Method for synthesizing magnetic Al2O3 nano material by urease method

Synthesis of magnetic Al2O3 nanomaterials by urease method solves the problem of lack of magnetic nanomaterials that effectively remove antibiotic pollutants in the prior art, and achieves the effect of efficient and stable removal of organic matter in water.

CN119500056AActive Publication Date: 2025-02-25TIANJIN TIANSHI COLLEGE
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411779676.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-12-05
Publication Date
2025-02-25
Estimated Expiration
2044-12-05

AI Technical Summary

Technical Problem

There is a lack of effective magnetic Al2O3 nanomaterials in the prior art for removing antibiotic contaminants, and the research on alumina materials is relatively limited.

Method used

The method of synthesizing magnetic Al2O3 nanomaterials by urease method is used to synthesize magnetic Al2O3 nanomaterials with high specific surface area and magnetism by adding iron tetraoxide and surfactant to the urea enzymatic method to control the stirring speed and reaction conditions.

Benefits of technology

The prepared magnetic Al2O3 nanomaterial has high adsorption performance and stability, which can significantly remove organic matter from water, and solve the problems of high adsorbent stability and cost in the prior art.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a method for synthesizing a magnetic Al2O3 nano material by a urease method, and relates to the technical field of magnetic nano materials. The preparation method comprises the following steps: firstly, mixing and dispersing salt and urea in water, mixing and dispersing ferroferric oxide and a surfactant in water, then mixing the two materials, adding urease, controlling the stirring speed, and carrying out enzymolysis reaction to obtain a precipitation product; and finally, washing and drying the precipitation product, and roasting to obtain the magnetic Al2O3 nano material. The magnetic Al2O3 nano material disclosed by the invention has relatively high specific surface area and magnetism, and can be used for remarkably removing organic matters in water.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of magnetic nanomaterials, and in particular to a method for synthesizing magnetic Al2O3 nanomaterials using a urease method. Background Art

[0002] At present, the adsorbents commonly used to remove antibiotic pollutants include activated carbon, biochar, mineral materials, metal oxides and hydroxides, metal organic frameworks and composite materials, etc. Activated carbon adsorbents have high cost and poor regeneration performance, and metal organic frameworks have poor stability.

[0003] Compared with other materials, alumina is one of the main metal oxides in minerals and soils. It can be synthesized in a simple way in the laboratory. Alumina has good stability. By changing the synthesis parameters, its specific surface area, pore structure and surface charge can be regulated, so it can be applied in the field of adsorption. For example, aluminum oxide nanomaterials are modified based on urea enzymatic hydrolysis, and the adsorption efficiency and stability are significantly improved by optimizing the material structure and adsorption performance, so as to quickly and efficiently remove antibiotics. However, there are few reports on the research of magnetic Al2O3 nanomaterials. Summary of the invention

[0004] Based on the above problems, the present invention provides a method for synthesizing magnetic Al2O3 nanomaterials by urease method. In the process of synthesizing aluminum oxide nanomaterials by urea enzymatic hydrolysis, ferroferric oxide and a surfactant are first added, and then urease is added, and process parameters such as stirring speed are controlled to obtain a magnetic Al2O3 nanomaterial with excellent adsorption performance.

[0005] The method for synthesizing magnetic Al2O3 nanomaterials by urease method of the present invention comprises the following steps:

[0006] (1) Aluminum salt and urea are mixed in a mass ratio of 1:3-6 and ultrasonically dispersed in water, and then aqueous ammonia is added dropwise to adjust the pH value of the solution to neutral or weak alkaline, thereby obtaining solution I;

[0007] (2) mixing ferrosoferric oxide and a surfactant in a mass ratio of 1-3:1-3, and dispersing the mixture in water to obtain a solution II;

[0008] (3) mixing the solution I and the solution II, controlling the mass ratio of aluminum salt to ferrosoferric oxide to be 2 to 3:1, adding urease after fully mixing, and stirring evenly, wherein the stirring speed is 300 to 500 r / min; after stopping stirring, reacting at 35 to 45° C. for 20 to 30 hours, and collecting the precipitate by centrifugation after the reaction is completed;

[0009] (4) washing and drying the precipitate to obtain a precursor;

[0010] (5) calcining the precursor at a temperature of 450° C. to 550° C. for 1 h to 3 h to obtain a magnetic Al 2 O 3 nanomaterial.

[0011] Preferably, the aluminum salt in step (1) is any one of aluminum chloride, aluminum sulfate and aluminum nitrate.

[0012] Preferably, the surfactant is a quaternary ammonium salt surfactant.

[0013] Preferably, the amount of urease added in step (3) accounts for 3-5% of the mass of the aluminum chloride.

[0014] Preferably, step (4) is performed by washing with deionized water and ethanol.

[0015] Preferably, the drying temperature in step (4) is 50°C to 70°C.

[0016] Compared with the prior art, the present invention has the following beneficial effects:

[0017] The invention provides a method for preparing a magnetic aluminum oxide nano material, which comprises the following steps: firstly mixing and dispersing salt and urea in water, mixing and dispersing ferroferric oxide and a surfactant in water, then mixing the two, adding urease, controlling the stirring speed, performing urease reaction, and obtaining a precipitated product; and finally washing and drying the precipitated product and performing a roasting treatment to obtain a magnetic Al2O3 nano material. The magnetic Al2O3 nano material of the invention has a high specific surface area and magnetism, and can significantly remove organic matter in water. DETAILED DESCRIPTION

[0018] For making the purpose, technical scheme and advantage of the present invention clearer, below in conjunction with embodiment, preferred embodiment of the present invention is described in further detail.Based on the embodiment among the present invention, those of ordinary skill in the art, without making the every other embodiment that obtains under the creative work premise, all belong to the scope of protection of the present invention.The quaternary ammonium salt surfactant adopted in the present invention is octadecyl trimethyl ammonium chloride.

[0019] Example 1

[0020] A method for synthesizing magnetic Al2O3 nanomaterials by urease method comprises the following steps:

[0021] (1) aluminum chloride and urea were mixed in a mass ratio of 1:3 and ultrasonically dispersed in water, and then aqueous ammonia was added dropwise to adjust the pH value of the solution to 8 to obtain solution I;

[0022] (2) mixing ferrosoferric oxide and a quaternary ammonium salt surfactant in a mass ratio of 1:2, and dispersing the mixture in water to obtain a solution II;

[0023] (3) The solution I and the solution II are mixed, the mass ratio of aluminum salt to ferrosoferric oxide is controlled to be 2:1, urease is added after being fully mixed, and stirred evenly, wherein the stirring speed is 500 r / min; after stopping stirring, the mixture is reacted at 37° C. for 24 hours, and after the reaction is completed, the precipitate is collected by centrifugation; wherein the amount of urease added is 3% of the mass of the aluminum chloride.

[0024] (4) washing the precipitate with deionized water and ethanol, and drying the precipitate at 60° C. overnight to obtain a precursor;

[0025] (5) calcining the precursor at 500° C. for 2 h to obtain Al 2 O 3 nanomaterials having magnetic properties.

[0026] After testing, the specific surface area of ​​the magnetic Al2O3 nanomaterial prepared in Example 1 is 1224.1 m 2 / g, pore volume 0.50cm 3 / g.

[0027] Example 2

[0028] A method for synthesizing magnetic Al2O3 nanomaterials by urease method comprises the following steps:

[0029] (1) aluminum sulfate and urea are mixed in a mass ratio of 1:3 and ultrasonically dispersed in water, and then aqueous ammonia is added dropwise to adjust the pH value of the solution to neutral or weak alkaline, to obtain solution I;

[0030] (2) mixing ferrosoferric oxide and a quaternary ammonium salt surfactant in a mass ratio of 2:3, and dispersing the mixture in water to obtain a solution II;

[0031] (3) mixing the solution I and the solution II, controlling the mass ratio of aluminum salt to ferrosoferric oxide to be 3:1, adding urease after fully mixing, stirring evenly, wherein the stirring speed is 500 r / min; after stopping stirring, reacting at 37° C. for 24 hours, and collecting the precipitate by centrifugation after the reaction is completed; wherein the amount of urease added accounts for 3% of the mass of the aluminum sulfate;

[0032] (4) washing the precipitate with deionized water and ethanol, and drying the precipitate at 60° C. overnight to obtain a precursor;

[0033] (5) calcining the precursor at 500° C. for 2 h to obtain Al 2 O 3 nanomaterials having magnetic properties.

[0034] After testing, the specific surface area of ​​the magnetic Al2O3 nanomaterial prepared in Example 2 is 1189.5 m 2 / g, pore volume 0.53cm 3 / g.

[0035] Example 3

[0036] A method for synthesizing magnetic Al2O3 nanomaterials by urease method comprises the following steps:

[0037] (1) aluminum nitrate and urea are mixed in a mass ratio of 1:5 and ultrasonically dispersed in water, and then aqueous ammonia is added dropwise to adjust the pH value of the solution to neutral or weak alkaline, to obtain solution I;

[0038] (2) mixing ferrosoferric oxide and a quaternary ammonium salt surfactant in a mass ratio of 3:1, and dispersing the mixture in water to obtain a solution II;

[0039] (3) mixing the solution I and the solution II, controlling the mass ratio of aluminum salt to ferrosoferric oxide to be 2:1, adding urease after fully mixing, stirring evenly, wherein the stirring speed is 300 r / min; stopping stirring and reacting at 37° C. for 24 h, and collecting the precipitate by centrifugation after the reaction is completed; wherein the amount of urease added accounts for 5% of the mass of the aluminum nitrate;

[0040] (4) washing the precipitate with deionized water and ethanol, and drying the precipitate at 70° C. overnight to obtain a precursor;

[0041] (5) calcining the precursor at 550° C. for 1 h to obtain Al 2 O 3 nanomaterials having magnetic properties.

[0042] After testing, the specific surface area of ​​the magnetic Al2O3 nanomaterial prepared in Example 3 is 1301.4 m 2 / g, pore volume 0.52cm 3 / g.

[0043] Example 4

[0044] A method for synthesizing magnetic Al2O3 nanomaterials by urease method comprises the following steps:

[0045] (1) aluminum chloride and urea are mixed in a mass ratio of 1:6 and ultrasonically dispersed in water, and then ammonia water is added dropwise to adjust the pH value of the solution to neutral or weak alkaline, to obtain solution I;

[0046] (2) mixing ferrosoferric oxide and a quaternary ammonium salt surfactant in a mass ratio of 1:3, and dispersing the mixture in water to obtain a solution II;

[0047] (3) mixing the solution I and the solution II, controlling the mass ratio of aluminum salt to ferrosoferric oxide to be 3:1, adding urease after fully mixing, stirring evenly, wherein the stirring speed is 500 r / min; after stopping stirring, reacting at 38° C. for 24 hours, and collecting the precipitate by centrifugation after the reaction is completed; wherein the amount of urease added accounts for 4% of the mass of the aluminum chloride;

[0048] (4) washing the precipitate with deionized water and ethanol, and drying at 50° C. overnight to obtain a precursor;

[0049] (5) The precursor is calcined at 450° C. for 3 h to obtain a magnetic Al 2 O 3 nanomaterial.

[0050] After testing, the specific surface area of ​​the magnetic Al2O3 nanomaterial prepared in Example 4 is 1142.6 m 2 / g, pore volume 0.51cm 3 / g.

[0051] Comparative Example 1

[0052] A method for synthesizing Al2O3 nanomaterials by urease method comprises the following steps:

[0053] (1) aluminum chloride and urea were mixed in a mass ratio of 1:3 and ultrasonically dispersed in water, and then aqueous ammonia was added dropwise to adjust the pH value of the solution to 8 to obtain solution I;

[0054] (2) adding urease to the solution I at 37° C., stirring evenly, stopping stirring and reacting for 24 hours, and collecting the precipitate by centrifugation after the reaction is completed; wherein the amount of urease added is 3% of the mass of the aluminum chloride, and the stirring speed is 500 r / min;

[0055] (3) washing the precipitate with deionized water and ethanol, and drying at 60° C. overnight to obtain a precursor;

[0056] (4) calcining the precursor at 500°C for 2h to obtain Al2O3 nanomaterials.

[0057] After testing, the specific surface area of ​​the Al2O3 nanomaterial prepared in Comparative Example 1 is 811.3 m 2 / g, pore volume 0.25cm 3 / g.

[0058] Comparative Example 2

[0059] A method for synthesizing magnetic Al2O3 nanomaterials by urease method comprises the following steps:

[0060] (1) aluminum chloride and urea were mixed in a mass ratio of 1:3 and ultrasonically dispersed in water, and then aqueous ammonia was added dropwise to adjust the pH value of the solution to 8 to obtain solution I;

[0061] (2) dispersing ferrosoferric oxide in water to obtain solution II;

[0062] (3) Mixing the solution I and the solution II, controlling the mass ratio of aluminum salt to ferrosoferric oxide to be 2:1, adding urease after fully mixing, stirring evenly and then stopping stirring, reacting at 37° C. for 24 hours, wherein the amount of urease added is 3% of the mass of the aluminum chloride. After the reaction is completed, centrifugation is performed to collect the precipitate; wherein the stirring speed is 500 r / min;

[0063] (4) washing the precipitate with deionized water and ethanol, and drying the precipitate at 60° C. overnight to obtain a precursor;

[0064] (5) calcining the precursor at 500° C. for 2 h to obtain Al 2 O 3 nanomaterials having magnetic properties.

[0065] After testing, the specific surface area of ​​the magnetic Al2O3 nanomaterial prepared in Comparative Example 2 is 1007.4 m 2 / g, pore volume 0.32cm 3 / g.

[0066] The nanomaterials prepared in Examples 1 to 4 and Comparative Examples 1-2 were used as adsorbents to conduct an adsorption experiment on tetracycline in water. The specific operation was as follows:

[0067] First, a tetracycline aqueous solution with a concentration of 25 ug / mL was prepared; then 30 mL of the tetracycline aqueous solution was weighed, 7.5 mg of the adsorbent was added, and adsorption experiments were carried out respectively. After adsorption equilibrium, the removal rate of tetracycline in water was determined, as shown in Table 1.

[0068] Table 1

[0069] Adsorbent Tetracycline removal rate Example 1 93.4% Example 2 92.1% Example 3 96.0% Example 4 92.8% Comparative Example 1 62.5% Comparative Example 2 78.3%

[0070] The embodiments described above are part of the embodiments of the present invention, rather than all of the embodiments. The detailed description of the embodiments of the present invention is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

Claims

1. A method for synthesizing magnetic Al2O3 nanomaterials by urease method, characterized in that: The following steps are involved: (1) Aluminum salt and urea are mixed in a mass ratio of 1:3-6 and ultrasonically dispersed in water, and then aqueous ammonia is added dropwise to adjust the pH value of the solution to neutral or weak alkaline, thereby obtaining solution I; (2) mixing ferrosoferric oxide and a surfactant in a mass ratio of 1-3:1-3, and dispersing the mixture in water to obtain a solution II; (3) mixing the solution I and the solution II, controlling the mass ratio of aluminum salt to ferrosoferric oxide to be 2 to 3:1, adding urease after fully mixing, and stirring evenly, wherein the stirring speed is 300 to 500 r / min; after stopping stirring, reacting at 35 to 45° C. for 20 to 30 hours, and collecting the precipitate by centrifugation after the reaction is completed; (4) washing and drying the precipitate to obtain a precursor; (5) calcining the precursor at a temperature of 450° C. to 550° C. for 1 h to 3 h to obtain a magnetic Al 2 O 3 nanomaterial.

2. The method for synthesizing magnetic Al2O3 nanomaterials by urease method according to claim 1, characterized in that: The aluminum salt in step (1) is any one of aluminum chloride, aluminum sulfate and aluminum nitrate.

3. The method for synthesizing magnetic Al2O3 nanomaterials by urease method according to claim 1, characterized in that: The surfactant is a quaternary ammonium salt surfactant.

4. The method for synthesizing magnetic Al2O3 nanomaterials by urease method according to claim 1, characterized in that: The amount of urease added in step (3) accounts for 3-5% of the mass of the aluminum chloride.

5. The method for synthesizing magnetic Al2O3 nanomaterials by urease method according to claim 1, characterized in that: Step (4) is to wash with deionized water and ethanol.

6. The method for synthesizing magnetic Al2O3 nanomaterials by urease method according to claim 1, characterized in that: The drying temperature in step (4) is 50°C to 70°C.

Citation Information

Patent Citations

  • Process for preparing iron based oxygen carrier

    CN101486941A

  • Modified magnetic alumina absorbent, preparation method for modified magnetic alumina absorbent and application of modified magnetic alumina absorbent

    CN107281998A

  • Preparation method of magnetic composite adsorbing material and application thereof

    CN112619591A

  • Batch synthesis of basic carbonate and metal oxide nanotubes by urea enzymolysis method

    CN113388645A

  • Preparation and application of Al2O3 modified Fe3O4 nanoparticles for anionic dye

    CN113634221A