Liquid composition, prepreg, metal base with resin, wiring board and silica particles

By using the combination of silica particles with specific characteristics and the thermosetting resin, the problem of insufficient adhesion and toughness of the metal substrate layer during curing is solved, and excellent cured and prepreg performance is achieved, thereby suppressing the suppression of The wall attachment and bubble are improved, and the dispersion and operability are improved.

CN119095918APending Publication Date: 2024-12-06AGC INC +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380036371.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-28
Filing Date
2023-04-21
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The conventional liquid compositions are insufficient to the adhesion and toughness of the metal base layer during curing, and there are problems with the dispersion and operability of the silica particles, making it difficult to effectively suppress the foaming of the attached walls and the composition.

Method used

Silica particles with water vapor adsorption and moisture-keeping variable amounts within a specific range are used to form excellent cured substances and pre-impregnation by adjusting the particle size, charge amount and powder dynamic friction angle of the silica particles. The material can inhibit the wall attachment of silica particles and the foaming of the composition, and improve its dispersion.

Benefits of technology

The cured product with excellent adhesion and high toughness to the metal base layer is achieved, and the wall attachment of the silica particles and the foaming of the composition is suppressed, and the dispersion and operability of the liquid composition are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005101753200000261
    Figure BDA0005101753200000261
  • Figure BDA0005101753200000271
    Figure BDA0005101753200000271
  • Figure BDA0005101753200000281
    Figure BDA0005101753200000281
Patent Text Reader

Abstract

A liquid composition containing a thermosetting resin and silica particles, the silica particles being (1) having a specific water vapor adsorption amount and moisture retention variation amount, or (2) having a specific charge amount and d50, or (3) having a specific powder friction angle, d50 and aggregation state; a prepreg using the liquid composition; a metal substrate with a resin; and a wiring board. And silica particles used in the liquid composition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a liquid composition, a prepreg, a metal substrate with a resin, a wiring board, and silica particles. Background Art

[0002] A liquid composition containing a thermosetting resin and silica particles is used to manufacture an electrical insulating layer of a metal-clad laminate that can be processed into a printed wiring board (see Patent Documents 1 and 2). Specifically, a metal-clad laminate having a semi-cured product of the liquid composition laminated on the surface of a metal substrate layer as an electrical insulating layer; a metal-clad laminate having a glass cloth impregnated with a liquid composition as an electrical insulating layer and laminated on the surface of a metal substrate layer. In recent years, the electrical insulating layer of a printed wiring board has been required to have higher properties such as a low dielectric constant, a low dielectric loss tangent, a low linear expansion coefficient, and toughness.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2013-212956

[0006] Patent Document 2: Japanese Patent Application Publication No. 2015-36357 Summary of the invention

[0007] Problem that the invention aims to solve

[0008] On the other hand, from the perspective of reliability of wiring boards, etc., for the liquid composition used to form an electrical insulating layer such as glass cloth impregnated with a liquid composition or a liquid composition, excellent adhesion to the metal substrate layer when forming a cured product is also required. In particular, in recent years, the miniaturization of wiring boards and the low roughness of metal substrate layers have been promoted, and for liquid compositions, cured products thereof and prepregs, further excellent adhesion of cured products to metal substrate layers is required. However, the previously known liquid compositions, cured products thereof and prepregs have room for improvement in the above-mentioned adhesion.

[0009] The problem to be solved by one embodiment of the present disclosure is to provide: a liquid composition and a prepreg capable of forming a cured product having excellent adhesion to a metal substrate layer. The problem to be solved by one embodiment of the present disclosure is to provide: a metal substrate with a resin and a wiring board having excellent adhesion to a metal substrate layer from a cured product of a liquid composition. The problem to be solved by one embodiment of the present disclosure is to provide: silica particles for forming a prepreg having excellent adhesion to a metal substrate layer when mixed with a liquid composition containing a thermosetting resin to form a cured product.

[0010] Furthermore, in recent years, various properties have been required of an electrical insulating layer included in a printed wiring board, and excellent toughness is required as one of them.

[0011] The problem to be solved by one embodiment of the present disclosure is to provide: a liquid composition and a prepreg capable of forming a cured product with excellent toughness. The problem to be solved by one embodiment of the present disclosure is to provide: a metal substrate with a resin and a wiring board comprising the above-mentioned liquid composition capable of forming a cured product with excellent toughness, a semi-cured product, a prepreg, or a cured product thereof. The problem to be solved by one embodiment of the present disclosure is to provide: silica particles for forming a prepreg capable of forming a cured product with excellent toughness when mixed with a liquid composition comprising a thermosetting resin.

[0012] In addition, when mixing and dispersing silica particles in a curable resin, in addition to the dispersibility of the silica particles, excellent mixing operability is also required. For example, when mixing silica particles in a curable resin, the adhesion of the silica particles to the wall of the container of the mixer (hereinafter also referred to as "wall adhesion") becomes a problem, or the foaming of the composition sometimes becomes a problem. On the other hand, to date, there is no understanding of a method for obtaining a liquid composition that can effectively suppress the wall adhesion of silica particles and the foaming of the composition and has excellent dispersibility of silica particles.

[0013] The problem to be solved by one embodiment of the present disclosure is to provide: a liquid composition in which the adhesion of silica particles and the foaming of the composition during mixing are suppressed and the dispersibility of the silica particles is excellent; a prepreg, a metal substrate with a resin, and a wiring board using the aforementioned liquid composition; and silica particles used in the aforementioned liquid composition.

[0014] Solutions for solving problems

[0015] Means for solving the above-mentioned problems include the following aspects.

[0016] <1> A liquid composition comprising a thermosetting resin and silicon dioxide particles, wherein the silicon dioxide particles have a water vapor adsorption amount of 0.01 to 10.00 cm2 at a relative water vapor pressure of 0.8 in a water vapor adsorption isotherm at 25°C. 3 / g, and further, when the water content by mass of the silica particles after standing at a temperature of 85°C and a relative humidity of 85% for 24 hours is set to A, and the water content by mass of the silica particles after standing at a temperature of 85°C and a relative humidity of 85% for 24 hours and further standing at a temperature of 25°C and a relative humidity of 50% for 24 hours is set to B, the water retention change amount calculated by (AB) / A×100 is less than 20%.

[0017] <2> according to <1> The liquid composition, wherein the specific surface area of ​​the silicon dioxide particles is 0.1 to 10.0 m 2 / g.

[0018] <3> according to <1> or <2> The liquid composition, wherein the silicon dioxide particles contain 30 to 1500 mass ppm of a metal element.

[0019] <4> according to <1> ~ <3> The liquid composition described in any one of the preceding claims, wherein the silica particles have a median particle size d50 of 1.0 to 10.0 μm.

[0020] <5> according to <1> ~ <4> The liquid composition described in any one of the above, wherein the content of the silica particles is 50 to 400 parts by mass based on 100 parts by mass of the thermosetting resin.

[0021] <6> A liquid composition comprises: a thermosetting resin; and silicon dioxide particles having an absolute value of charge of 0.7 to 200 nC / g and a median particle size d50 of 1.0 to 10.0 μm.

[0022] <7> according to <6> In the liquid composition, the silicon dioxide particles are particles whose surfaces are not treated.

[0023] <8> according to <6> or <7> The liquid composition, wherein the internal carbon content of the silica particles is 10% by mass or less.

[0024] <9> according to <6> ~ <8> The liquid composition described in any one of the preceding claims, wherein the silica particles have a median particle size d50 of more than 1.0 μm and not more than 5.0 μm.

[0025] <10> according to <6> ~ <9> The liquid composition described in any one of the above, wherein the content of the silica particles is 50 to 400 parts by mass based on 100 parts by mass of the thermosetting resin.

[0026] <11> A liquid composition comprising a thermosetting resin and silica particles, wherein the silica particles have a powder dynamic friction angle of 10 to 40 degrees and a median particle size d50 of 1.0 to 10.0 μm, and further, when the median particle size d50 of the silica particles after being dispersed in toluene is set as A1 and the median particle size d50 of the silica particles after being dispersed in toluene and further subjected to ultrasonic treatment is set as B1, the ratio of A1 to B1 (A1 / B1) is 1.0 to 50.0.

[0027] <12> according to <11> The liquid composition, wherein the angle of repose of the silicon dioxide particles is 25 to 50 degrees.

[0028] <13> according to <11> or <12> In the liquid composition, the content of the silica particles is 10 to 400 parts by mass based on 100 parts by mass of the thermosetting resin.

[0029] <14> according to <1> ~ <13> The liquid composition described above, wherein the thermosetting resin is an epoxy resin, a polyphenylene ether resin, or an o-divinylbenzene resin.

[0030] <15> according to <1> ~ <14> The liquid composition described above further comprises at least one solvent selected from the group consisting of toluene, cyclohexanone, methyl ethyl ketone and N-methylpyrrolidone.

[0031] <16> A prepreg comprising: <1> ~ <15> The liquid composition or a semi-cured product thereof as described above; and a fibrous substrate.

[0032] <17> according to <16> In the prepreg, the fibrous substrate contains a glass component.

[0033] <18> A metal substrate with resin, comprising: <1> ~ <15> The liquid composition or semi-cured product thereof, or <16> or <17> The prepreg; and a metal substrate layer.

[0034] <19> according to <18> The metal substrate with resin, wherein the metal substrate layer is copper foil.

[0035] <20> according to <19> In the metal substrate with resin, the maximum height roughness Rz of the surface on the copper foil, the liquid composition, the semi-cured product or the prepreg side is 2 μm or less.

[0036] <21> A wiring board comprising: <1> ~ <15> A cured product of the liquid composition described above; and a metal wiring.

[0037] <22> A silica particle is used for mixing with a liquid composition containing a thermosetting resin to form a prepreg, wherein the silica particle has a water vapor adsorption amount of 0.01 to 10.00 cm2 at a relative water vapor pressure of 0.8 in a water vapor adsorption isotherm at 25°C. 3 / g, and further, when the water content by mass of the silica particles after standing at a temperature of 85°C and a relative humidity of 85% for 24 hours is set to A, and the water content by mass of the silica particles after standing at a temperature of 85°C and a relative humidity of 85% for 24 hours and further standing at a temperature of 25°C and a relative humidity of 50% for 24 hours is set to B, the water retention change amount calculated by (AB) / A×100 is less than 20%.

[0038] <23> according to <22> The silicon dioxide particles have a specific surface area of ​​0.1 to 10.0 m 2 / g.

[0039] <24> A silica particle is used for mixing with a liquid composition containing a thermosetting resin to form a prepreg, wherein the absolute value of the charge of the silica particle is 0.7 to 200 nC / g and the median particle diameter d50 is 1.0 to 10.0 μm.

[0040] <25> according to <24> The silicon dioxide particles have an internal carbon content of 10% by mass or less.

[0041] <26> A silica particle is used to be mixed with a liquid composition containing a thermosetting resin to form a prepreg, wherein the silica particles have a powder dynamic friction angle of 10 to 40 degrees, a median particle size d50 of 1.0 to 10.0 μm, and a ratio of A1 to B1 (A1 / B1) of 1.0 to 50.0 when the median particle size d50 of the silica particles after being dispersed in toluene is set to A1 and the median particle size d50 of the silica particles after being dispersed in toluene and further subjected to ultrasonic treatment is set to B1.

[0042] <27> according to <26> The silica particles described above have a repose angle of 25 to 50 degrees.

[0043] Effects of the Invention

[0044] According to one embodiment of the present disclosure, there are provided: a liquid composition and a prepreg capable of forming a cured product having excellent adhesion to a metal substrate layer. According to one embodiment of the present disclosure, there are provided: a metal substrate with a resin and a wiring board having excellent adhesion to a metal substrate layer from a cured product of a liquid composition. According to one embodiment of the present disclosure, there are provided: silica particles for forming a prepreg having excellent adhesion to a metal substrate layer when mixed with a liquid composition containing a thermosetting resin to form a cured product.

[0045] According to one embodiment of the present disclosure, there are provided: a liquid composition and a prepreg capable of forming a cured product having excellent toughness. According to one embodiment of the present disclosure, there are provided: a metal substrate with a resin and a wiring board comprising the above-mentioned liquid composition capable of forming a cured product having excellent toughness, a semi-cured product, a prepreg or a cured product thereof. According to one embodiment of the present disclosure, there are provided: silica particles for forming a prepreg capable of forming a cured product having excellent toughness by mixing with a liquid composition comprising a thermosetting resin.

[0046] According to one embodiment of the present disclosure, provided are: a liquid composition in which the wall adhesion of silica particles and the foaming of the composition during mixing are suppressed and the dispersibility of silica is excellent; a prepreg, a metal substrate with a resin, and a wiring board using the liquid composition; and silica particles used in the liquid composition. DETAILED DESCRIPTION

[0047] The following describes the embodiments of the present disclosure in detail. However, the embodiments of the present disclosure are not limited to the following embodiments. In the following embodiments, the constituent elements (including element steps, etc.) are not required unless specifically indicated. The same is true for numerical values ​​and their ranges, which do not limit the embodiments of the present disclosure.

[0048] In the numerical range expressed by "to" in the present disclosure, the numerical values ​​described before and after "to" are respectively regarded as the minimum value and the maximum value.

[0049] In the present disclosure, each component may include a plurality of corresponding substances. When a plurality of corresponding substances exist in the composition, the content rate or content of each component refers to the total content rate or content of the plurality of substances present in the composition unless otherwise specified.

[0050] In the present disclosure, particles corresponding to each component may include multiple types. When multiple types of particles corresponding to each component exist in the composition, the particle size of each component refers to the value for the mixture of the multiple types of particles present in the composition unless otherwise specified.

[0051] In the present disclosure, “silicon dioxide particles” refers to a group of a plurality of silicon dioxide particles unless otherwise specified.

[0052] In the present disclosure, "the amount of water vapor adsorbed at a relative water vapor pressure of 0.8 in the water vapor adsorption isotherm at 25°C" is measured under the following conditions. It should be noted that in the present disclosure, the relative water vapor pressure refers to the ratio of the pressure of water vapor in adsorption equilibrium to the saturated vapor pressure of water vapor (pressure of water vapor in adsorption equilibrium / saturated vapor pressure of water vapor).

[0053] (Measurement conditions)

[0054] Device: BELSORP MINI (made by BEL Co., Ltd., Japan)

[0055] ·Determination principle: constant volume method

[0056] Adsorption temperature: 298K (24.85℃)

[0057] Adsorbed gas: water vapor

[0058] Pretreatment: 150℃, normal pressure (1.013×10 5 Dry for 1 hour at 400 Pa

[0059] · Target: 1.0g of silicon dioxide particles

[0060] In the present disclosure, the "variation in water retention" is calculated by the formula (AB) / A×100, when the water content of the silica particles based on the mass after standing for 24 hours in an environment of temperature 85°C and relative humidity 85% is set as A, and the water content of the silica particles based on the mass after standing for 24 hours in an environment of temperature 85°C and relative humidity 85% is set as B. The water content is measured by the following method: after placing in the above environment, the water content is measured by the Karl Fischer method (coulometric titration method) using a thermo-hygrostat model IG420 manufactured by Yamato Scientific Co., Ltd. or an apparatus equivalent thereto.

[0061] (Conditions of Karl Fischer method (coulometric titration))

[0062] ·Trace moisture measuring device (CA-200 model, manufactured by Mitsubishi Chemical Analytech Co., Ltd.)

[0063] · Moisture vaporization device (VA-200, manufactured by Mitsubishi Chemical Analytech Co., Ltd.)

[0064] Anolyte (HYDRANAL Coulomat AG-OVEN, manufactured by Hayashi Jun Chemical Industries, Ltd.)

[0065] Cathodic liquid (HYDRANAL Coulomat CG, manufactured by Hayashi Jun Chemical Industries, Ltd.)

[0066] Heating temperature: 200℃

[0067] Nitrogen flow rate: about 250ml / min

[0068] In the present disclosure, the "charge amount" is measured as follows. First, 10 g of silica particles are placed in an aluminum container (internal dimensions Φ42 mm, depth 70 mm), fixed to the sample rotation arm and installed. The left and right swing angles are set to 150 degrees on the left and 210 degrees on the right (the left and right swing speed is 540 deg / s), and 12 reciprocating times are recorded as one test unit (at the end of the 6 reciprocating times in the middle, 2 turns of powder falling rotation action are applied). Silica particles that are charged after friction stirring with 3 test units are put into a Faraday cage, and the charge of the silica particles is measured and converted into the charge per unit mass (charge of silica particles / amount of silica particles put in 10 g). The charge amount can be measured, for example, using a powder friction charge measuring device (manufactured by NanoSeeds Corporation, NS-K100 model).

[0069] In the present disclosure, the "internal carbon content" is determined as follows. The silica particles are heated in an atmospheric furnace at 500°C for 1 hour, the carbon components attached to the surface are removed, and then cooled to about 25°C. After the obtained silica particles are weighed, Sn particles are placed in a furnace heated to 1000°C to make them burn instantly, and the amount of carbon dioxide generated is analyzed by mass using a mass spectrometer (e.g., PerkinElmer, 2400II, CHN meter). The ratio (mass %) of carbon contained in the silica particles is taken as the internal carbon content.

[0070] In the present disclosure, the "median particle size d50" (hereinafter also referred to as "d50") is the volume-based cumulative 50% diameter of particles determined by a laser diffraction particle size distribution measuring device (e.g., "MT3300EXII" manufactured by MicrotracBEL Corp.). That is, the particle size distribution is measured by the laser diffraction / scattering method, and the total volume of the particles is set to 100% to obtain a cumulative curve, and the particle size at the point where the cumulative volume becomes 50% on the cumulative curve.

[0071] In the present disclosure, "10% particle diameter d10" (hereinafter also referred to as "d10") is the volume-based cumulative 10% diameter of particles determined by a laser diffraction particle size distribution measuring device (e.g., "MT3300EXII" manufactured by MicrotracBEL Corp.). That is, the particle size distribution is measured by the laser diffraction / scattering method, and the total volume of the particles is set to 100% to obtain a cumulative curve, and the particle size at the point where the cumulative volume from the small particle diameter side becomes 10% on the cumulative curve.

[0072] In the present disclosure, the “specific surface area” is determined by the BET method based on a nitrogen adsorption method using a specific surface area / pore distribution measuring apparatus (for example, “Tristar II” manufactured by Micromeritics).

[0073] In the present disclosure, the "powder dynamic friction angle" is an index of the fluidity of the powder, and the smaller the value, the higher the fluidity. The powder dynamic friction angle is measured using a powder layer shear tester (for example, "NS-S300" manufactured by Nano Seeds Corporation) in accordance with JIS Z8835 (2016).

[0074] In the present disclosure, "sphericity" is expressed as follows: for any 100 particles in a projection image of a photograph obtained by taking a scanning electron microscope (SEM) photograph, the maximum diameter (DL) and the short diameter (DS) orthogonal thereto are measured, and the average value of the ratio (DS / DL) of the minimum diameter (DS) to the maximum diameter (DL) is calculated.

[0075] In the present disclosure, the "dielectric loss tangent" and the "dielectric constant" are measured by a resonant method using a dedicated device (for example, "Vector Network Analyzer E5063A" manufactured by Keycom Co., Ltd.).

[0076] In the present disclosure, the content of metal elements in silica particles is measured by adding perchloric acid and hydrofluoric acid to silica particles, applying strong heat to remove silicon as a main component, and then measuring by inductively coupled plasma (ICP) emission spectrometry.

[0077] In the present disclosure, the term "viscosity" refers to the viscosity at 30 seconds measured at a shear rate of 1 rpm for 30 seconds at 25°C using a rotational rheometer (for example, modular rheometer Physica MCR-301 manufactured by Anton Paar).

[0078] In the present disclosure, the “thixotropic ratio” is calculated by dividing the viscosity measured at a rotation speed of 1 rpm by the viscosity measured at a rotation speed of 60 rpm using a rotational rheometer.

[0079] In the present disclosure, the "weight average molecular weight" is determined by gel permeation chromatography (GPC) in terms of polystyrene.

[0080] In the present disclosure, the "surface tension" is measured using a surface tensiometer on a solvent at 25°C according to the Wilhelmy method.

[0081] In this disclosure, "boiling point" refers to normal pressure (1.013×10 5 Pa) boiling point.

[0082] In the present disclosure, the “evaporation rate” is a relative evaporation rate when the evaporation rate of butyl acetate at 23° C. is set to 1.

[0083] In the present disclosure, a "liquid composition" refers to a composition that is liquid at 25°C.

[0084] In the present disclosure, "semi-cured product" refers to a cured product of a liquid composition in which an exothermic peak accompanying the curing of a thermosetting resin appears when a cured product of the liquid composition is measured by differential scanning calorimetry. In other words, a semi-cured product refers to a cured product in which uncured thermosetting resin remains.

[0085] In the present disclosure, the term "cured product" refers to a cured product in which the exothermic peak accompanying the curing of the thermosetting resin does not appear when the cured product of the liquid composition is measured by differential scanning calorimetry. In other words, the term "cured product" refers to a cured product in which no uncured thermosetting resin remains.

[0086] In the present disclosure, the maximum height roughness Rz is measured in accordance with JIS B 0601 (2013).

[0087] The liquid composition 1 of the present disclosure (hereinafter also referred to as the present composition 1) comprises a thermosetting resin and silica particles, wherein the silica particles have a water vapor adsorption amount at a relative water vapor pressure of 0.8 (hereinafter also referred to as the water vapor adsorption amount) of 0.01 to 10.00 cm in a water vapor adsorption isotherm at 25°C. 3 / g, and when the water content of the silica particles based on the mass after standing at a temperature of 85°C and a relative humidity of 85% for 24 hours is A, and the water content of the silica particles based on the mass after standing at a temperature of 85°C and a relative humidity of 85% for 24 hours and further standing at a temperature of 25°C and a relative humidity of 50% for 24 hours is B, the water retention variation (hereinafter also referred to as the water retention variation) calculated by (AB) / A×100 is 20% or less. In other words, the present composition 1 is a liquid thermosetting composition.

[0088] The liquid composition 2 of the present disclosure (hereinafter also referred to as the present composition 2) comprises: a thermosetting resin; and silica particles having an absolute value of charge of 0.7 to 200 nC / g and d50 of 1.0 to 10.0 μm. In other words, the present composition 2 is a liquid thermosetting composition.

[0089] The liquid composition 3 of the present disclosure (hereinafter also referred to as the present composition 3) comprises a thermosetting resin and silica particles, wherein the powder dynamic friction angle of the silica particles is 10 to 40 degrees, and d50 is 1.0 to 10.0 μm. In addition, when the median particle size d50 of the silica particles after being dispersed in toluene is set to A1, and the median particle size d50 of the silica particles after being dispersed in toluene and further subjected to ultrasonic treatment is set to B1, the ratio of A1 to B1 (A1 / B1) is 1.0 to 50.0. In other words, the present composition 3 is a liquid thermosetting composition.

[0090] This composition 1 can produce a cured product with excellent adhesion to the metal substrate layer. Its mechanism of action is uncertain, but it is roughly presumed as follows. This composition 1 contains silica particles having a specific range of water vapor adsorption and moisture retention variation. In other words, the silica particles in this composition 1 also allow polar groups such as silanol groups to be present on the particle surface, and their amount is limited, and are also considered to be silica particles with low moisture retention capacity, especially moisture retention capacity in high temperature areas. It is believed that the above-mentioned silica particles are easy to balance the interaction with the polar components contained in the composition and the polar parts of the thermosetting resin, and its liquid properties, especially uniform dispersibility, are easily improved. In addition, it is believed that the above-mentioned silica particles not only suppress their own moisture adsorption in the high temperature area where the thermosetting resin is cured, but also embody moisture discharge capacity due to their hydrophobicity. As a result, it is believed that in the present composition 1, a dense network is formed between the silica particles and the thermosetting resin, and the polar groups on the surface of the silica particles improve the adhesion to the metal substrate layer, so the adhesion of the cured product obtained from the present composition 1 to the metal substrate layer is improved. In addition, by keeping the variation of the moisture content of the silica particles within a specific range, the change in the moisture content caused by environmental changes can be reduced, and a uniformly dispersed state can be maintained. Hereinafter, the adhesion to the metal substrate layer is also referred to as adhesion.

[0091] The cured product obtained from the present composition 2 has excellent toughness. Its mechanism of action is uncertain, but it is roughly presumed as follows. The present composition 2 contains silica particles having a specific range of d50 and charge. Silica particles having a d50 of about 1.0 to 10.0 μm can impart low dielectric loss tangent, low specific dielectric constant, low linear expansion, etc. to the cured product, while on the other hand, there is room for improvement in improving the adhesion with the thermosetting resin. By making the charge of the silica particles 0.7 to 200 nC / g, the balance of the electrostatic interaction with the thermosetting resin in the present composition 2 is adjusted, and the uniform dispersibility of the silica particles and the thermosetting resin can be improved. Therefore, the adhesion of the cured product obtained from the present composition 2 can be improved. As a result, it is believed that the toughness of the cured product obtained from the present composition 2 is improved.

[0092] According to the present composition 3, a liquid composition is obtained which can suppress the adhesion of silica particles and the foaming of the composition during mixing and has excellent dispersibility of silica particles. The reason may not be clear, but it is considered as follows. It is believed that when a composition containing silica particles is mixed, the silica particles will aggregate and cause adhesion, or cause foaming of the composition accompanied by shearing. The inventors focused on the dynamic fluidity and aggregation state of the silica particles before mixing and conducted in-depth research and found that balancing them is effective for the adhesion of silica particles and the foaming of the composition. In the present composition 3, the powder dynamic friction angle of the silica particles is 10 to 40 degrees, and the silica particles have a high dynamic fluidity. In addition, in the present composition 3, the aforementioned ratio (A / B) is 1.0 to 50.0, and the aggregation of silica particles is suppressed, or is in a moderate aggregation state. It is believed that the adhesion of silica particles and the foaming of the composition are suppressed during mixing by balancing these dynamic fluidity and aggregation state, and the silica particles can be well dispersed by mixing.

[0093] From the viewpoint of suppressing aggregation of silica particles, the viscosity of the present composition 1, the present composition 2 and the present composition 3 measured at a rotation speed of 1 rpm is preferably 130 to 5000 mPa·s, more preferably 150 to 3000 mPa·s, further preferably 180 to 1500 mPa·s, and particularly preferably 200 to 1000 mPa·s.

[0094] From the viewpoint of the ease of storage and fluidity during use of the present composition 1, the present composition 2 and the present composition 3, the thixotropic ratio calculated by dividing the viscosity measured at a rotation speed of 1 rpm by the viscosity measured at a rotation speed of 60 rpm is preferably 3.0 or less, more preferably 2.5 or less, and further preferably 2.0 or less. The lower limit of the thixotropic ratio is not particularly limited, and can be 0.5 or more.

[0095] The present composition 1, the present composition 2 and the present composition 3 contain a thermosetting resin. For each composition, one thermosetting resin may be used, or two or more thermosetting resins may be used. As the thermosetting resin, epoxy resin, polyphenylene ether resin, polyimide resin, phenolic resin, o-divinylbenzene resin, etc. may be cited. From the viewpoints of adhesion, heat resistance, etc., the thermosetting resin is preferably an epoxy resin, a polyphenylene ether resin or an o-divinylbenzene resin. The thermosetting resin preferably contains a resin of at least one selected from the group consisting of phenyl and phenylene.

[0096] Examples of the epoxy resin include bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol S epoxy resin, alicyclic epoxy resin, phenol novolac epoxy resin, cresol novolac epoxy resin, bisphenol A novolac epoxy resin, diglycidyl ethers of polyfunctional phenols, and diglycidyl ethers of polyfunctional alcohols.

[0097] The polyphenylene ether resin may be a modified polyphenylene ether or an unmodified polyphenylene ether. From the viewpoint of adhesion, a modified polyphenylene ether is preferred. The modified polyphenylene ether has a polyphenylene ether chain or a substituent bonded to the end of the polyphenylene ether chain. The substituent preferably has a reactive group, more preferably a vinyl, (meth)acryloyloxy or epoxy group.

[0098] The hydrogen atoms of the phenylene group in the polyphenylene ether chain may be substituted with an alkyl group, an alkenyl group, an alkynyl group, a formyl group, an alkylcarbonyl group, an alkenylcarbonyl group or an alkynylcarbonyl group.

[0099] The weight average molecular weight of the thermosetting resin is preferably 1,000 to 7,000, more preferably 1,000 to 5,000, and even more preferably 1,000 to 3,000 from the viewpoint of adhesion, dielectric properties, and the like.

[0100] From the viewpoint of adhesion to a metal substrate layer or the like of a wiring board such as a prepreg obtained from the present composition 1, the present composition 2 or the present composition 3, the content of the curable resin in the present composition 1, the present composition 2 or the present composition 3 relative to the total mass of each composition is preferably 10 to 40% by mass, more preferably 15 to 35% by mass, and still more preferably 20 to 30% by mass.

[0101] The composition 1 contains water vapor adsorption of 0.01 to 10.00 cm 3 / g, and the water retention fluctuation is 20% or less.

[0102] In addition to the above-mentioned mechanism of action, in particular from the viewpoint of adhesion, the water vapor adsorption amount is preferably 1.00 to 9.00 cm 3 / g, more preferably 3.00 to 8.50 cm 3 / g.

[0103] In addition to the above-mentioned mechanism of action, in particular from the viewpoint of adhesion, the above-mentioned water retention variation is preferably 15% or less, and more preferably 10% or less. The lower limit of the water retention variation is not particularly limited, and may be 0%.

[0104] In the present composition 2, from the viewpoint of further improving the toughness of the cured product, the charge amount of the silica particles is preferably 1 to 100 nC / g, more preferably 1 to 50 nC / g, further preferably 1 to 30 nC / g, and particularly preferably 1 to 10 nC / g.

[0105] In addition, in the present composition 2, the value obtained by dividing the charge (nC / g) of the silica particles by the d50 (μm) of the silica particles is preferably 0.1 or more, more preferably 1 or more, and can be 1.5 or more, and can be 2 or more. In addition, the value obtained by dividing the charge of the silica particles by the d50 of the silica particles is preferably 5 or less, more preferably less than 5, and further preferably 4 or less. If the value obtained by dividing the charge of the silica particles by the d50 of the silica particles is within the aforementioned range, the charge of each silica particle becomes easy to concentrate in the range that balances the electrostatic repulsion between the particles and the interaction between the thermosetting resin and the silica particles, and the above-mentioned mechanism of action is easy to be more highly manifested.

[0106] In the present composition 1, in addition to the above-mentioned mechanism of action, from the viewpoint of highly balancing the physical properties of the present composition itself, such as adhesion, dispersion stability, and fluidity, and the physical properties of a cured product formed from the present composition, such as adhesion and low dielectric loss tangent, the d50 of the silica particles is preferably 0.5 to 20.0 μm, more preferably 1.0 to 10.0 μm, and further preferably more than 1.0 μm and 5.0 μm or less.

[0107] In the present composition 2, the d50 of the silica particles is 1.0 to 10.0 μm, and is preferably greater than 1.0 μm and less than 5.0 μm from the viewpoint of highly balancing the physical properties of the present composition itself, such as dispersion stability and fluidity, with the physical properties of the cured product formed by the present composition, such as high toughness, adhesion to the metal substrate layer, and low dielectric loss tangent.

[0108] In the present composition 3, the d50 of the silica particles is 1.0 to 10.0 μm. From the perspective of the above-mentioned mechanism of action, and in particular, from the viewpoint of better suppressing the adhesion of the silica particles to the wall during mixing and the foaming of the composition, and from the viewpoint of suppressing the aggregation of the silica particles, the d50 is preferably greater than 1.0 μm and less than 5.0 μm, more preferably 1.5 to 4.0 μm, and even more preferably 2.0 to 3.5 μm.

[0109] The d10 of the silica particles is preferably 0.5 to 5.0 μm, more preferably 1.0 to 3.0 μm, from the viewpoint of improving uniform dispersibility in the present composition 1, the present composition 2, and the present composition 3 and enhancing the interaction between the silica particles and the thermosetting resin, in addition to the above-mentioned mechanism of action.

[0110] From the viewpoint of improving uniform dispersibility in the present composition and enhancing the interaction between the silica particles and the thermosetting resin, the ratio of d50 to d10 (d50 / d10) is preferably greater than 1.0 and less than 5.0, more preferably 1.3 to 4.0, and further preferably 1.5 to 3.0.

[0111] The particle size distribution of the silica particles contained in the present composition 1, the present composition 2 or the present composition 3 is preferably unimodal. The unimodal particle size distribution of the silica particles can be confirmed by the presence of one peak in the particle size distribution by the laser diffraction / scattering method.

[0112] In the present composition 1, the specific surface area of ​​the silica particles is preferably 0.1 to 10.0 m2 from the viewpoint of achieving a higher balance between the physical properties of the present composition itself, such as adhesion, dispersion stability, and fluidity, and the physical properties of the cured product formed from the present composition, such as adhesion and low dielectric loss tangent, in addition to the above-mentioned mechanism of action. 2 / g, more preferably 0.3 to 3.0 m 2 / g, more preferably 0.8 to 2.0 m 2 / g.

[0113] In the present composition 2, the specific surface area of ​​the silica particles is preferably 0.3 to 3.0 m from the viewpoint of achieving a more balanced balance between the physical properties of the present composition itself, such as dispersion stability and fluidity, and the physical properties of the cured product formed from the present composition, such as high toughness, adhesion to the metal substrate layer, and low dielectric loss tangent. 2 / g, more preferably 0.8 to 2.0 m 2 / g.

[0114] In the present composition 3, the specific surface area of ​​the silica particles is preferably 0.1 to 5.0 m2 from the viewpoint of better suppressing the adhesion of the silica particles during mixing and the foaming of the composition, and suppressing the aggregation of the silica particles. 2 / g, more preferably 0.2 to 3.5 m 2 / g, more preferably 0.3 to 3.0 m 2 / g, particularly preferably 0.8 to 2.0 m 2 / g.

[0115] From the viewpoint of toughness of the cured product of the present composition 1, the present composition 2 or the present composition 3 and adhesion to the metal substrate layer, and particularly from the viewpoint of better suppressing adhesion of silica particles during mixing and foaming of the composition in the composition 3, and suppressing aggregation of silica particles, the product A of the specific surface area of ​​the silica particles and the d50 of the silica particles is preferably 2.7 to 5.0 μm·m 2 / g, more preferably 2.9 to 4.5 μm·m 2 / g. In addition, the product A is particularly preferably 4.0 μm·m 2 The silica particles within the above product A range are also considered to be highly solid spherical particles, and the above mechanism of action is more likely to be highly manifested. In this case, the product A can be 2.7 μm·m 2 / g or more, can be 2.9μm·m2 / g or above.

[0116] In Composition 3, the powder dynamic friction angle of the silica particles is 10 to 40 degrees, and preferably 20 to 40 degrees from the viewpoint of better suppressing the adhesion of the silica particles during mixing and the foaming of the composition, and suppressing the aggregation of the silica particles.

[0117] In composition 3, when d50 of the silica particles after being dispersed in toluene is defined as A1 and d50 after being dispersed in toluene and further subjected to ultrasonic treatment is defined as B1, the ratio of A1 to B1 (A1 / B1) (hereinafter also referred to as "ratio (A1 / B1)") is 1.0 to 50.0. From the viewpoint of better suppressing the adhesion of silica particles to the wall during mixing and the foaming of the composition, and from the viewpoint of suppressing the aggregation of silica particles, the ratio (A1 / B1) is preferably 30.0 or less, more preferably 10.0 or less, further preferably 5.0 or less, particularly preferably 3.0 or less, and most preferably 2.0 or less. The ratio (A1 / B1) is preferably 1.0 or more, and more preferably more than 1.0.

[0118] The ratio (A1 / B1) is an index of the degree of aggregation of the silica particles before mixing, and is specifically measured as follows. Using an ultrasonic irradiator (e.g., "PC-3" manufactured by Beckman Coulter), 5% by mass of silica particles in toluene are dispersed under the condition of irradiation time of 1 minute. The d50 of the silica particles before and after ultrasonic dispersion is measured to obtain the ratio (A1 / B1).

[0119] It should be noted that in the present disclosure, unless otherwise specified, the description of the particle size (particle size distribution, including d50, d10 and d50 / d10) of the silica particles by ultrasonic dispersion refers to the particle size measured by dispersing the silica particles in water and preparing a measurement solution by ultrasonic dispersion under the above conditions.

[0120] In Composition 3, the repose angle of the silica particles is preferably 25 to 50 degrees, and may be 20 to 40 degrees, from the viewpoint of better suppressing adhesion of the silica particles during mixing and foaming of the composition, and suppressing aggregation of the silica particles.

[0121] The angle of repose is defined as follows: after a powder sample is passed through a sieve with a diameter of 80 mm and an aperture of 710 μm while vibrating, it is quietly dropped from a funnel at a height of 160 mm onto a table with a diameter of 80 mm on a horizontal plane. The angle between the generatrix of the cone formed by the powder and the horizontal plane is measured, and the value is defined as the smaller the value for a powder with better fluidity. Here, the amount of powder dropped is set to allow it to drop until the angle of repose is substantially stable.

[0122] The shape of each silica particle contained in the silica particles is preferably spherical from the viewpoint of highly balancing the physical properties of the present composition 1, the present composition 2 or the present composition 3 itself, such as dispersion stability and fluidity, and the physical properties of the cured product formed by the present composition 1, the present composition 2 or the present composition 3, such as high toughness, adhesion to the metal substrate layer, and low dielectric loss tangent, in addition to the above-mentioned mechanism of action. From the same viewpoint, the sphericity of the spherical silica particles is preferably 0.75 or more, more preferably 0.90 or more, further preferably 0.93 or more, and particularly preferably 1.00. In addition, from the same viewpoint, the silica particles are preferably non-porous particles.

[0123] From the viewpoint of reducing transmission loss in a circuit when the metal substrate with resin is used as a printed wiring board, the dielectric loss tangent of the silica particles is preferably 0.0020 or less, more preferably 0.0010 or less, and further preferably 0.0008 or less at a frequency of 1 GHz.

[0124] From the same viewpoint, the dielectric constant of the silica particles is preferably 5.0 or less, more preferably 4.5 or less, and even more preferably 4.1 or less at a frequency of 1 GHz.

[0125] Each silica particle can be treated with a silane coupling agent. By treating the surface of the silica particles with a silane coupling agent, the residual amount of silanol groups on the surface is reduced, the surface is hydrophobized, moisture adsorption is suppressed, and dielectric loss can be improved. In addition, the affinity with the thermosetting resin in the present composition is improved, and the adhesion, dispersibility and strength of the resin film after being formed can be improved.

[0126] Examples of the silane coupling agent include aminosilane coupling agents, epoxysilane coupling agents, mercaptosilane coupling agents, silane coupling agents, and organic silazane compounds. The silane coupling agent may be used alone or in combination of two or more.

[0127] The amount of the silane coupling agent attached is preferably 0.01 to 5 parts by mass, more preferably 0.10 to 2 parts by mass, based on 100 parts by mass of the silica particles.

[0128] Whether the surface of the silica particles is treated with a silane coupling agent can be confirmed by detecting a peak generated by a substituent of the silane coupling agent by IR. Alternatively, the amount of the silane coupling agent attached can be measured by the amount of carbon.

[0129] On the other hand, from the viewpoint of enhancing the interaction between the silica particles and the thermosetting resin and improving the toughness of the cured product, the silica particles are preferably not surface-treated with a silane coupling agent or the like. In particular, particles not surface-treated with a silane coupling agent or the like (hereinafter also referred to as surface-untreated particles) are preferred in the present composition 2.

[0130] In particular, in the present composition 2, from the viewpoint of further improving the toughness of the cured product, the internal carbon content of the silica particles is preferably 10 mass % or less, more preferably 5 mass % or less, further preferably 3 mass % or less, particularly preferably 1 mass % or less, and most preferably 0 mass %.

[0131] From the viewpoint of the adhesion of the present composition, etc., the content of the metal element in the silica particles is preferably 30 to 1500 mass ppm, more preferably 100 to 1000 mass ppm, and even more preferably 100 to 500 mass ppm.

[0132] Examples of the metal element include Ti, Na, K, Mg, Ca, Al, and Fe.

[0133] The silica particles preferably contain 30 to 1500 mass ppm of titanium (Ti), more preferably 100 to 1000 mass ppm, and further preferably 100 to 500 mass ppm. Ti is an arbitrary component contained in the manufacture of silica particles. When the silica particles are manufactured, the generation of fine powders caused by the rupture of the silica particles will increase the specific surface area of ​​the particles. By including Ti during the manufacture of silica particles, hot compaction is easy during sintering, and the rupture of the particles can be suppressed. As a result, the generation of fine powders can be suppressed, and the attached particles attached to the surface of the mother particles of the silica particles can be reduced, thereby making it easy to adjust the specific surface area of ​​the silica particles. By including more than 30 mass ppm of Ti, hot compaction is easy during sintering, so the generation of fine powders caused by rupture can be suppressed. If the Ti content is less than 1500 mass ppm, the aforementioned effect is obtained, and the increase in the amount of silanol groups can be suppressed, and the dielectric loss tangent can be increased.

[0134] The silica particles may also contain metal elements other than Ti within the range that does not hinder the effects of the present disclosure. As metal elements, in addition to Ti, for example, Na, K, Mg, Ca, Al, Fe, etc. may also be mentioned. The sum of the contents of alkali metals and alkaline earth metals in the metal elements is preferably 1500 mass ppm or less, more preferably 1000 mass ppm or less, and further preferably 200 mass ppm or less. In addition, the content of Na in the metal elements is preferably 1500 mass ppm or less, more preferably 1000 mass ppm or less, and further preferably 200 mass ppm or less.

[0135] The silica particles are preferably silica particles manufactured by a wet method. The wet method refers to a method including a process of using a liquid as a silica source and gelling it to obtain a raw material for the silica particles. By using the wet method, it becomes easy to adjust the shape of the silica particles, especially spherical silica particles, without the need to make the shape of the particles consistent by crushing, etc., and as a result, it is easy to obtain particles with a small specific surface area. In addition, the wet method has a tendency to be difficult to generate particles that are significantly smaller than the average particle size and the specific surface area tends to become smaller after firing. In addition, in the wet method, by adjusting the impurities in the silica source, the amount of metal elements such as Ti can be adjusted, and then the state in which the aforementioned metal elements are uniformly dispersed in the particles can be formed.

[0136] As wet method, spray method, emulsion / gelation method etc. can be cited. As emulsion / gelation method, for example, dispersed phase and continuous phase containing silica precursor are emulsified, and the obtained emulsion is gelled to obtain spherical silica precursor. As emulsification method, dispersed phase containing silica precursor is preferably supplied to continuous phase by micropore part or porous membrane, and the method of making emulsion. Thus, emulsion with uniform droplet diameter is made, and as a result, spherical silica particles with uniform particle size are obtained. As such emulsification method, micro-mixing method, membrane emulsification method etc. can be cited. For example, micro-mixing method is disclosed in International Publication No. 2013 / 062105.

[0137] Silica particles can be obtained by heat treating the aforementioned silica precursor. The heat treatment has the following effects: the spherical silica precursor is sintered to densify the shell, and the amount of silanol groups on the surface is reduced to reduce the dielectric loss tangent. The temperature of the heat treatment is preferably above 700°C. In addition, from the viewpoint of suppressing the aggregation of particles, the temperature of the heat treatment is preferably below 1600°C. In addition, the obtained silica particles can be surface treated with a silane coupling agent. On the other hand, from the viewpoint of the toughness of the cured product, it is also preferred not to implement surface treatment.

[0138] From the viewpoint of toughness of the cured product and adhesion to the metal substrate layer, the content of the silica particles is preferably 50 parts by mass or more, more preferably 70 parts by mass or more, further preferably 90 parts by mass or more, and particularly preferably 100 parts by mass, relative to 100 parts by mass of the thermosetting resin in the present composition 1 and the present composition 2. In addition, the above content is preferably 400 parts by mass or less, more preferably 300 parts by mass or less, and further preferably 250 parts by mass or less.

[0139] From the viewpoint of better suppressing the attachment of silica particles during mixing and the foaming of the composition, the viewpoint of suppressing the aggregation of silica particles, and the viewpoints of reduced water absorption, low dielectric loss tangent, and close adhesion, the content of silica particles is preferably 10 to 400 parts by mass, more preferably 50 to 300 parts by mass, and further preferably 70 to 250 parts by mass relative to 100 parts by mass of the thermosetting resin in the present composition 3. In the case where it is particularly desired to form a high filling of silica particles, the content of the aforementioned silica particles is preferably 80 parts by mass or more, more preferably 90 parts by mass or more, and particularly preferably 100 parts by mass or more. In this case, the content of the aforementioned silica particles can be 400 parts by mass or less, 300 parts by mass or less, or 250 parts by mass or less.

[0140] The silica particles in the present composition 1, the present composition 2 or the present composition 3 are in a state of being fully wetted and uniformly dispersed due to the above-mentioned mechanism of action, and are in a state of being easily and highly interactive with the thermosetting resin. Therefore, in the present composition having the above-mentioned content within the above-mentioned range, that is, in the present composition having a large amount of silica particles filled with respect to the thermosetting resin, both components are easily stabilized, and a cured product having excellent adhesion to the metal substrate layer can be formed.

[0141] The present composition may contain one or more curing agents. The curing agent is an agent that initiates the curing reaction of the thermosetting resin by the action of heat, and specifically, α,α'-bis(tert-butylperoxy-m-isopropyl)benzene, 2,5-dimethyl-2,5-di(tert-butylperoxy)-3-hexyne, benzoyl peroxide, 3,3',5,5'-tetramethyl-1,4-diphenoquinone, chlorobenzoquinone, 2,4,6-tri-tert-butylphenol, tert-butylperoxyisopropyl monocarbonate, azobisisobutyronitrile, etc. The content of the curing agent relative to 100 parts by mass of the thermosetting resin is preferably 0.1 to 5 parts by mass.

[0142] The present composition may contain one or more curing accelerators. Examples of the curing accelerator include triallyl isocyanurate compounds such as triallyl isocyanurate, polyfunctional acrylic compounds having two or more acryloyl or methacryloyl groups in the molecule, polyfunctional vinyl compounds having two or more vinyl groups in the molecule, and vinylbenzyl compounds such as styrene having vinylbenzyl groups in the molecule. The content of the curing accelerator is preferably 10 to 100 parts by mass relative to 100 parts by mass of the thermosetting resin.

[0143] The present composition 1, the present composition 2 or the present composition 3 may contain one or more solvents. From the viewpoint of reducing the water absorption of the present composition 1, the present composition 2 or the present composition 3 and the cured product thereof, the surface tension of the solvent is preferably 45 mN / m or less, more preferably 40 mN / m or less, further preferably 35 mN / m or less, and particularly preferably 30 mN / m or less. The lower limit of the surface tension is not particularly limited, and may be 5 mN / m or more.

[0144] From the viewpoint of workability when forming a molded article such as a prepreg by thermally curing the present composition 1, the present composition 2 or the present composition 3, the boiling point of the solvent is preferably 75° C. or higher, more preferably 80° C. or higher, and further preferably 90° C. or higher. The upper limit of the boiling point is not particularly limited, but can be 200° C. or lower.

[0145] When the evaporation rate of butyl acetate at 23°C is set to 1, the evaporation rate of the solvent is preferably 0.3 to 3.0, more preferably 0.4 to 2.0, from the viewpoint of workability when the present composition 1, the present composition 2 or the present composition 3 is thermally cured to form a molded product such as a prepreg.

[0146] As the solvent, acetone, methanol, ethanol, butanol, 2-propanol, 2-methoxyethanol, 2-ethoxyethanol, toluene, xylene, methyl ethyl ketone, N,N-dimethylformamide, methyl isobutyl ketone, N-methylpyrrolidone, n-hexane, cyclohexane, etc. can be mentioned. From the viewpoint of the adhesion of the cured product to the metal substrate layer, the solvent preferably includes at least one selected from the group consisting of toluene (110°C, 28mN / cm, 0.58), cyclohexanone (156°C, 35mN / cm, 0.32), methyl ethyl ketone (80°C, 24.6mN / cm, 3.7) and N-methylpyrrolidone (202°C, 42mN / m, 0.3 to 4.0). It should be noted that the boiling point, surface tension and evaporation rate are indicated in parentheses in order.

[0147] The content of the solvent relative to the total mass of the present composition is not particularly limited, but can be 10 to 60% by mass.

[0148] The present composition 1, the present composition 2 or the present composition 3 may contain one or more plasticizers. Examples of the plasticizer include butadiene-styrene copolymers, etc. The content of the plasticizer relative to 100 parts by mass of the thermosetting resin is preferably 10 to 50 parts by mass, more preferably 20 to 40 parts by mass.

[0149] In addition to the above-mentioned components, the present composition may also contain other components such as surfactants, thixotropic modifiers, pH adjusters, pH buffers, viscosity adjusters, defoamers, silane coupling agents, dehydrating agents, weathering agents, antioxidants, heat stabilizers, lubricants, antistatic agents, brighteners, colorants, conductive materials, release agents, surface treatment agents, flame retardants, various organic or inorganic fillers, etc. within the range that does not impair their effects.

[0150] The prepreg 1 of the present disclosure comprises the present composition 1 or a semi-cured product thereof and a fibrous base material.

[0151] The prepreg 2 of the present disclosure includes the present composition 2 or a semi-cured product thereof and includes a fibrous base material.

[0152] The prepreg 3 of the present disclosure includes the present composition 3 or a semi-cured product thereof and includes a fibrous base material.

[0153] The fibrous substrate preferably contains a glass component. As the fibrous substrate, glass cloth, aramid cloth, polyester cloth, glass nonwoven fabric, aramid nonwoven fabric, polyester nonwoven fabric, pulp paper, etc. can be cited. The thickness of the fibrous substrate is not particularly limited and can be set to 3 to 10 μm. It should be noted that, as described above, about the present compositions 1 to 3, the description is omitted here.

[0154] The prepreg 1, prepreg 2 or prepreg 3 of the present disclosure can be produced by coating or impregnating a fibrous substrate with the corresponding present composition 1, present composition 2 or present composition 3. After coating or impregnation with the present composition 1, present composition 2 or present composition 3, the liquid composition can be heated to semi-cure.

[0155] The metal substrate 1 with resin of the present disclosure comprises the present composition 1 or its semi-cured product or the above-mentioned prepreg 1 and comprises a metal substrate layer. The metal substrate layer may be provided on one surface of the present composition 1 or its semi-cured product or the above-mentioned prepreg 1, or may be provided on both surfaces.

[0156] The metal substrate 2 with resin disclosed in the present invention comprises the present composition 2 or its semi-cured product or the above-mentioned prepreg 2 and comprises a metal substrate layer. The metal substrate layer may be provided on one surface of the present composition 2 or its semi-cured product or the above-mentioned prepreg 2, or may be provided on both surfaces.

[0157] The metal substrate 3 with resin of the present disclosure comprises the present composition 3 or its semi-cured product or the above-mentioned prepreg 3 and comprises a metal substrate layer. The metal substrate layer may be provided on one surface of the present composition 3 or its semi-cured product or the above-mentioned prepreg 3, or may be provided on both surfaces.

[0158] The type of metal substrate layer is not particularly limited. As the metal constituting the metal substrate, copper, copper alloy, stainless steel, nickel, nickel alloy (also including 42 alloy), aluminum, aluminum alloy, titanium, titanium alloy, etc. can be cited. The metal substrate layer is preferably a metal foil, and more preferably a copper foil such as a rolled copper foil and an electrolytic copper foil. The surface of the metal foil can be treated with rust prevention (oxide coating such as chromate, etc.), or it can be roughened. As the metal foil, a metal foil with a carrier formed by a carrier copper foil (thickness: 10 to 35 μm) and an extremely thin copper foil (thickness: 2 to 5 μm) laminated on the surface of the carrier copper foil via a peeling layer can also be used. The surface of the metal substrate layer can be treated with a silane coupling agent. In this case, the entire surface of the metal substrate layer can be treated with a silane coupling agent, and a portion of the surface of the metal substrate layer can be treated with a silane coupling agent. As a silane coupling agent, the above-mentioned substances can be used.

[0159] The thickness of the metal substrate layer is preferably 1 to 40 μm, more preferably 2 to 15 μm. From the viewpoint of reducing the transmission loss when using a metal substrate with a resin as a printed wiring board, the maximum height roughness (Rz) of the metal substrate layer (e.g., copper foil) is preferably 2 μm or less, more preferably 1.2 μm or less. Preferably, the Rz of the surface of the metal substrate layer (e.g., copper foil), the liquid composition, the semi-cured material, or the prepreg side is in the above range. When a metal substrate with a resin is used as a printed wiring board, the transmission loss can usually be reduced, but there is a tendency that the adhesion between the metal substrate layer and the prepreg, etc. is usually reduced. According to the prepreg 1, prepreg 2 or prepreg 3 using the present composition 1, the present composition 2 or the present composition 3 disclosed herein, the reduction in the above-mentioned adhesion can be suppressed, and the transmission loss can be reduced.

[0160] In one embodiment, the metal substrate with resin 1, the metal substrate with resin 2, or the metal substrate with resin 3 of the present disclosure can be manufactured by coating the surface of the metal substrate layer with the corresponding present composition 1, present composition 2, or present composition 3. After the present composition 1, present composition 2, or present composition 3 is coated, the liquid composition can be heated to semi-cured.

[0161] In another embodiment, the metal substrate with resin 1, the metal substrate with resin 2, or the metal substrate with resin 3 of the present disclosure can be manufactured by laminating the prepreg 1, prepreg 2, or prepreg 3 corresponding to the metal substrate layer. As a method for laminating the metal substrate layer and the prepreg 1, prepreg 2, or prepreg 3, a method of thermocompression bonding them can be cited.

[0162] Wiring board 1 of the present disclosure includes a cured product of present composition 1 and includes metal wiring.

[0163] Wiring board 2 of the present disclosure includes a cured product of present composition 2 and includes metal wiring.

[0164] Wiring board 3 of the present disclosure includes a cured product of present composition 3 and includes metal wiring.

[0165] As the metal wiring, one produced by etching the above-mentioned metal base material layer or the like can be used.

[0166] The wiring board 1, wiring board 2 or wiring board 3 disclosed in the present invention can be manufactured by a method of etching the metal substrate layer possessed by the corresponding metal substrate with resin 1, metal substrate with resin 2 or metal substrate with resin 3, a method of forming a pattern circuit on the surface of the cured product of the present composition 1, the present composition 2 or the present composition 3 using an electrolytic plating method (semi-additive method (SAP method), modified semi-additive method (MSAP method), etc.).

[0167] In one embodiment, silica particles are used to mix with a liquid composition containing a thermosetting resin to form a prepreg, and the water vapor adsorption amount of the silica particles is 0.01 to 10.00 cm 3 / g, and the water retention fluctuation is less than 20%.

[0168] In another embodiment, silica particles are mixed with a liquid composition containing a thermosetting resin to form a prepreg, wherein the absolute value of the charge of the silica particles is 0.7 to 200 nC / g and d50 is 1.0 to 10.0 μm.

[0169] In another embodiment, silica particles are used to be mixed with a liquid composition containing a thermosetting resin to form a prepreg, wherein the silica particles have a powder dynamic friction angle of 10 to 40 degrees, d50 of 1.0 to 10.0 μm, and when the median particle size d50 after dispersion in toluene is set to A1 and the median particle size d50 after further ultrasonic treatment after dispersion in toluene is set to B1, the ratio of A1 to B1 (A1 / B1) is 1.0 to 50.0.

[0170] The preferred embodiments and numerical ranges of the charge, particle size distribution, d50, d10, specific surface area, d50 / d10, the product of the specific surface area and the d50 of the silica particles, the powder dynamic friction angle, the ratio (A1 / B1), the angle of repose, the shape, the sphericity, the dielectric loss tangent, the water vapor adsorption amount, the water retention variation, the internal carbon content, the surface treatment, the elements that can be contained, the manufacturing method, etc. of the silica particles are as described above, and therefore, the description is omitted here. In addition, as described above, the silica particles may also contain metal elements.

[0171] Example

[0172] Hereinafter, the embodiments of the present disclosure will be described in detail based on examples, but the embodiments of the present disclosure are not limited to these.

[0173] 1. Preparation of ingredients for making liquid composition

[0174] [Thermosetting resin]

[0175] Polyphenylene ether resin: a modified polyphenylene ether obtained by modifying the terminal hydroxyl group of polyphenylene ether with a methacryloyloxy group (manufactured by SABIC: Noryl SA9000, Mw: 1700, number of functional groups per molecule: 2)

[0176] [Silicon dioxide particles]

[0177] Silica particles A: Silica powder produced by a wet method (AGC-Si-Tech Co., Ltd., H-31, d50: 3.5 μm, specific surface area: 1.0 m 2 15 g of the mixture was filled into an alumina crucible, heated at 1200°C for 1 hour in an electric furnace, cooled to 25°C, and ground into silica particles (water vapor adsorption: 6.00 cm 3 / g, moisture retention change: 5%, Na content: 20 mass ppm, total amount of metal elements: 40 ppm, charge: 8 nC / g, internal carbon content: 0 mass %).

[0178] Silica particles B: Silica powder produced by a wet method (manufactured by Suzuki Oil & Fats Co., Ltd.: E-2C, d50: 2.5 μm, specific surface area: 2.2 m 2 15 g of the mixture was filled into an alumina crucible, heated at 1200°C for 1 hour in an electric furnace, cooled to 25°C, and ground into silica particles (water vapor adsorption: 8.00 cm 3 / g, moisture retention change: 8%, Na content: 20 mass ppm, total amount of metal elements: 40 ppm, charge: 10 nC / g, internal carbon content: 0 mass %).

[0179] Silica particles C: Silica particles produced by VMC (Vaporized Metal Combustion) (manufactured by Admatechs: SC5500-SQ, d50: 1.5 μm, specific surface area: 5.0 m 2 / g, water vapor adsorption: 22.00cm 3 / g, moisture retention variation: 25%, Na content: 100 mass ppm, total amount of metal elements: 500 ppm).

[0180] Silica particles D: Silica particles produced by a dry process (manufactured by NIPPON STEEL Chemical & Material Co., Ltd.: SPH516, d50: 0.64 μm, specific surface area: 12.7 m 2 / g, water vapor adsorption: 30.00cm 3 / g, moisture retention variation: 40%, Na content: 150 mass ppm, total amount of metal elements: 1700 ppm).

[0181] Silica particles C2: manufactured by AGC-Si-Tech Co., Ltd., model "H-31", charge amount: 12 nC / g, internal carbon content: 0 mass %.

[0182] Silica particles D2: manufactured by Admatechs, model number “SO-C2”, charge amount: 0.03 nC / g, internal carbon content: 0% by mass.

[0183] Silica particles E2: manufactured by Nippon Shokubai, model number “Seahostar (registered trademark) KE-S-S150”, charge amount: 250 nC / g, internal carbon content: 0.8 mass %.

[0184] Silica particles C3: manufactured by NIPPON STEEL Chemical & Material Co., Ltd., trade name "HS-206"

[0185] [Plasticizer]

[0186] Butadiene-styrene random copolymer (Ricon 100, Cray Valley)

[0187] [Curing accelerator]

[0188] Triallyl isocyanurate (TAIC, Mitsubishi Chemical Corporation)

[0189] [Curing agent]

[0190] α,α'-Di(tert-butylperoxy)diisopropylbenzene (Perbutyl(registered trademark) P, NOF Corporation)

[0191] [Solvent]

[0192] Toluene

[0193] 2. Manufacture of liquid composition, prepreg and metal substrate with resin

[0194] <Example 11>

[0195] 59 parts by mass of polyphenylene ether resin, 16 parts by mass of butadiene-styrene random copolymer, 25 parts by mass of triallyl isocyanurate, 1 part by mass of α,α'-di(tert-butylperoxy)diisopropylbenzene, 55 parts by mass of silica particles A, and 80 parts by mass of toluene were placed in a plastic bottle, and Φ20 mm alumina balls were added. The mixture was mixed at 30 rpm for 12 hours, and the alumina balls were removed to obtain a liquid composition.

[0196] The liquid composition was impregnated and coated on a glass cloth of IPC Spec 2116, and then heated and dried at 160° C. for 4 minutes to obtain a prepreg.

[0197] Copper foil with carrier (thickness: 3 μm, maximum height roughness Rz: 2 μm, manufactured by Mitsui Metal Industries, Ltd., MT18E) was laminated on both sides of the prepreg and heated at 230°C and a pressure of 30 kg / cm 2 The mixture was heated and molded for 120 minutes to obtain a metal substrate with resin having a cured product of the prepreg and a copper foil with a carrier.

[0198] <Examples 12~14>

[0199] The as-made composition, the prepreg, and the metal substrate with the resin were prepared in the same manner as in Example 11 except that the silica particles A were changed to the silica particles described in Table 1.

[0200] <Examples 15, 16>

[0201] In Example 11, the amount of polyphenylene ether resin was set to 40 parts by mass. Similarly, for the liquid composition of Example 15, in which 138 parts by mass of silica particles A were contained relative to 100 parts by mass of polyphenylene ether resin, and in Example 12, the amount of polyphenylene ether resin was set to 40 parts by mass, and similarly, a liquid composition of Example 16, in which 138 parts by mass of silica particles B were contained relative to 100 parts by mass of polyphenylene ether resin, was obtained.

[0202] [Determination of peel strength]

[0203] The metal substrates with resin produced in Examples 11 to 16 were subjected to a HAST test in accordance with IEC 60068-2-66 (JIS C 60068-2-66 (2001)) at a temperature of 120° C., a relative humidity of 85%, and an exposure time of 96 hours.

[0204] After the HAST test, the peel strength between the cured product and the copper foil with a carrier was measured in accordance with IPC-TM650-2.4.8. The measurement results are summarized in Table 1.

[0205] It should be noted that Examples 11, 12, 15 and 16 are embodiments, and Examples 13 and 14 are comparative examples.

[0206] [Table 1]

[0207]

[0208] As can be seen from Table 1, the cured product of the prepreg 1 using the present composition 1 has excellent adhesion to the metal base material layer.

[0209] <Example 21>

[0210] In the same manner as in Example 11, a liquid composition, a prepreg, and a metal substrate with a resin were produced.

[0211] <Examples 22~25>

[0212] A liquid composition, a prepreg, and a metal substrate with a resin were produced in the same manner as in Example 21 except that the silica particles A were changed to the silica particles described in Table 2.

[0213] <Examples 26, 27>

[0214] In Example 21, the amount of polyphenylene ether resin was set to 40 parts by mass. Similarly, for the liquid composition of Example 26 containing 138 parts by mass of silica particles A relative to 100 parts by mass of polyphenylene ether resin, and in Example 22, the amount of polyphenylene ether resin was set to 40 parts by mass, and similarly, a liquid composition of Example 27 containing 138 parts by mass of silica particles B relative to 100 parts by mass of polyphenylene ether resin was obtained.

[0215] [Evaluation of toughness]

[0216] The bending modulus of the metal substrates with resin produced in Examples 21 to 27 was measured using TENSILON (RTF-1350, manufactured by A&D Company, Limited) in accordance with JIS K7171 at a load cell rating of 10 kN, a support distance of 64 mm, and a speed of 2 mm / min. The measurement results are summarized in Table 2.

[0217] It should be noted that Examples 21, 22, 26 and 27 are embodiments, and Examples 23 to 25 are comparative examples.

[0218] [Table 2]

[0219]

[0220] As can be seen from Table 2, the metal substrate with a resin using the present composition 2 has a higher flexural modulus and is superior in toughness compared to the metal substrate with a resin not using the present composition 2.

[0221] <Example 31>

[0222] A liquid composition was obtained in the same manner as in Example 11 except that kneading was performed in a planetary disperser.

[0223] The liquid composition was impregnated and coated on a glass cloth of IPC Spec 2116, and then heated and dried at 160° C. for 4 minutes to obtain a prepreg.

[0224] Three prepregs were stacked, and ultra-thin copper foil with a carrier (thickness: 3 μm, Rz: 2 μm, manufactured by Mitsui Kinzoku Co., Ltd., MT18E) was stacked on top and bottom. The prepreg was heated at 230°C and a pressure of 30 kg / cm 2 The heat molding was carried out for 120 minutes to obtain a metal substrate with resin.

[0225] <Examples 32~35>

[0226] A liquid composition, a prepreg, and a metal substrate with a resin were produced in the same manner as in Example 31 except that the silica particles A were changed to the silica particles described in Table 3.

[0227] In addition, in each example, d50, ratio (A1 / B1), powder dynamic friction angle and repose angle of the silica particles were measured according to the above-mentioned method using the above-mentioned equipment.

[0228] [Evaluation of dispersibility of liquid composition]

[0229] The median particle size of the liquid composition was determined according to the particle size analyzer method described in JIS K 5600-2-5 (1999).

[0230] [Evaluation of wall adhesion during mixing]

[0231] After mixing the components, adhesion of the silica particles to the wall surface of the planetary disperser was visually confirmed, and the wall adhesion of the silica particles was evaluated according to the following criteria.

[0232] A: The thickness of the wall is less than 0.1mm

[0233] B: The thickness of the attached wall is more than 0.1 mm and less than 1.0 mm

[0234] C: The thickness of the wall exceeds 1.0 mm

[0235] [Evaluation of foaming during mixing]

[0236] After mixing the components, the foaming of the composition was visually observed and evaluated based on the following criteria.

[0237] A: There is bubbling

[0238] C: No bubbling

[0239] [Evaluation of uniformity of prepreg]

[0240] The prepreg was observed at 100 times magnification using an optical microscope, and the uniformity of the prepreg was evaluated according to the following criteria.

[0241] A: No uneven portion with a diameter of 0.5 mm or more was observed.

[0242] C: Uneven portions with a diameter of 0.5 mm or more were observed.

[0243] The evaluation results are shown in Table 3. Examples 31 and 32 are examples, and Examples 33 to 35 are comparative examples.

[0244] [Table 3]

[0245]

[0246] As can be seen from Table 3, in Examples 31 and 32 using the present composition 3, adhesion of silica particles during mixing and foaming of the composition were suppressed. In addition, in Examples 31 and 32, the dispersibility of silica particles was excellent, and the uniformity of the prepreg was excellent.

[0247] The disclosures of Japanese Patent Application Nos. 2022-075461, 2022-075462, and 2022-075146 filed on April 28, 2022 are incorporated herein by reference in their entirety. All documents, patent applications, and technical standards described in this specification are incorporated herein by reference to the same extent as if each document, patent application, and technical standard were specifically and individually described as being incorporated by reference.

Claims

1. A liquid composition comprising a thermosetting resin and silica particles, wherein the silica particles have a water vapor adsorption capacity of 0.01 to 10.00 cm at a relative water vapor pressure of 0.8 in a water vapor adsorption isotherm at 25°C. 3 / g, and further, when the water content by mass of the silica particles after standing at a temperature of 85°C and a relative humidity of 85% for 24 hours is set to A, and the water content by mass of the silica particles after standing at a temperature of 85°C and a relative humidity of 85% for 24 hours and further standing at a temperature of 25°C and a relative humidity of 50% for 24 hours is set to B, the water retention change amount calculated by (AB) / A×100 is less than 20%.

2. The liquid composition according to claim 1, wherein The specific surface area of ​​the silicon dioxide particles is 0.1 to 10.0 m 2 / g.

3. The liquid composition according to claim 1, wherein The silica particles contain 30 to 1500 ppm by mass of a metal element.

4. The liquid composition according to claim 1, wherein The median particle size d50 of the silicon dioxide particles is 1.0 to 10.0 μm.

5. The liquid composition according to claim 1, wherein The content of the silica particles is 50 to 400 parts by mass based on 100 parts by mass of the thermosetting resin.

6. A liquid composition comprising: a thermosetting resin; and silica particles having an absolute value of a charge of 0.7 to 200 nC / g and a median particle size d50 of 1.0 to 10.0 μm.

7. The liquid composition according to claim 6, wherein The silicon dioxide particles are particles whose surfaces are not treated.

8. The liquid composition according to claim 6, wherein The silica particles have an internal carbon content of 10% by mass or less.

9. The liquid composition according to claim 6, wherein The silica particles have a median particle size d50 of more than 1.0 μm and not more than 5.0 μm.

10. The liquid composition according to claim 6, wherein The content of the silica particles is 50 to 400 parts by mass based on 100 parts by mass of the thermosetting resin.

11. A liquid composition comprising a thermosetting resin and silica particles, wherein the silica particles have a powder dynamic friction angle of 10 to 40 degrees and a median particle size d50 of 1.0 to 10.0 μm, and further, when the median particle size d50 of the silica particles after being dispersed in toluene is set to A1, and the median particle size d50 of the silica particles after being dispersed in toluene and further subjected to ultrasonic treatment is set to B1, the ratio of A1 to B1, i.e. A1 / B1, is 1.0 to 50.

0.

12. The liquid composition according to claim 11, wherein The repose angle of the silicon dioxide particles is 25 to 50 degrees.

13. The liquid composition according to claim 11, wherein The content of the silica particles is 10 to 400 parts by mass based on 100 parts by mass of the thermosetting resin.

14. The liquid composition according to any one of claims 1 to 13, wherein The thermosetting resin is epoxy resin, polyphenylene ether resin or o-divinylbenzene resin. 15 . The liquid composition according to claim 1 , further comprising at least one solvent selected from the group consisting of toluene, cyclohexanone, methyl ethyl ketone and N-methylpyrrolidone. 16 . A prepreg comprising: the liquid composition according to claim 1 or a semi-cured product thereof; and a fibrous base material.

17. The prepreg according to claim 16, wherein The fibrous substrate includes a glass component.

18. A metal substrate with resin, comprising: the liquid composition or semi-cured product thereof according to any one of claims 1 to 13, or a prepreg containing the liquid composition or semi-cured product thereof and containing a fibrous substrate; and a metal substrate layer.

19. The metal substrate with resin according to claim 18, wherein The metal substrate layer is copper foil.

20. The metal substrate with resin according to claim 19, wherein The maximum height roughness Rz of the surface of the copper foil on the liquid composition, the semi-cured product, or the prepreg side is 2 μm or less. 21 . A wiring board comprising: a cured product of the liquid composition according to claim 1 ; and metal wiring.

22. A silica particle for use in mixing with a liquid composition containing a thermosetting resin to form a prepreg, wherein the silica particle has a water vapor adsorption amount of 0.01 to 10.00 cm2 at a relative water vapor pressure of 0.8 in a water vapor adsorption isotherm at 25°C. 3 / g, and further, when the water content by mass of the silica particles after standing at a temperature of 85°C and a relative humidity of 85% for 24 hours is set to A, and the water content by mass of the silica particles after standing at a temperature of 85°C and a relative humidity of 85% for 24 hours and further standing at a temperature of 25°C and a relative humidity of 50% for 24 hours is set to B, the water retention change amount calculated by (AB) / A×100 is less than 20%.

23. The silicon dioxide particles according to claim 22, having a specific surface area of ​​0.1 to 10.0 m 2 / g.

24. Silica particles for use in mixing with a liquid composition containing a thermosetting resin to form a prepreg, wherein the absolute value of the charge of the silica particles is 0.7 to 200 nC / g and the median particle size d50 is 1.0 to 10.0 μm. The silica particles according to claim 24 , wherein the amount of internal carbon is 10% by mass or less.

26. A silica particle used for mixing with a liquid composition containing a thermosetting resin to form a prepreg, wherein the silica particles have a powder dynamic friction angle of 10 to 40 degrees and a median particle size d50 of 1.0 to 10.0 μm. When the median particle size d50 of the silica particles after being dispersed in toluene is set to A1 and the median particle size d50 of the silica particles after being dispersed in toluene and further subjected to ultrasonic treatment is set to B1, the ratio of A1 to B1, i.e. A1 / B1, is 1.0 to 50.

0.

27. The silicon dioxide particles according to claim 26, wherein The repose angle of the silicon dioxide particles is 25 to 50 degrees.