated carboxylic acid glycidyl ester. The monomer unit B is present at least in the main chain of the polyolefin copolymer. The monomer unit B may not be present at the end of the polyolefin copolymer.

[0039] The unsaturated carboxylic acid glycidyl ester from which the monomer unit B is derived may also be a compound represented by the following formula (1). 1 represents an alkenyl group having 2 to 18 carbon atoms, and the alkenyl group may have one or more substituents. Examples of the compound represented by formula (1) include glycidyl acrylate, glycidyl methacrylate, and glycidyl itaconate.

[0040] [Chemistry 1]

[0041]

[0042] The glycidyl ether having an unsaturated group from which the monomer unit B is derived may also be a compound represented by the following formula (2). In formula (2), R 2 represents an alkenyl group having 2 to 18 carbon atoms, which may have one or more substituents. X represents CH2-O (CH2 and R 2 Examples of the compound represented by the formula (2) include allyl glycidyl ether, 2-methylallyl glycidyl ether, and styrene p-glycidyl ether.

[0043] [Chemistry 2]

[0044]

[0045] Based on the mass of the polyolefin copolymer, the proportion of monomer unit B can be 0.1% by mass or more, 0.5% by mass or more, 1% by mass or more, 1.5% by mass or more, 2% by mass or more, 2.1% by mass or more, 2.2% by mass or more, or 2.3% by mass or more. Based on the mass of the polyolefin copolymer, the proportion of monomer unit B can be less than 6% by mass, 5.5% by mass or less, 5.3% by mass or less, 5% by mass or less, 4% by mass or less, 3.5% by mass or less, 3% by mass or less, 2.5% by mass or less, 2.4% by mass or less, 2.3% by mass or less, or 2.2% by mass or less. Based on the mass of the polyolefin copolymer, the proportion of monomer unit B can be 0.1% by mass or more and less than 6% by mass, 0.5-5.5% by mass, 1-5.5% by mass, 1.5-5.5% by mass, 2-5.5% by mass, or 2.2-5.3% by mass.

[0046] The mass ratio of monomer unit B to monomer unit A (the ratio of monomer unit B / the ratio of monomer unit A) may be 0.001 or more, 0.005 or more, 0.01 or more, 0.015 or more, or 0.02 or more. The mass ratio of monomer unit B to monomer unit A (the ratio of monomer unit B / the ratio of monomer unit A) may be 0.06 or less, 0.05 or less, 0.04 or less, 0.03 or less, or 0.025 or less. The mass ratio of monomer unit B to monomer unit A (the ratio of monomer unit B / the ratio of monomer unit A) may be 0.001 to 0.06 or 0.005 to 0.05.

[0047] The main chain of the polyolefin copolymer may or may not further contain a monomer unit C derived from (meth)acrylate or vinyl ether (excluding a monomer unit corresponding to monomer unit B). "(Meth)acrylate" means acrylate or methacrylate, and this also applies to similar compounds.

[0048] Examples of (meth)acrylates include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, and butyl (meth)acrylate. Examples of vinyl ethers include methyl vinyl ether, ethyl vinyl ether, propyl vinyl ether, and phenyl vinyl ether.

[0049] Based on the mass of the polyolefin copolymer, the proportion of monomer unit C may be 3% by mass or less, 2% by mass or less, 1% by mass or less, less than 1% by mass, 0.5% by mass or less, 0.1% by mass or less, 0.05% by mass or less, or 0.01% by mass or less. Based on the mass of the polyolefin copolymer, the proportion of monomer unit C may be 0% by mass.

[0050] Based on the mass of the polyolefin copolymer, the total ratio of monomer units B and monomer units C may be less than 6 mass%, 5.5 mass% or less, 5.3 mass% or less, 5 mass% or less, 4.5 mass% or less, 4 mass% or less, 3.5 mass% or less, 3 mass% or less, 2.7 mass% or less, 2.5 mass% or less, 2.4 mass% or less, 2.3 mass% or less, or 2.2 mass% or less. Based on the mass of the polyolefin copolymer, the total ratio of monomer units B and monomer units C may be 0.1 mass% or more, 0.5 mass% or more, 1 mass% or more, 1.5 mass% or more, 1.8 mass% or more, 2 mass% or more, 2.1 mass% or more, 2.2 mass% or more, or 2.3 mass% or more. The total ratio of monomer units B and monomer units C based on the mass of the polyolefin copolymer may be 0.1 mass % or more and less than 6 mass %, 0.5 to 5.5 mass %, 1 to 5.5 mass %, 1.5 to 5.5 mass %, 2 to 5.5 mass %, or 2.2 to 5.3 mass %.

[0051] The mass ratio of monomer unit C to monomer unit B (the ratio of monomer unit C / the ratio of monomer unit B) may be 0.1 or less, 0.05 or less, or 0.01 or less. The mass ratio of monomer unit C to monomer unit B (the ratio of monomer unit C / the ratio of monomer unit B) may be 0.

[0052] Examples of polyolefin copolymers include ethylene-glycidyl (meth)acrylate copolymers, ethylene-glycidyl (meth)acrylate-methyl (meth)acrylate copolymers, ethylene-glycidyl (meth)acrylate-ethyl (meth)acrylate copolymers, ethylene-glycidyl (meth)acrylate-n-propyl (meth)acrylate copolymers, ethylene-glycidyl (meth)acrylate-isopropyl (meth)acrylate copolymers, ethylene-glycidyl (meth)acrylate-n-butyl (meth)acrylate copolymers, ethylene-glycidyl (meth)acrylate-isobutyl (meth)acrylate copolymers, and ethylene-glycidyl (meth)acrylate-vinyl ether copolymers. The polyolefin copolymer may also be ethylene-glycidyl (meth)acrylate copolymers.

[0053] Polyolefin copolymers can be synthesized by various methods. For example, polyolefin copolymers can be produced by bulk polymerization, emulsion polymerization, solution polymerization, etc. using a free radical initiator. A typical polymerization method for synthesizing polyolefin copolymers is as follows: in the presence of a polymerization initiator that generates free radicals, a polymerization pressure of 500 kg / cm 2Under the above conditions, at a polymerization temperature of 40 to 300° C., an olefin monomer having 2 to 8 carbon atoms, a monomer having a glycidyl group, and, if necessary, a (meth)acrylate or vinyl ether are copolymerized. The polymerization pressure may be 1000 kg / cm 2 Above, can be 2000kg / em 2 The polymerization temperature may be 100 to 250° C., or 150 to 200° C. In order to copolymerize the olefin monomer having 2 to 8 carbon atoms, the monomer having a glycidyl group, and (meth)acrylate or vinyl ether as required randomly, the olefin monomer having 2 to 8 carbon atoms and the monomer having a glycidyl group are present at least in the main chain.

[0054] The melt flow rate (MFR) of the polyolefin-based copolymer can be 0.2 g / 10 min or more, 0.5 g / 10 min or more, 1 g / 10 min or more, 1.5 g / 10 min or more, 2 g / 10 min or more, 2.5 g / 10 min or more, 3 g / 10 min or more, 5 g / 10 min or more, 10 g / 10 min or more, 20 g / 10 min or more, 30 g / 10 min or more, 40 g / 10 min or more, or 43 g / 10 min or more. The melt flow rate (MFR) of the polyolefin copolymer may be 300 g / 10 minutes or less, 250 g / 10 minutes or less, 220 g / 10 minutes or less, 200 g / 10 minutes or less, 190 g / 10 minutes or less, 170 g / 10 minutes or less, 150 g / 10 minutes or less, 130 g / 10 minutes or less, 110 g / 10 minutes or less, 100 g / 10 minutes or less, 90 g / 10 minutes or less, or 85 g / 10 minutes or less. The MFR of the polyolefin copolymer can be measured under the conditions of a temperature of 190° C. and a load of 2.16 kgf in accordance with JIS K7210.

[0055] From the viewpoint of easily obtaining an engineering plastic composition with a low dielectric constant, the dielectric constant of the polyolefin copolymer may be 2.55 or less, 2.50 or less, 2.47 or less, 2.45 or less, or 2.43 or less. The dielectric constant of the polyolefin copolymer may also be 2.0 or more, 2.2 or more, or 2.3 or more. The dielectric constant of the polyolefin copolymer may also be 2.0 to 2.55, 2.2 to 2.50, or 2.3 to 2.47. The dielectric constant of the polyolefin copolymer can be measured by the method described in the examples described below.

[0056] From the viewpoint of being particularly easy to obtain an engineering plastic composition with a low dielectric loss tangent, the dielectric loss tangent of the polyolefin copolymer can be 0.012 or less, 0.010 or less, 0.0095 or less, 0.0080 or less, 0.0070 or less, 0.0060 or less, or 0.0055 or less. The dielectric loss tangent of the polyolefin copolymer can also be 0.001 or more, 0.002 or more, 0.003 or more, or 0.004 or more. The dielectric loss tangent of the polyolefin copolymer can also be 0.001 to 0.012, 0.002 to 0.010, or 0.003 to 0.0095. The dielectric loss tangent of the polyolefin copolymer can be measured by the method described in the examples described later.

[0057] Based on the total mass of the resin particles, the content of the polyolefin copolymer may be 80 mass % or more, 85 mass % or more, 90 mass % or more, or 95 mass % or more. Based on the total mass of the resin particles, the content of the polyolefin copolymer may be 100 mass %.

[0058] The resin particles may further contain additives such as a compatibilizer, an antioxidant, a heat stabilizer, an ultraviolet absorber, an anti-coloring agent, a plasticizer, a flame retardant, a plasticizer, a mold release agent, an antistatic agent, and a colorant.

[0059] The resin pellets can be obtained, for example, by a method including melt-kneading a mixture containing a polyolefin-based copolymer and additives added as needed.

[0060] Melt kneading can be performed using, for example, a twin-screw kneader or a Labo Plastomill. Examples of the twin-screw kneader include a co-rotating twin-screw kneading extruder.

[0061] The maximum temperature of the melt-kneaded mixture may be 50 to 350°C, 80 to 320°C, 100 to 300°C, 120 to 280°C, or 150 to 250°C.

[0062] The kneading time of melt kneading may be 1 second to 1800 seconds, 10 seconds to 1200 seconds, or 30 seconds to 600 seconds.

[0063] The resin particles can be used as a modifier for engineering plastics to improve various properties (e.g., impact resistance) of engineering plastics. An engineering plastic composition containing engineering plastics and a polyolefin copolymer (or modifier) ​​can be obtained, for example, by a method comprising the following steps: melt-kneading a mixture containing a polyolefin copolymer (or modifier) ​​and an engineering plastic. The engineering plastic composition can also contain a continuous phase containing engineering plastics and particles containing a polyolefin copolymer dispersed in the continuous phase.

[0064] Engineering plastics refer to plastics with a deflection temperature under load of 100°C or higher as measured by ASTM D648, a tensile strength of 50 MPa as measured by ASTM D638, and a flexural modulus of 2.4 GPa or higher as measured by ASTM D790. Plastics with a heat resistance of 150°C or higher are called special engineering plastics or super engineering plastics, but in this specification, special engineering plastics and super engineering plastics are also included in engineering plastics.

[0065] Examples of engineering plastics include polybutylene terephthalate (PBT), polyphenylene sulfide (PPS), polycarbonate, polyethylene terephthalate, liquid crystal polymers, polyethersulfone, polyamide, polyphthalamide, polyketone, polyetherketone, polyetheretherketone, polyacetal, and polysulfone. The engineering plastic composition may be substantially free of polyethylene terephthalate resin, and the content of polyethylene terephthalate may be less than 1% by mass based on the mass of the engineering plastic in the engineering plastic composition. The polyethylene terephthalate resin herein also includes a modified product in which a part of the monomer units derived from terephthalic acid is replaced by monomer units derived from dicarboxylic acids other than terephthalic acid.

[0066] The engineering plastic composition may further contain: other ingredients added in addition to the polyolefin copolymer (or modifier), resin components (excluding the resin components equivalent to the above-mentioned polyolefin copolymer), fillers, antioxidants, heat stabilizers, ultraviolet absorbers, anti-coloring agents, plasticizers, flame retardants, plasticizers, release agents, antistatic agents and colorants.

[0067] The resin component may also be an olefin copolymer without an epoxy group. The olefin copolymer may also be an ethylene-α-olefin copolymer having monomer units derived from ethylene and monomer units derived from α-olefins. Examples of olefin copolymers without an epoxy group include ethylene-1-butene copolymers, ethylene-1-hexene copolymers, ethylene-1-octene copolymers, ethylene-1-decene copolymers, and ethylene-(3-methyl-1-butene) copolymers.

[0068] The MFR of the resin component at a temperature of 190° C. and a load of 2.16 kgf may be 0.1 g / 10 min or more, 0.5 g / 10 min or more, or 1 g / 10 min or less, or 50 g / 10 min or less, or 20 g / 10 min or less, or 10 g / 10 min or less.

[0069] The density of the resin component can be 0.85g / cm 3 Above, 0.87g / cm 3 Above, or 0.89g / cm3 Above, it can also be 0.95g / cm 3 Below, 0.92g / cm 3 Below, or 0.90g / cm 3 the following.

[0070] The dielectric constant of the engineering plastic composition may be 2.96 or less, 2.95 or less, 2.94 or less, 2.93 or less, or 2.92 or less. The dielectric constant of the engineering plastic composition may be 2.0 or more, 2.2 or more, 2.3 or more, 2.4 or more, 2.5 or more, 2.6 or more, 2.7 or more, 2.8 or more, or 2.9 or more. The dielectric constant of the engineering plastic composition may also be 2.0 to 2.96, 2.2 to 2.96, or 2.3 to 2.96. The dielectric constant of the engineering plastic composition can be measured by the method described in the examples below.

[0071] The dielectric loss tangent of the engineering plastic composition may be 0.0060 or less, 0.0059 or less, 0.0058 or less, 0.0057 or less, 0.0056 or less, or 0.0055 or less. The dielectric loss tangent of the engineering plastic composition may be 0.001 or more, 0.002 or more, 0.003 or more, 0.004 or more, or 0.005 or more. The dielectric loss tangent of the engineering plastic composition may also be 0.001 to 0.0060 or 0.002 to 0.0059. The dielectric loss tangent of the engineering plastic composition can be measured by the method described in the examples below.

[0072] The MFR retention rate of the engineering plastic composition may be 50% or more, 70% or more, or 90% or more. The MFR retention rate of the engineering plastic composition may be 150% or less, 130% or less, 120% or less, or 110% or less. The MFR retention rate of the engineering plastic composition may be 50% to 150%, 70% to 130%, or 90% to 120%. The MFR retention rate of the engineering plastic composition means: the rate of change of the MFR of the engineering plastic composition after storage for 1 month to 6 months at room temperature relative to the MFR of the engineering plastic composition just after preparation (MFR of the engineering plastic composition after storage / MFR of the engineering plastic composition before storage), and can be measured by the method described in the examples described below.

[0073] The Izod impact strength of the engineering plastic composition at -30°C can be 2.8 kJ / m 2 Above, 2.9kJ / m 2 Above, 3.0kJ / m 2 Above, or 3.1kJ / m 2 The Izod impact strength of the engineering plastic composition at -30°C can be 5.0 kJ / m2 Below, 4.0kJ / m 2 Below, or 3.5kJ / m 2 The Izod impact strength of the engineering plastic composition at -30°C can be 2.8 to 5.0 kJ / m 2 2.8~4.0kJ / m 2 , or 2.8~3.5kJ / m 2 The Izod impact strength of the engineering plastic composition at -30°C can be measured by the method described in the examples below.

[0074] The flexural strength of the engineering plastic composition may be 74 MPa or more or 75 MPa or more. The flexural strength of the engineering plastic composition may be 90 MPa or less or 80 MPa or less. The flexural strength of the engineering plastic composition may be 74 to 90 MPa or 75 to 80 MPa. The flexural strength of the engineering plastic composition can be measured by the method described in the examples below.

[0075] The flexural modulus of the engineering plastic composition may be 2050 MPa or more or 2100 MPa or more. The flexural modulus of the engineering plastic composition may be 2300 MPa or less or 2200 MPa or less. The flexural modulus of the engineering plastic composition may be 2050 to 2300 MPa or 2050 to 2200 MPa. The flexural modulus of the engineering plastic composition can be measured by the method described in the examples below.

[0076] The HDT (heat deformation temperature) of the engineering plastic composition may be 59.5° C. or more or 60° C. or more. The HDT of the engineering plastic composition may be 80° C. or less, 70° C. or less, or 65° C. or less. The HDT of the engineering plastic composition may be 59.5 to 80° C. or 60 to 70° C. The HDT of the engineering plastic composition can be measured by the method described in the examples below.

[0077] Based on the total mass of the engineering plastic composition, the content of the polyolefin copolymer may be 1% by mass or more, 3% by mass or more, or 5% by mass or more. Based on the total mass of the engineering plastic composition, the content of the polyolefin copolymer may be 50% by mass or less, 40% by mass or less, 30% by mass or less, 20% by mass or less, or 10% by mass or less. Based on the total mass of the engineering plastic composition, the content of the polyolefin copolymer may be 1 to 50% by mass.

[0078] Based on the total mass of the engineering plastic composition, the content of the engineering plastic may be 50% by mass or more, 60% by mass or more, 70% by mass or more, or 80% by mass or more. Based on the total mass of the engineering plastic composition, the content of the engineering plastic may be 95% by mass or less or 90% by mass or less. Based on the total mass of the engineering plastic composition, the content of the engineering plastic may be 50 to 95% by mass.

[0079] The engineering plastic composition can be molded by any molding method such as injection molding, extrusion molding, vacuum molding, and hollow molding to obtain a resin molded body of the engineering plastic composition. The obtained resin molded body has a low dielectric constant and a low dielectric loss tangent, and can be, for example, a member of an automobile component or a member of an electrical / electronic component.

[0080] Example

[0081] The invention is described in detail below based on examples, but the present application is not limited to the following examples.

[0082] 1.Raw materials

[0083] The following preparations were performed as raw materials for preparing the polybutylene terephthalate resin composition: The polyolefin copolymer, engineering plastic, and other resin components were prepared in the form of resin pellets.

[0084] (A) Polyolefin copolymer

[0085] BF-2C (trade name, manufactured by Sumitomo Chemical Co., Ltd., random copolymer of 94 parts by mass of ethylene and 6 parts by mass of glycidyl methacrylate, MFR=3 g / 10 min, polymerization pressure: 1346 kg / cm 2 , polymerization temperature: 194℃)

[0086] BF-7L (trade name, manufactured by Sumitomo Chemical Co., Ltd., a random copolymer of 70 parts by mass of ethylene, 3 parts by mass of glycidyl methacrylate, and 27 parts by mass of methyl acrylate, MFR = 7 g / 10 min, polymerization pressure: 1804 kg / cm 2 , polymerization temperature: 191°C)

[0087] EGMA-1 (random copolymer of 97.8 parts by mass of ethylene and 2.2 parts by mass of glycidyl methacrylate, MFR = 3 g / 10 min, polymerization pressure: 1356 kg / cm 2 , polymerization temperature: 196℃)

[0088] EGMA-2 (a random copolymer of 97.7 parts by mass of ethylene and 2.3 parts by mass of glycidyl methacrylate, MFR = 43 g / 10 min, polymerization pressure: 1356 kg / cm2 , polymerization temperature: 195℃)

[0089] EGMA-3 (a random copolymer of 97.7 parts by mass of ethylene and 2.3 parts by mass of glycidyl methacrylate, MFR = 85 g / 10 min, polymerization pressure: 1356 kg / cm 2 , polymerization temperature: 195℃)

[0090] EGMA-4 (a random copolymer of 97.7 parts by mass of ethylene and 2.3 parts by mass of glycidyl methacrylate, MFR = 190 g / 10 min, polymerization pressure: 1356 kg / cm 2 , polymerization temperature: 195℃)

[0091] EGMA-5 (a random copolymer of 94.7 parts by mass of ethylene and 5.3 parts by mass of glycidyl methacrylate, MFR = 3 g / 10 min, polymerization pressure: 1346 kg / cm 2 , polymerization temperature: 195℃)

[0092] (B) Engineering Plastics

[0093] ·Polybutylene terephthalate (PBT): TORAYCON1401X06 (trade name, manufactured by Toray Co., Ltd., intrinsic viscosity: 1.74)

[0094] (C) Other resin components

[0095] EHR: FX201 (trade name, manufactured by Sumitomo Chemical Co., Ltd., ethylene-hexene copolymer, MFR = 2 g / 10 min, density: 0.898 g / cm 3 )

[0096] 2. Preparation of Formed Body A

[0097] (Example 1)

[0098] Using a vacuum press (IMC-19E6 model, manufactured by Imoto Seisakusho Co., Ltd.), EGMA-1 was heated at 190°C for 10 minutes and then cooled at 30°C for 5 minutes to produce a sheet-shaped molded body A having a thickness of 1.0 mm.

[0099] (Example 2)

[0100] A molded body A was prepared in the same manner as in Example 1 except that EGMA-2 was used instead of EGMA-1.

[0101] (Example 3)

[0102] A molded body A was produced in the same manner as in Example 1 except that EGMA-3 was used instead of EGMA-1.

[0103] (Example 4)

[0104] A molded body A was produced in the same manner as in Example 1 except that EGMA-4 was used instead of EGMA-1.

[0105] (Example 5)

[0106] A molded body A was produced in the same manner as in Example 1 except that EGMA-5 was used instead of EGMA-1.

[0107] (Comparative Example 1)

[0108] A molded body A was produced in the same manner as in Example 1 except that BF-2C was used instead of EGMA-1.

[0109] (Comparative Example 2)

[0110] A molded body A was prepared in the same manner as in Example 1 except that BF-7L was used instead of EGMA-1.

[0111] 3. Preparation of engineering plastic composition and molded bodies B to D

[0112] (Example 6)

[0113] At the hopper port of the barrel C1 of the twin-screw compounding extruder (KZW20TW, manufactured by Technovel), 90% by mass of polybutylene terephthalate (PBT) was fed from the main feeder, and 10% by mass of EGMA-1 was fed from the secondary feeder. The temperature of the nozzle head was set to 260°C, the number of revolutions of the screw was set to 300 rpm, and PBT and EGMA-1 were melt-mixed. The molten compound was discharged from the twin-screw extruder at a discharge rate of 5 kg / hour, and the molten compound was cut with a granulator to obtain resin pellets of an engineering plastic composition containing PBT. The resin pellets were injection molded using an injection molding machine (manufactured by Sumitomo Heavy Industries, Ltd., SE100EV) at a mold temperature of 80°C, a cylinder temperature of 260°C, and an injection speed of 15 mm / second to produce a sheet-shaped molded body B with a thickness of 3.2 mm and a sheet-shaped molded body C with a thickness of 6.4 mm. Furthermore, the resin pellets were heated and pressed by a vacuum press at 260° C. for 10 minutes and then cooled at 30° C. for 5 minutes to produce a sheet-like molded body D having a thickness of 1.0 mm.

[0114] (Example 7)

[0115] Molded bodies B to D were prepared in the same manner as in Example 6 except that EGMA-2 was used instead of EGMA-1.

[0116] (Example 8)

[0117] Molded bodies B to D were prepared in the same manner as in Example 6 except that EGMA-3 was used instead of EGMA-1.

[0118] (Example 9)

[0119] Molded bodies B to D were prepared in the same manner as in Example 6 except that EGMA-4 was used instead of EGMA-1.

[0120] (Example 10)

[0121] Molded bodies B to D were prepared in the same manner as in Example 6 except that EGMA-5 was used instead of EGMA-1.

[0122] (Comparative Example 3)

[0123] Molded bodies B to D were prepared in the same manner as in Example 6 except that BF-2C was used instead of EGMA-1.

[0124] (Comparative Example 4)

[0125] Molded bodies B to D were prepared in the same manner as in Example 6 except that BF-7L was used instead of EGMA-1.

[0126] (Comparative Example 5)

[0127] Molded articles B to D were produced in the same manner as in Example 6 except that 93.3% by mass of polybutylene terephthalate (PBT) was fed from the main feeder and 6.7% by mass of BF-2C was fed from the sub-feeder.

[0128] (Comparative Example 6)

[0129] Molded articles B to D were produced in the same manner as in Example 6 except that 97.5% by mass of polybutylene terephthalate (PBT) was fed from the main feeder and 2.5% by mass of BF-2C was fed from the sub-feeder.

[0130] (Comparative Example 7)

[0131] Molded articles B to D were produced in the same manner as in Example 6 except that 99% by mass of polybutylene terephthalate (PBT) was fed from the main feeder and 1% by mass of BF-2C was fed from the sub-feeder.

[0132] 4. Preparation of Engineering Plastic Composition and Molded Body E

[0133] (Example 11)

[0134] The temperatures of nine barrels C1 to C9 provided along the extrusion direction from the hopper side of the twin-screw kneading extruder were set as follows.

[0135] C1: 100℃

[0136] C2: 200℃

[0137] C3~C9:260

[0138] 80% by mass of PBT was fed from the main feeder, and 5% by mass of EGMA-1 and 15% by mass of FX201 (trade name, manufactured by Sumitomo Chemical Co., Ltd., ethylene-hexene copolymer (EHR), MFR=2 g / 10 min, density: 0.898 g / cm2) were fed from the sub-feeder into the hopper port of the barrel C1 of the twin-screw kneading extruder (KZW20TW, manufactured by Technovel Co., Ltd.). 3 ). The temperature of the nozzle head is set to 260°C, the number of screw revolutions is set to 300 rpm, and PBT, EGMA-1 and EHR are melt-kneaded. The molten kneaded product is discharged from the twin-screw extruder at a discharge rate of 5 kg / hour, and the molten kneaded product is cut with a granulator to obtain resin pellets of an engineering plastic composition containing PBT and EHR. The resin pellets are injection molded using an injection molding machine (manufactured by Sumitomo Heavy Industries, Ltd., SE100EV) at a mold temperature of 80°C, a cylinder temperature of 260°C, and an injection speed of 30 mm / second to produce a sheet-like molded body E with a thickness of 2.0 mm.

[0139] (Example 12)

[0140] A molded body E was produced in the same manner as in Example 11 except that EGMA-2 was used instead of EGMA-1.

[0141] (Example 13)

[0142] A molded body E was produced in the same manner as in Example 11 except that EGMA-3 was used instead of EGMA-1.

[0143] (Example 14)

[0144] A molded body E was produced in the same manner as in Example 11 except that EGMA-4 was used instead of EGMA-1.

[0145] (Comparative Example 8)

[0146] A molded body E was produced in the same manner as in Example 11 except that BF-2C was used instead of EGMA-1, the content of BF-2C was changed to 1.7 mass %, and the content of EHR was changed to 18.3 mass %.

[0147] (Comparative Example 9)

[0148] A molded body E was produced in the same manner as in Example 11 except that BF-7L was used instead of EGMA-1.

[0149] 5. Evaluation

[0150] [Evaluation of dielectric constant and dielectric loss tangent]

[0151] Test pieces of 64 mm in length, 64 mm in width and 1.0 mm in thickness were prepared from the molded body A and the molded body D. The dielectric constant and dielectric loss tangent at 1 GHz were measured by the volumetric method in an atmosphere of 23°C using the test pieces.

[0152] [MFR retention rate]

[0153] The resin pellets prepared in Examples 6 to 10 or Comparative Examples 3 to 7 are sealed in an aluminum bag, and the resin pellets sealed in the bag are stored at room temperature for more than 1 month. The storage period of the resin pellets prepared in Examples 6 to 9 and Comparative Example 3 is set to 6 months, the storage period of the resin pellets prepared in Example 10 is set to 2 months, and the storage period of the resin pellets prepared in Comparative Examples 4 to 7 is set to 1 month. The MFR of the resin pellets (engineering plastic composition) before and after storage is measured by a melt flow tester under the conditions of a temperature of 190°C and a load of 2.16 kgf. The rate of change of the MFR of the engineering plastic composition after storage relative to the MFR of the engineering plastic composition before storage is calculated from the measured MFR of the engineering plastic composition before and after storage.

[0154] [Izod impact test]

[0155] A notched test piece with a length of 63.5 mm, a width of 12.7 mm, and a thickness of 3.2 mm was prepared from the molded body B. The test piece was used to measure the Izod impact strength (kJ / m 2 ).

[0156] [Bending test]

[0157] A test piece with a length of 127 mm, a width of 12.7 mm, and a thickness of 3.2 mm was prepared from the formed body B, and the flexural strength (MPa) and flexural modulus (MPa) were measured by a flexural test in accordance with JIS-K7203 (ASTM-D-790) using a double-bending tester (RTF-1350-2M, manufactured by A&D Co., Ltd.) in an atmosphere of 23°C.

[0158] [HDT measurement]

[0159] A test piece having a length of 127 mm, a width of 12.7 mm, and a thickness of 6.4 mm was prepared from the molded product C, and the HDT (° C.) was measured in accordance with JIS K7197-1 and 2.

[0160] [Surface peeling test]

[0161] In the vicinity of the resin inlet in the molded body E, 100 squares were cut with a cutter with each square being 2 mm x 2 mm. A transparent tape (registered trademark, manufactured by Nichiban Co., Ltd.) was attached to the cut positions. The transparent tape was peeled off with force, and the number of peeled squares (peeled pieces) among the 100 squares was measured. The fewer the number of peeled squares, the better the appearance of the molded body.

[0162] [Table 1]

[0163]

[0164] [Table 2]

[0165]

[0166] [Table 3]

[0167]

[0168] [Table 4]

[0169]

Claims

1. A polyolefin copolymer having a main chain, wherein the main chain comprises a monomer unit A derived from an olefin monomer having 2 to 8 carbon atoms and a monomer unit B having a glycidyl group, The main chain optionally also contains monomer units C derived from (meth)acrylates or vinyl ethers, The ratio of the monomer unit A is 94% by mass or more, and the total ratio of the monomer unit B and the monomer unit C is less than 6% by mass, based on the mass of the polyolefin-based copolymer.

2. The polyolefin copolymer according to claim 1, wherein The monomer unit A is a monomer unit derived from ethylene, a monomer unit derived from an α-olefin, or a combination thereof.

3. The polyolefin copolymer according to claim 1, wherein The monomer unit A is a monomer unit derived from ethylene.

4. The polyolefin copolymer according to claim 1, wherein The monomer unit B is a monomer unit derived from an unsaturated carboxylic acid glycidyl ester, a monomer unit derived from a glycidyl ether having an unsaturated group, or a combination thereof.

5. The polyolefin copolymer according to claim 1, wherein The monomer unit B is a monomer unit derived from glycidyl (meth)acrylate.

6. The polyolefin copolymer according to claim 1, wherein The ratio of the monomer unit B is 1% by mass or more based on the mass of the polyolefin-based copolymer.

7. The polyolefin copolymer according to claim 1, wherein The proportion of the monomer unit C is less than 1% by mass based on the mass of the polyolefin-based copolymer. 8 . Resin pellets comprising the polyolefin-based copolymer according to claim 1 . 9 . A modifier for engineering plastics, comprising the polyolefin-based copolymer according to claim 1 .

10. An engineering plastic composition comprising: The polyolefin copolymer according to any one of claims 1 to 7, and Engineering plastics.

11. The engineering plastic composition according to claim 10, which does not substantially contain polyethylene terephthalate resin.