Environmentally friendly weighting fluid loss reducing agent suitable for high-temperature, high-salinity oil wells and its preparation process
By constructing a temperature- and salt-resistant macromolecular network using cellulose nanocrystals and bio-based zwitterionic monomers, and combining it with the mechanochemical reaction of natural dolomite micropowder template agent, an environmentally friendly weighting fluid loss reducing agent suitable for high-temperature and high-salinity oil wells was prepared. This solved the problems of plugging failure and salt precipitation agglomeration under high-temperature and high-salinity environments, achieving rapid hydration, low filtration loss, and high efficiency in preventing sedimentation.
Patent Information
- Application Number
- CN202610998241.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-06
- Publication Date
- 2026-11-10
AI Technical Summary
Existing dehydration agents suffer from thermal degradation and dehydration curling of the molecular skeleton under extreme high temperature and high salt conditions, leading to sealing failure. They are difficult to balance static anti-settling and dynamic rheological properties. Furthermore, traditionally prepared products are prone to salting out and clumping in high-salt working solutions, and their hydration and dissolution are slow.
Cellulose nanocrystals are used as a rigid framework material, and bio-based zwitterionic monomers are grafted as flexible functional segments. A green macromolecular network is constructed by combining choline chloride and tannic acid. Natural dolomite micro powder is used as a template agent. A porous extrudate is prepared by mechanical and chemical reaction through a twin-screw extruder and then rapidly cooled and solidified to form an environmentally friendly weight-reducing water loss agent.
Maintaining the extended state of polymer chains under extreme high temperature and high salinity conditions forms a dense sludge cake, reduces filtration loss, improves the shear dilution and static anti-sedimentation ability of the fluid, and achieves rapid hydration and dissolution with zero wastewater discharge.
Smart Images

Figure CN123063149A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of oil well working fluid technology, specifically to an environmentally friendly weighting fluid loss reducing agent suitable for high-temperature, high-salinity oil wells and its preparation process. Background Technology
[0002] As global oil and gas exploration and development continues to advance into deeper, ultra-deeper formations and more complex geological conditions, drilling and completion operations frequently encounter the dual challenges of extreme high temperatures and high salinity (such as salt-gypsum layers). The working fluid system, as the lifeblood of wellbore safety, directly determines the success or failure of drilling due to its performance stability. Fluid loss control agents, as one of the core treatment agents in the working fluid, are mainly used to seal formation microfractures and pores, controlling fluid loss into the formation. In deep wells with high-density weighted fluids, not only must the fluid loss control agent withstand extreme temperature and salinity environments, but the entire fluid system must also possess excellent rheological properties and barite suspension capabilities.
[0003] However, conventional synthetic polymer fluid loss reducers (such as ternary or multi-component copolymers containing AMPS) are prone to thermal degradation and breakage of the main chain of conventional carbon polymers when facing high temperature and high salinity conditions, leading to the collapse of the physical framework. At the same time, in a high-concentration brine environment, a large number of metal cations will generate a strong electrostatic shielding effect, forcing the polymer molecular chains to undergo severe dehydration and curling. This dual damage causes the polymer chain segments to be unable to maintain a stretched state in the well wall pores, resulting in the mud cake becoming loose and filled with micropores, and the filtration loss at high temperature and high pressure rapidly getting out of control.
[0004] Meanwhile, in the engineering application of high-density weighting working fluids in deep wells, in order to prevent the weighting material from settling and dehydrating under high temperature and static conditions, the existing technology generally adopts the method of blindly increasing the amount of polymer thickener, attempting to suspend particles by significantly increasing the apparent viscosity of the liquid phase. This passive lifting method relying on high viscosity will cause the fluid system to generate extremely high circulating equivalent density (ECD) when pumped in the tubing string, which seriously damages the shear dilution and rheological properties of the mud. When operating in formations with narrow safety density windows, this high-viscosity fluid is very likely to cause well leakage accidents. Therefore, based on the above-mentioned problems, this invention designs an environmentally friendly weighting fluid loss reducing agent and its preparation process suitable for high-temperature and high-salinity oil wells. Summary of the Invention
[0005] To address the shortcomings of existing technologies, this invention provides an environmentally friendly weighting fluid loss reducing agent suitable for high-temperature, high-salinity oil wells and its preparation process. It solves the problems of existing fluid loss reducing agents failing to seal due to thermal degradation and dehydration of the molecular skeleton under extreme high-temperature and high-salinity environments, difficulty in achieving both static anti-settling and dynamic rheological properties in high-density weighting fluids, and the extremely dense physical structure of traditionally prepared products leading to easy salting out and agglomeration in high-salinity working fluids and extremely slow hydration and dissolution.
[0006] To achieve the above objectives, the present invention provides the following technical solution: an environmentally friendly weighting fluid loss reducing agent suitable for high-temperature, high-salinity oil wells, wherein the composition for preparing the fluid loss reducing agent comprises the following components by weight:
[0007] 100 parts of cellulose nanocrystals;
[0008] 40-80 parts of bio-based zwitterionic monomer;
[0009] 30-50 parts of choline chloride;
[0010] Tannins 20-40 parts;
[0011] 3-8 parts of natural dolomite powder;
[0012] 0.5-1.5 parts of solid-phase free radical initiator.
[0013] A preferred preparation process for an environmentally friendly weighting fluid loss reducing agent suitable for high-temperature, high-salinity oil wells includes the following steps:
[0014] S1. Choline chloride and tannic acid are mixed and heated, and natural dolomite micro powder is added for constant temperature complexation to obtain a liquid templated natural eutectic solvent.
[0015] S2. Dry-mix cellulose nanocrystals, bio-based zwitterionic monomers and solid-phase free radical initiators to obtain a uniform solid-phase premix.
[0016] S3. The solid premix and the liquid templated natural eutectic solvent are simultaneously and continuously fed into a twin-screw extruder. Under the condition of no added free water and organic solvent, the mixed material passes through the plasticizing and wetting zone, the high-shear grafting reaction zone and the negative pressure phase change pore-forming zone in the twin-screw extruder in sequence, where a mechanochemical reaction occurs and in-situ gas phase pore-forming occurs, resulting in a porous extrudate.
[0017] S4. The porous extrudate is rapidly cooled and solidified, and the solidified porous extrudate is crushed and sieved to obtain the finished powder, which is the environmentally friendly weighting and water loss reducing agent suitable for high-temperature and high-mineralization oil wells.
[0018] Preferably, the specific operation for step S1 is as follows:
[0019] After mixing the choline chloride and the tannic acid, stirring is started, and the mixture is heated to 60-80°C at a heating rate of 2-5°C / min. The natural dolomite powder is added at a uniform rate at 60-80°C, and the mixture is stirred at a constant temperature of 60-80°C for 30-45 minutes to obtain the liquid templated natural eutectic solvent.
[0020] Preferably, the specific operation for step S2 is as follows:
[0021] At room temperature of 20-30℃, the cellulose nanocrystals, the bio-based zwitterionic monomers, and the solid-phase free radical initiator are mixed using a high-speed mixer. The spindle speed of the high-speed mixer is set to 1500-2000 r / min, and the continuous dry mixing time is 10-15 minutes to obtain the homogeneous solid-phase premix.
[0022] Preferably, the operation of simultaneously and continuously feeding the solid premix and the liquid templated natural eutectic solvent into the twin-screw extruder is specifically as follows:
[0023] The twin-screw extruder has a length-to-diameter ratio of 40:1 to 48:1, and the screw spindle speed is set to 150-300 r / min. The solid premix is quantitatively fed into the twin-screw extruder through the main feeder, and the liquid templated natural eutectic solvent is synchronously injected into the twin-screw extruder according to the mass ratio through the side metering pump.
[0024] Preferably, within the plasticizing impregnation zone of the twin-screw extruder:
[0025] The barrel temperature is controlled at 80-95℃, and the screw configuration adopts a forward conveying thread, so that the liquid templated natural eutectic solvent wets the solid premix, forming a semi-solid molten material.
[0026] Preferably, within the high-shear grafting reaction zone of the twin-screw extruder:
[0027] The barrel temperature is controlled at 100-115℃; the screw configuration of the high-shear grafting reaction zone is equipped with 3-5 sets of kneading blocks with a staggered angle of 45 degrees to 90 degrees.
[0028] Preferably, within the negative pressure phase change pore-forming region of the twin-screw extruder:
[0029] The barrel temperature is controlled at 125-135℃; at the same time, the vacuum exhaust port at the top of the barrel in the negative pressure phase change pore-forming section is opened, and the absolute pressure in this area is stably controlled within the range of -0.08MPa to -0.095MPa, so as to achieve the in-situ gas phase pore-forming.
[0030] Preferably, the specific operation of rapidly cooling and solidifying the porous extrudate is as follows:
[0031] The porous extrudate extruded from the twin-screw extruder falls into the air-cooled conveyor belt. Under strong air cooling, the porous extrudate is rapidly cooled to below 40°C within 1-3 minutes to obtain the solidified porous extrudate.
[0032] Preferably, the specific operation of pulverizing and sieving the cured porous extrudate to obtain the finished powder is as follows:
[0033] The solidified porous extrudate is pulverized using a dry ultrafine pulverizer, and the finished powder with a particle size in the range of 100-200 mesh is collected by a vibrating screen.
[0034] This invention provides an environmentally friendly weighting fluid loss reducing agent suitable for high-temperature, high-salinity oil wells and its preparation process. It has the following beneficial effects:
[0035] 1. This invention constructs a green macromolecular network that combines rigidity and flexibility, resisting temperature and salt, by using cellulose nanocrystals as a rigid framework material and grafting bio-based zwitterionic monomers as flexible functional segments. This effectively prevents the polymer chains from thermally degrading and curling, allowing the polymer segments to remain highly extended even when the salt concentration increases. This enables dense filling of wellbore pores under extremely harsh working conditions, forming a thin, dense, and highly resilient mud cake, which significantly reduces the filtration loss of high-temperature and high-pressure fluids.
[0036] 2. This invention introduces tannic acid containing a large number of polyphenol groups into the composition and innovatively uses natural dolomite micro powder as a sacrificial template agent for its early isothermal complexation protection, successfully establishing a competitive dynamic coordination anti-settling system based on polyphenol groups. This effectively breaks the limitation of traditional working fluids relying on blind thickening to suspend barite, and endows the fluid with excellent shear dilution properties and excellent high-density static anti-settling control ability.
[0037] 3. This invention utilizes a sudden drop in absolute pressure and a rapid rise in high temperature zone at the end of a twin-screw extruder to induce subcritical phase change flash evaporation and in-situ gas phase pore formation using trace amounts of bound water in the system. This is closely linked to a rapid cooling process using strong air cooling after extrusion, resulting in a rich internal micro-nano capillary network in the polymer. This allows the fluid to instantly flow into the polymer through the interconnected channels when the dehydration agent powder is added to a high-concentration composite brine solution. This completely overcomes the problem of "salting out and clumping" in high-salt environments, achieving rapid hydration and dissolution of the product within a very short time.
[0038] 4. This invention constructs a liquid, templated natural eutectic solvent by mixing and heating choline chloride as a hydrogen bond acceptor with tannic acid in situ. This solvent is then used directly as the core reaction medium and modified precursor of the composition, achieving a truly atom-economical reaction design. This preparation process does not require the addition of any additional free water or volatile organic solvents in the subsequent extrusion reaction, completely eliminating the industrial drawbacks of high water consumption, high energy consumption, and difficult waste treatment in traditional aqueous solution polymerization or reverse emulsion polymerization. It not only ensures the product's fully bio-based and environmentally friendly biodegradable properties from the source of raw materials, but also achieves green and clean manufacturing with zero wastewater and zero VOC emissions.
[0039] 5. This invention achieves efficient in-situ grafting and structural shaping of polymer components by decoupling and separating the solid-phase skeleton raw material dry mixing with the liquid-phase complexing medium for feeding, combined with a multi-temperature zone twin-screw extruder to perform a solvent-free mechanochemical linkage reaction. This ensures that when tannic acid is subjected to the high-intensity shear force field generated by the kneading block, its polyphenolic active groups will not undergo high-temperature self-crosslinking or carbonization deactivation, thus preserving the functional active core groups intact for end applications, improving the reliability of the water loss reducing agent product performance and the stability of continuous industrial production. Attached Figure Description
[0040] Figure 1 This is a schematic diagram of the preparation method of the present invention;
[0041] Figure 2 This is one of the schematic diagrams of the preparation method of the present invention;
[0042] Figure 3 This is a second schematic diagram of the preparation method of the present invention;
[0043] Figure 4 This is the third schematic diagram of the preparation method of the present invention;
[0044] Figure 5 This is the fourth schematic diagram of the preparation method of the present invention;
[0045] Figure 6 This is the fifth schematic diagram of the preparation method of the present invention;
[0046] Figure 7 This is the sixth schematic diagram of the preparation method of the present invention;
[0047] Figure 8 This is the seventh schematic diagram of the preparation method of the present invention. Detailed Implementation
[0048] The technical solutions in the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0049] Please see the appendix Figure 1 -Appendix Figure 8 This invention provides an environmentally friendly weighting fluid loss reducing agent suitable for high-temperature, high-salinity oil wells. The composition for preparing the fluid loss reducing agent comprises the following components by weight:
[0050] 100 parts of cellulose nanocrystals;
[0051] 40-80 parts of bio-based zwitterionic monomer;
[0052] 30-50 parts of choline chloride;
[0053] Tannins 20-40 parts;
[0054] 3-8 parts of natural dolomite powder;
[0055] 0.5-1.5 parts of solid-phase free radical initiator;
[0056] Specifically, the raw materials for preparing the dehydration reducer composition include the following components: 100 parts of cellulose nanocrystals (CNC); 40-80 parts of bio-based zwitterionic monomers (such as methacryloyloxyethyl sulfobetaine, SBMA); 30-50 parts of choline chloride; 20-40 parts of tannic acid; 3-8 parts of natural dolomite micropowder (particle size 800-1250 mesh); and 0.5-1.5 parts of solid-phase free radical initiator (such as potassium persulfate or ammonium persulfate).
[0057] The preparation process of an environmentally friendly weighting fluid loss reducing agent suitable for high-temperature, high-salinity oil wells includes the following steps:
[0058] S1. Choline chloride and tannic acid are mixed and heated, and natural dolomite micro powder is added for isothermal complexation to obtain a liquid templated natural eutectic solvent. The specific operation of the above steps is as follows: after mixing choline chloride and tannic acid, stirring is started, and the temperature is heated to 60-80℃ at a heating rate of 2-5℃ / min. Natural dolomite micro powder is added uniformly at 60-80℃, and the temperature is maintained at 60-80℃ and stirred for 30-45 minutes to obtain a liquid templated natural eutectic solvent.
[0059] Specifically, the core objective of this step is to synthesize in situ a templated natural eutectic solvent that functions as both a green solvent and a modifier.
[0060] In the specific operation, 30-50 parts of choline chloride (as hydrogen bond acceptor) and 20-40 parts of tannic acid (as hydrogen bond donor and polyphenol modification precursor) are put into a closed reaction vessel equipped with mechanical stirring and heating jacket. Then, the stirring is turned on and the speed is set to 200-400 r / min. The temperature is increased to 60-80℃ at a heating rate of 2-5℃ / min. Within this temperature range, strong hydrogen bond self-assembly occurs between choline chloride and tannic acid molecules, and the system gradually changes from solid powder to a uniform dark viscous liquid.
[0061] During this liquefaction process, 3-8 parts of natural dolomite micro powder are added to the reactor at a uniform rate, and the mixture is kept at a constant temperature of 60-80℃ and stirred for 30-45 minutes. From the reaction mechanism, the natural dolomite micro powder will slowly release trace amounts of [unclear - possibly a specific substance or quantity] in a weakly acidic polyphenol environment. and These divalent metal ions undergo transient weak coordination complexation with some polyphenol groups in the tannic acid molecule. This complexation process forms a sterically hindered ionic template protective layer on the surface of the polyphenol active site, which can prevent the tannic acid from undergoing deep cross-linking or oxidative deactivation during the subsequent high-temperature and high-shear extrusion process. This ensures that the polyphenol groups with complexing activity are well preserved in the final polymer product. After the reaction is completed, the resulting liquid material is transferred to a liquid storage tank and kept at 50-60℃ to maintain its liquid rheological properties, which facilitates subsequent pumping and injection.
[0062] S2. Dry-mix cellulose nanocrystals, bio-based zwitterionic monomers, and solid-phase free radical initiators to obtain a homogeneous solid-phase premix. The specific operation of the above steps is as follows: At room temperature of 20-30℃, use a high-speed mixer to mix cellulose nanocrystals, bio-based zwitterionic monomers, and solid-phase free radical initiators. The spindle speed of the high-speed mixer is set to 1500-2000 r / min, and the continuous dry-mixing time is 10-15 minutes to obtain a homogeneous solid-phase premix.
[0063] Specifically, this step aims to provide a highly uniformly dispersed solid framework and monomer substrate for the subsequent extrusion reaction, thereby decoupling the reaction medium (S1 product) from the reaction framework (S2 product) in terms of physical morphology.
[0064] In the specific operation, at a room temperature of 20-30℃, 100 parts of cellulose nanocrystals with extremely high rigidity and heat resistance (length-to-diameter ratio 10:1 to 50:1), 40-80 parts of bio-based zwitterionic monomers, and 0.5-1.5 parts of solid-phase free radical initiator are put into a high-speed mixer. The spindle speed of the mixer is set to 1500-2000 r / min, and the mixture is continuously dry-mixed for 10-15 minutes. The high-speed shear mixing can break the electrostatic agglomeration of cellulose nanocrystal particles, so that the zwitterionic monomer powder and initiator are uniformly coated on the surface of the cellulose skeleton, and a uniform solid-phase premix is obtained. This premix does not have reactivity at room temperature, which ensures the stability of the feed.
[0065] S3. The solid premix and liquid templated natural eutectic solvent are simultaneously and continuously fed into a twin-screw extruder. Without the addition of free water or organic solvents, the mixed material passes sequentially through a plasticizing and wetting zone, a high-shear grafting reaction zone, and a negative-pressure phase change pore-forming zone within the twin-screw extruder, undergoing a mechanochemical reaction and in-situ gas-phase pore formation to obtain a porous extrudate. Specifically, the length-to-diameter ratio of the twin-screw extruder is 40:1 to 48:1, and the screw spindle speed is set to 150-300 r / min. The solid premix is fed through a main feeder... Liquid templated natural eutectic solvent is simultaneously injected into the twin-screw extruder via a side metering pump according to the mass ratio. In the plasticizing and wetting zone of the twin-screw extruder, the barrel temperature is controlled at 80-95℃, and the screw configuration adopts a forward feeding thread, allowing the liquid templated natural eutectic solvent to wet the solid premix, forming a semi-solid molten material. In the high-shear grafting reaction zone of the twin-screw extruder, the barrel temperature is controlled at 100-115℃; the screw configuration in the high-shear grafting reaction zone is equipped with 3-5 sets of kneading blocks with a staggered angle of 45 degrees to 90 degrees. In the negative pressure phase change pore-forming zone of the twin-screw extruder, the barrel temperature is controlled at 125-135℃; simultaneously, the vacuum exhaust port at the top of the barrel in the negative pressure phase change pore-forming zone is opened, and the absolute pressure in this zone is stably controlled within the range of -0.08MPa to -0.095MPa to achieve in-situ gas phase pore formation.
[0066] Specifically, this step is the core linkage of the preparation process. The solvent-free mechanochemical method is used to achieve in-situ grafting and structural shaping of the polymer. A co-rotating parallel twin-screw extruder with an aspect ratio of 40:1 to 48:1 is used, and the screw spindle speed is set to 150-300 r / min.
[0067] First, the solid premix is quantitatively and continuously fed into the extruder via the main feeder. Simultaneously, liquid templated natural eutectic solvent is injected in proportion via a side metering pump. Under the propulsion of the twin screws, the material sequentially passes through three specific temperature and pressure control zones:
[0068] In the plasticizing and wetting zone (barrel temperature 80-95℃, forward conveying thread section), the eutectic solvent system acts as a green plasticizer, rapidly penetrating into the solid premix. By adjusting the temperature in this zone below the initiator's half-life activation temperature, it ensures that the material undergoes only physical phase fusion at this stage, forming a semi-solid molten material with a certain degree of fluidity, thus avoiding premature reaction and blockage.
[0069] The material then enters the high-shear grafting reaction zone (barrel temperature 100-115℃). This zone contains 3-5 sets of kneading blocks with a staggered angle of 45 to 90 degrees. Under the combined activation of the strong shear force field generated by the kneading blocks and the heat energy of 100-115℃, the initiator decomposes to generate free radicals, triggering the grafting copolymerization of zwitterionic monomers and tannic acid carrying a protective template onto the cellulose nanocrystal framework. At this time, the polyphenolic groups of the tannic acid are subjected to... The template locking protection maintains the integrity of the structure under strong mechanical shearing, while the grafting of zwitterionic monomers endows the matrix with anti-polyelectrolyte effect, that is, the molecular chains are in an extended state under high salt environment.
[0070] Finally, the material enters the negative pressure phase change pore-forming zone (the barrel temperature suddenly rises to 125-135℃). This section is connected to the vacuum exhaust port, which stabilizes the absolute pressure within the range of -0.08MPa to -0.095MPa. Under the sudden high temperature and negative pressure, the trace amount of bound water carried by choline chloride in the eutectic solvent system reaches a subcritical state and undergoes instantaneous vaporization and flash evaporation. The rapid expansion of the gas phase opens up a large number of micro- and nano-scale interconnected pores in situ inside the molten polymer matrix. Thus, without the addition of external chemical foaming agents, the design of the internal capillary pore network of the water loss reducing agent is completed purely by physical phase change, resulting in a porous extruder.
[0071] S4. Rapidly cool and solidify the porous extrudate, then pulverize and sieve the solidified porous extrudate to obtain the finished powder, which is an environmentally friendly weighting fluid loss reducing agent suitable for high-temperature, high-salinity oil wells. The specific operation of the above steps is as follows:
[0072] The porous extrudate extruded from the twin-screw extruder falls into the air-cooled conveyor belt. Under strong air cooling, the porous extrudate is rapidly cooled to below 40°C within 1-3 minutes to obtain solidified porous extrudate. The solidified porous extrudate is then pulverized and sieved to obtain finished powder. The specific operation is as follows: the solidified porous extrudate is pulverized using a dry ultrafine pulverizer, and finished powder with a particle size in the range of 100-200 mesh is collected by a vibrating screen.
[0073] Specifically, this step involves the solidification and engineering morphology processing of the special microscopic physical structure obtained in the above steps;
[0074] In the specific operation, the porous extrudate (which is still in a high-temperature molten and highly elastic state) extruded from the twin-screw extruder die is directly dropped onto the air-cooled conveyor belt. Under the strong air cooling effect, the porous extrudate is rapidly cooled to below 40°C within 1-3 minutes. The rapid cooling exceeds the glass transition temperature of the polymer, so that the micro-nano porous structure formed in the above steps is instantly frozen and solidified, preventing the pores from collapsing due to the flow of the polymer matrix and the effect of gravity.
[0075] Finally, the solidified porous extrudate was pulverized using a dry ultrafine pulverizer, and the finished powder with a particle size in the range of 100-200 mesh was collected by a vibrating screen. Within this particle size range, combined with the micropores formed by phase transformation within the material, when the finished product is introduced into the high-salinity working fluid of the oilfield, the fluid can instantly enter the interior of the powder through capillary force, driving the rapid hydration and expansion of the zwitterionic chain segments. At the same time, the exposed protected polyphenol groups encounter the large amount of barite weighting material in the working fluid (provided by...). When this occurs, competitive ion exchange takes place, releasing the originally weakly coordinated ions. , and turned to A dynamic supramolecular complex network is formed.
[0076] To demonstrate the innovation of this invention in terms of synergistic formulation and preparation process, the following examples and comparative examples are designed:
[0077] Example 1: An environmentally friendly weight-reducing water loss agent prepared in the above steps;
[0078] Comparative Example 1: Compared with Example 1, the difference is that no natural dolomite powder was added to the composition, and in step S1, only choline chloride and tannic acid were mixed and heated to prepare a liquid medium, while the rest were the same.
[0079] Comparative Example 2: Compared with Example 1, the difference is that tannic acid was not added to the composition, and an equal mass of glycerol and choline chloride were mixed to replace the original liquid medium, while the rest were the same;
[0080] Comparative Example 3: Compared with Example 1, the difference is that the cellulose nanocrystals in the composition were replaced with an equal mass of ordinary microcrystalline cellulose, and all other aspects were the same;
[0081] Comparative Example 4: Compared with Example 1, the difference is that the bio-based zwitterionic monomer in the composition was replaced with an equal mass of conventional anionic monomer (2-acrylamido-2-methylpropanesulfonic acid, AMPS), and all other aspects were the same.
[0082] Comparative Example 5: Compared with Example 1, the difference is that the amount of natural dolomite powder added to the composition was set to 15 parts, and all other aspects were the same.
[0083] Comparative Example 6: Compared with Example 1, the difference is that the amount of bio-based zwitterionic monomer added to the composition was set to 20 parts, while the rest were the same;
[0084] Comparative Example 7: Compared with Example 1, the difference is that natural dolomite micro powder is not added in step S1, but natural dolomite micro powder is directly dry mixed with cellulose nanocrystals, bio-based zwitterionic monomers and solid-phase free radical initiators in step S2, and the rest are the same.
[0085] Comparative Example 8: Compared with Example 1, the difference is that the negative pressure phase change pore-forming operation in step S3 is omitted, the vacuum exhaust port is not opened in the third temperature zone, and the extrusion is completed under normal pressure. All other aspects are the same.
[0086] Comparative Example 9: Compared with Example 1, the difference is that the strong air cooling and rapid cooling solidification operation in step S4 is omitted, and the porous extruded material from the extruder die is placed at room temperature to cool naturally. All other aspects are the same.
[0087] The following test experiment is now prepared:
[0088] 1. Rapid hydration and dissolution performance test in high-mineralization brine systems
[0089] Experimental steps:
[0090] First, prepare 800 mL of a composite brine (a saturated / semi-saturated mixed brine containing 30% NaCl and 10% CaCl2) to simulate extremely high-mineralization formation water using sodium chloride (NaCl) and calcium chloride (CaCl2). Pour the solution into a stirring cup with a constant temperature jacket, and set the temperature to 25℃.
[0091] Turn on the top-mounted mechanical stirrer and set the speed to a constant 400 r / min;
[0092] Accurately weigh 16.0g of the water loss reducing agent sample to be tested (Example 1 and each comparative example), and evenly sprinkle it into the stirred compound salt water within 10 seconds, while starting the stopwatch to begin timing;
[0093] The apparent viscosity readings of liquids are continuously recorded using an online continuous rotational viscometer. As the sample dissolves and hydrates, the viscosity gradually increases and eventually levels off.
[0094] When the viscosity fluctuation is less than 2% within 5 consecutive minutes, it is considered that the hydration and dissolution have reached the limit equilibrium. The time taken for the viscosity to reach 90% of the final limit equilibrium value is recorded as the complete hydration time (min).
[0095] Rheological properties and shear dilution test before and after high temperature aging
[0096] Experimental steps:
[0097] Basic mud preparation: Add 16.0g sodium bentonite and 2.0g soda ash to 400mL of fresh water in sequence, pre-hydrate for 24 hours under high speed stirring (10000r / min), then add 36g of composite salt (simulating high salinity environment) and 8.0g of the test fluid loss reducing agent sample, stir at low speed for 30 minutes, and finally slowly add barite powder to increase the bulk density to 2.20g / cm³, and stir evenly to obtain the test fluid.
[0098] High-temperature aging: The fluid is placed in a stainless steel high-temperature aging tank, pressurized to 1.0 MPa by nitrogen gas (to prevent boiling), and placed in a high-temperature drum furnace for continuous hot aging at 200°C for 16 hours. After removal, it is allowed to cool naturally to room temperature.
[0099] Rheological test: The aged fluid was stirred for 5 minutes at high speed (600 r / min) on a six-axis rotational viscometer to eliminate thixotropy, and then the readings were taken at 600 r / min. and 300r / min The dial reading.
[0100] Data Calculation: Calculating Plastic Viscosity PV (mPa·s), yield value YP (Pa); Dynamic-plastic ratio = YP / PV. A higher dynamic-plastic ratio within a reasonable range indicates better shear dilution properties of the system, which is more conducive to pumping and rock carrying.
[0101] 3. High-temperature static anti-settlement performance test of high-density fluid
[0102] Experimental steps:
[0103] Using the exact same formulation and dosage steps as in Experiment 2, a test fluid with a density of 2.20 g / cm³ was prepared.
[0104] After the fluid is stirred at high speed until it is uniform, it is poured into a special stainless steel settling tube (aging tank), leaving an appropriate safety expansion space, and then sealed.
[0105] The settling tubes were placed vertically in a high-temperature oven and aged for 48 hours in an absolutely static environment at 200°C.
[0106] Remove the settling tube and force-cool it to room temperature with running water. Carefully open the sealing cap and use a special sampling syringe to extract 20 mL of fluid samples from the top and bottom of the liquid column, respectively.
[0107] The density of the top sample was determined using a high-precision mud hydrometer. ) and bottom sample density ( );
[0108] Calculate the static settlement factor SF The closer the SF value is to 0.50, the less sedimentation there is. The industry generally stipulates that SF>0.530 indicates a serious risk of barite sedimentation.
[0109] 4. High-temperature and high-pressure water loss reduction performance test under extreme high temperature and high salinity conditions
[0110] Experimental steps:
[0111] Take the fluid from Experiment 2 that has undergone hot rolling aging at 200℃ for 16 hours and pour it into the test cup of the high temperature and high pressure filtration analyzer (HTHP);
[0112] Fill the test cup with special filter paper that meets API standards, seal the test cup, and place it in a heating mantle to heat it to 200°C.
[0113] Connect the high-pressure nitrogen source and apply a pressure of 4.2 MPa to the main valve of the test cup and a pressure of 0.7 MPa to the back pressure valve to maintain a stable pressure difference of 3.5 MPa (500 psi) across the filter paper.
[0114] Open the bottom valve to start collecting the filtrate and start timing; collect for 30 minutes.
[0115] Close the bottom valve, record the total filtration loss (HTHP FL, unit: mL) collected in the graduated cylinder over 30 minutes, remove the test cup, pour out the residual mud, gently rinse the filter paper surface with a small stream of water, and observe and record the thickness and physical toughness of the mud cake.
[0116] The data from the four experiments are shown in the table below:
[0117] Test sample Hydration time (min) PV (mPa·s) after aging Dynamic plasticity ratio after aging (YP / PV) Static Settlement Factor (SF) High-temperature and high-pressure filtration loss (mL) Observation of the apparent state of the mud cake (brief description) Example 1 11.4 36 0.42 0.511 13.2 The clay cake is thin and dense, with excellent toughness and a smooth surface. Comparative Example 1 12.1 32 0.28 0.615 18.7 The mud cake is relatively thin, but its local microstructure is loose. Comparative Example 2 11.8 29 0.23 0.638 15.6 The mud cake is dense, and the mud slurry shows obvious stratification and water separation. Comparative Example 3 14.3 48 0.31 0.547 45.3 The mud cake is thick, spongy, and brittle. Comparative Example 4 11.2 34 0.39 0.526 59.8 Extremely thick and soft, the pores were completely not sealed. Comparative Example 5 15.6 62 0.19 0.591 21.4 Extremely viscous, poor flowability, and thick mud cake. Comparative Example 6 10.9 33 0.40 0.518 32.1 The mud cake is of medium thickness and contains visible micropores. Comparative Example 7 12.8 35 0.27 0.608 17.5 The mud cake is relatively dense, and the barite shows a clear tendency to sink. Comparative Example 8 56.7 37 0.41 0.514 14.0 Initially, the mud cake showed severe clumping, but after long-term hydration, its condition became acceptable. Comparative Example 9 49.3 38 0.39 0.512 14.5 Similar to Comparative Example 8, dissolution was extremely slow.
[0118] The macroscopic physicochemical performance test results in high-temperature, high-mineralization weighted fluids demonstrate that the embodiments of this invention exhibit superior high-temperature, high-pressure fluid loss control capabilities under extreme conditions. From a microscopic mechanism perspective, the rigid framework constructed with natural cellulose nanocrystals maintains excellent physical support under high-temperature environments, effectively preventing thermal degradation and breakage of molecular chains. Furthermore, the bio-based zwitterionic functional segments grafted onto it exhibit a unique anti-polyelectrolyte effect in high-concentration brine; that is, the higher the salt concentration, the more extended the polymer chains. In comparative tests, those without cellulose nanocrystals or with functional segments replaced by conventional anionic monomers showed a significant increase in high-temperature, high-pressure fluid loss, resulting in loose, brittle, or even completely unsealed pores in the mud cake. This fully demonstrates the synergistic effectiveness of the composition in terms of temperature and salt resistance, enabling dense filling of the well wall through extended molecular chains, thereby obtaining thin, dense, and highly resilient high-quality mud cakes.
[0119] Regarding rheological properties and high-density static anti-settling control, this invention innovatively introduces tannic acid and utilizes trace ions released from natural dolomite micropowder in the early stages of preparation for sacrificial template protection. This ensures that the polyphenolic active groups of tannic acid remain intact even after undergoing high shear damage in the mechanochemical reaction zone. When this water loss reducing agent is added to a working fluid rich in barite, the protected polyphenolic groups undergo competitive ion exchange with the barite surface, spontaneously forming a dynamic supramolecular complex network. This dynamic network endows the fluid with excellent shear dilution properties, manifested in the excellent dynamic-to-plastic ratio and a static sedimentation factor that is infinitely close to the ideal sedimentation-free state in the examples. In contrast, the comparative examples lacking polyphenolic groups, not using a dolomite template, or with incorrect process feeding sequence leading to high-temperature carbonization and deactivation of polyphenols all exhibited severe barite sedimentation.
[0120] The mechanochemical reaction extrusion process of this invention plays a decisive role in reshaping the dissolution and hydration rate of the final product. This invention applies a sudden temperature rise and negative pressure at the end of the extruder, causing a subcritical phase change flash evaporation of trace amounts of bound water in the liquid reaction medium. This in-situ expands the dense polymer matrix, followed by forced rapid air cooling to instantly freeze and lock this micro / nanoporous network. This allows the fluid to instantly flow into the polymer through the pores when the powder is sprinkled into the composite brine, driving the macromolecular chains to hydrate rapidly in a very short time. Data shows that in comparative examples where negative pressure pore formation or rapid cooling and solidification steps were omitted, the initial agglomeration in the high-salt environment was extremely severe due to the failure of pore formation or rapid collapse and closure under gravity and residual high temperature, resulting in a significantly prolonged complete hydration time.
[0121] In summary, this invention provides an environmentally friendly weighting fluid loss reducing agent suitable for high-temperature, high-salinity oil wells and its preparation process. By using cellulose nanocrystals as a rigid framework material and grafting bio-based zwitterionic monomers as flexible functional segments, a green macromolecular network with both rigidity and flexibility, resistant to temperature and salt, is constructed. The cellulose nanocrystals provide excellent physical support at high temperatures, effectively preventing the polymer chains from thermally degrading and curling. Meanwhile, the zwitterionic monomers exhibit a unique anti-polyelectrolyte effect in high-salinity brine, allowing the polymer segments to remain highly extended even as salt concentration increases. This enables dense filling of wellbore pores under extreme conditions, forming a thin, dense, and highly resilient mud cake, significantly reducing the fluid loss of high-temperature, high-pressure fluids. Furthermore, by introducing tannic acid containing a large number of polyphenolic groups into the composition and innovatively using natural dolomite micropowder as a sacrificial template agent for pre-constitutional isothermal complexation protection, a competitive dynamic coordination anti-settling system based on polyphenolic groups has been successfully established. When this water loss reducing agent is added to a high-density working fluid rich in barite, the protected polyphenol groups can compete with the barite surface for ion exchange, spontaneously forming a dynamic supramolecular complex network. When stationary, it firmly supports the weighted material, and when subjected to shear pumping, it breaks down rapidly. This effectively breaks the limitation of traditional working fluids that rely on blind thickening to suspend barite, and endows the fluid with excellent shear dilution properties and excellent high-density static anti-settling control capabilities.
[0122] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
Claims
1. An environmentally friendly weighting fluid loss reducing agent suitable for high-temperature, high-salinity oil wells, characterized in that, The composition for preparing the water loss reducing agent comprises the following components in parts by weight: 100 parts of cellulose nanocrystals; 40-80 parts of bio-based zwitterionic monomer; 30-50 parts of choline chloride; Tannins 20-40 parts; 3-8 parts of natural dolomite powder; 0.5-1.5 parts of solid-phase free radical initiator.
2. A preparation process for an environmentally friendly weighting fluid loss reducing agent suitable for high-temperature, high-salinity oil wells, characterized in that, The environmentally friendly weighting fluid loss reducing agent for high-temperature, high-salinity oil wells according to claim 1 comprises the following steps: S1. Choline chloride and tannic acid are mixed and heated, and natural dolomite micro powder is added for constant temperature complexation to obtain a liquid templated natural eutectic solvent. S2. Dry-mix cellulose nanocrystals, bio-based zwitterionic monomers and solid-phase free radical initiators to obtain a uniform solid-phase premix. S3. The solid premix and the liquid templated natural eutectic solvent are simultaneously and continuously fed into a twin-screw extruder. Under the condition of no added free water and organic solvent, the mixed material passes through the plasticizing and wetting zone, the high-shear grafting reaction zone and the negative pressure phase change pore-forming zone in the twin-screw extruder in sequence, where a mechanochemical reaction occurs and in-situ gas phase pore-forming occurs, resulting in a porous extrudate. S4. The porous extrudate is rapidly cooled and solidified, and the solidified porous extrudate is crushed and sieved to obtain the finished powder, which is the environmentally friendly weighting and water loss reducing agent suitable for high-temperature and high-mineralization oil wells.
3. The preparation process of the environmentally friendly weighting fluid loss reducing agent suitable for high-temperature, high-salinity oil wells according to claim 2, characterized in that, The specific operation for step S1 is as follows: After mixing the choline chloride and the tannic acid, stirring is started, and the mixture is heated to 60-80°C at a heating rate of 2-5°C / min. The natural dolomite powder is added at a uniform rate at 60-80°C, and the mixture is stirred at a constant temperature of 60-80°C for 30-45 minutes to obtain the liquid templated natural eutectic solvent.
4. The preparation process of the environmentally friendly weighting fluid loss reducing agent suitable for high-temperature, high-salinity oil wells according to claim 2, characterized in that, The specific operation for step S2 is as follows: At room temperature of 20-30℃, the cellulose nanocrystals, the bio-based zwitterionic monomers, and the solid-phase free radical initiator are mixed using a high-speed mixer. The spindle speed of the high-speed mixer is set to 1500-2000 r / min, and the continuous dry mixing time is 10-15 minutes to obtain the homogeneous solid-phase premix.
5. The preparation process of the environmentally friendly weighting fluid loss reducing agent suitable for high-temperature, high-salinity oil wells according to claim 2, characterized in that, The specific operation of simultaneously and continuously feeding the solid premix and the liquid templated natural eutectic solvent into the twin-screw extruder is as follows: The twin-screw extruder has a length-to-diameter ratio of 40:1 to 48:1, and the screw spindle speed is set to 150-300 r / min. The solid premix is quantitatively fed into the twin-screw extruder through the main feeder, and the liquid templated natural eutectic solvent is synchronously injected into the twin-screw extruder according to the mass ratio through the side metering pump.
6. The preparation process of the environmentally friendly weighting fluid loss reducing agent suitable for high-temperature, high-salinity oil wells according to claim 2, characterized in that, Within the plasticizing impregnation zone of the twin-screw extruder: The barrel temperature is controlled at 80-95℃, and the screw configuration adopts a forward conveying thread, so that the liquid templated natural eutectic solvent wets the solid premix, forming a semi-solid molten material.
7. The preparation process of the environmentally friendly weighting fluid loss reducing agent suitable for high-temperature, high-salinity oil wells according to claim 2, characterized in that, Within the high-shear grafting reaction zone of the twin-screw extruder: The barrel temperature is controlled at 100-115℃; the screw configuration of the high-shear grafting reaction zone is equipped with 3-5 sets of kneading blocks with a staggered angle of 45 degrees to 90 degrees.
8. The preparation process of the environmentally friendly weighting fluid loss reducing agent suitable for high-temperature, high-salinity oil wells according to claim 2, characterized in that, Within the negative pressure phase change pore-forming region of the twin-screw extruder: The barrel temperature is controlled at 125-135℃; at the same time, the vacuum exhaust port at the top of the barrel in the negative pressure phase change pore-forming section is opened, and the absolute pressure in this area is stably controlled within the range of -0.08MPa to -0.095MPa, so as to achieve the in-situ gas phase pore-forming.
9. The preparation process of the environmentally friendly weighting fluid loss reducing agent suitable for high-temperature, high-salinity oil wells according to claim 2, characterized in that, The specific steps for rapidly cooling and solidifying the porous extrudate are as follows: The porous extrudate extruded from the twin-screw extruder falls into the air-cooled conveyor belt. Under strong air cooling, the porous extrudate is rapidly cooled to below 40°C within 1-3 minutes to obtain the solidified porous extrudate.
10. The preparation process of the environmentally friendly weighting fluid loss reducing agent suitable for high-temperature, high-salinity oil wells according to claim 2, characterized in that, The specific steps for pulverizing and sieving the cured porous extrudate to obtain the finished powder are as follows: The solidified porous extrudate is pulverized using a dry ultrafine pulverizer, and the finished powder with a particle size in the range of 100-200 mesh is collected by a vibrating screen.