A copper-based amorphous solder, its preparation method and application
By functionalizing and co-designing copper-based amorphous brazing filler metals and optimizing the manufacturing process, the problems of achieving both low melting point and high toughness, as well as melting point compatibility and compositional uniformity in existing copper-based amorphous brazing filler metals have been solved, achieving low-temperature brazing of ultra-thin copper and copper alloy pipes.
Patent Information
- Application Number
- CN202611360945.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-03
- Publication Date
- 2026-11-17
AI Technical Summary
Existing copper-based amorphous brazing fillers cannot simultaneously achieve both low melting point and high toughness. They have limited melting point compatibility, lack precise synergistic design in component ratio, and suffer from compositional segregation and dimensional inhomogeneity issues in their manufacturing processes, making it difficult to meet the brazing requirements of ultra-thin copper and copper alloy pipe fittings.
Through functional synergistic design, precise proportions of elements such as P, Sn, Ni, Si, Ce, Ga, and In are used, combined with a preparation process of graded gradient heating, pressure adjustment, and gradient speed spinning, to form a multi-element synergistic effect, which reduces the melting point and improves toughness and amorphous formation ability.
It achieves good toughness and wettability at a low melting point, ensuring the compositional uniformity and dimensional accuracy of amorphous brazing filler metal, and is suitable for low-temperature brazing of micron or nano-scale ultrathin copper and copper alloy pipes, reducing damage to the substrate structure.
Smart Images

Figure CN123103249A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of solder technology, specifically to a copper-based amorphous solder, its preparation method, and its application. Background Technology
[0002] Copper alloy pipe fittings, with their high strength, high toughness, excellent corrosion resistance, and good machinability, are widely used in mechanical parts, waveguides, radiators, and condenser piping. Thin-walled copper pipes, in particular, have been used in China for over thirty years due to their excellent machinability, and the corresponding brazing connection technology has also continuously developed. Copper-phosphorus (Cu-P) brazing filler metal, with its relatively low melting point, good fluidity and wettability, self-brazing properties, and low price, has become an important material for connecting copper and copper alloy pipe fittings.
[0003] Traditional Cu-P binary solders have a solidus temperature of approximately 710–925°C, resulting in a relatively high melting point. Furthermore, the high phosphorus (P) content easily forms the brittle Cu3P phase, leading to difficulties in solder processing and poor toughness. To improve these properties, existing technologies introduce elements such as tin (Sn), nickel (Ni), silicon (Si), cerium (Ce), and gallium (Ga) into the Cu-P binary system, forming a multi-element copper-based amorphous solder with a Cu-P-Sn-Ni matrix. However, this type of solder still has the following shortcomings in practical applications:
[0004] First, achieving both low melting point and high toughness is difficult. To achieve a low melting point, current technologies often use Ga as the core melting point reducing element. However, excessive Ga addition leads to embrittlement of the brazing filler metal strip, failing to meet the high toughness requirements for brazing ultra-thin copper tubes. Conversely, reducing the amount of Ga makes it difficult to achieve the desired low melting point. This performance contradiction limits the application of copper-based amorphous brazing filler metals in the connection of ultra-thin-walled tubes.
[0005] Secondly, the melting points of existing brazing filler metals are generally too high, limiting their adaptability to various processes. According to publicly available literature, CN114058980A discloses a Si-doped copper-phosphorus-tin-nickel amorphous solder with a melting point of 628-632℃; CN101530952A reports a boron-containing Cu-P-based amorphous brazing filler metal, whose melting point, while slightly lower, remains between 602-663℃; CN117038368A discloses a copper-phosphorus amorphous brazing filler metal for connecting tungsten sheets and copper rivets, with a brazing temperature even higher at 780-850℃. The melting temperatures of these filler metals are generally above 600℃, which is suitable for conventional thin-walled copper tubes, but still too high for micron- or even nanometer-scale ultrathin copper tubes. High brazing temperatures easily damage the microstructure of ultrathin substrates, leading to a significant decrease in the overall mechanical properties of the tube.
[0006] Third, the composition ratio lacks precise functional synergistic design. Existing technologies mostly involve the simple stacking of multiple trace elements without strictly defining the ratio between the core element, trace elements, and other components. This results in large fluctuations in solder performance, making it difficult to simultaneously achieve amorphous formation ability, wettability, and toughness.
[0007] Fourth, the manufacturing process has defects. In the melting stage, existing technologies generally use a one-time heating and constant vacuum process, which easily leads to component segregation, oxide inclusions, and the loss of low-melting-point elements, thus affecting the amorphous forming ability and mechanical uniformity. In the strip spinning stage, the constant rotation speed cooling method results in poor dimensional uniformity and large thickness deviation of the prepared amorphous strip, which cannot meet the stringent requirements for the dimensional accuracy of the brazing filler metal in ultra-thin copper tube brazing.
[0008] In summary, existing copper-based amorphous brazing fillers have significant shortcomings in terms of balancing low melting point and high toughness, melting point range, synergistic optimization of multi-component ratios, and control of manufacturing processes. They are unable to meet the comprehensive performance requirements of micron or nano-scale ultrathin copper and copper alloy pipe fittings for lower brazing temperatures, higher toughness, and better dimensional accuracy. Summary of the Invention
[0009] To address the shortcomings of existing technologies, this invention discloses a copper-based amorphous brazing filler metal, its preparation method, and its applications. This invention achieves the effects of lower melting point, improved toughness, improved dimensional accuracy, and enhanced welding performance through functionalized synergistic design of the brazing filler metal composition system and innovative optimization of the preparation process.
[0010] To achieve the above technical objectives, in a first aspect, the present invention provides a copper-based amorphous brazing filler metal, wherein, by mass percentage, the copper-based amorphous brazing filler metal comprises the following elemental composition: P: 5.8%~7.2%, Sn: 9.5%~12.0%, Ni: 5.8%~8.0%, Si: 0.2%~0.5%, Ce: 0.03%~0.06%, Ga: 0.3%~0.5%, In: 0.08%~0.25%, with the balance being Cu and mass percentage ≥71%; Wherein, the mass ratio of P to Sn is 1:(1.6~1.9), the mass ratio of Ga to In is (1.2~6.25):1, and the total mass ratio of Ni and Ce to Si is (15~25):(1~2).
[0011] In the above composition system, there are specific and interrelated synergistic effects among the elements. Copper (Cu), as the matrix element, has a content of not less than 71%, which is beneficial to ensuring the strength, formability and microstructure compatibility of the solder with the copper-based base material.
[0012] Phosphorus (P), as a core melting point reducing element, forms a eutectic structure with copper to lower the solder melting point. Simultaneously, P has the ability to reduce copper oxide, enabling flux-free brazing to a certain extent and improving fluidity. To avoid excessive formation of the Cu3P brittle phase due to excessive P content, this invention controls the mass ratio of P to Sn (tin) within the range of 1:(1.6~1.9). Sn, as an auxiliary melting point reducing element, can further lower the melting point and improve wettability. This ratio helps suppress the continuous precipitation of the brittle phase, thus balancing low melting point and toughness.
[0013] The addition of nickel (Ni) aims to improve the wettability and joint strength of the solder, and to strengthen the matrix structure. It should be noted that existing technologies (such as CN108381058A) generally consider the Ni content to be no more than 3%, otherwise it easily forms brittle phases such as Ni3P with P, reducing the solder's toughness. This invention proposes a Ni content of 5.8%~8.0%, significantly higher than this perceived upper limit. To achieve a performance balance at a higher Ni content, this invention simultaneously introduces Ce and Si, forming a Ni-Ce-Si multi-component synergistic system. Specifically, Ce can purify the alloy interface, reduce oxide inclusions, and work with Ni to suppress the continuous network precipitation of Ni3P; Si, as an amorphous modifier, helps refine the microstructure and improve amorphous formation ability, and its combination with Ni can further stabilize the amorphous structure. Furthermore, there is a synergistic effect between Ce and Si: Ce stabilizes the amorphous phase and improves wettability, while Si promotes nucleation refinement. The composite modified system formed by the two helps to suppress the precipitation of crystalline phases in amorphous ribbons during rapid cooling. Based on this, the present invention further limits the total mass ratio of Ni and Ce to Si to (15~25):(1~2) to ensure that the synergistic effect of the three is relatively fully realized within this ratio range.
[0014] Gallium (Ga) is a strong melting point reducing element, but excessive addition of it alone can easily lead to embrittlement of the solder strip. Therefore, this invention uses Ga in combination with indium (In), controlling the mass ratio of Ga to In at (1.2~6.25):1. In also has a melting point reducing effect and good atomic size matching with Ga. The combination of the two can improve the toughness reduction problem caused by the introduction of Ga alone while maintaining a low melting point. Simultaneously, Ga and In can form a eutectic toughening mechanism with Sn and Ni, further improving the toughness of the solder. Since Ni is also a key component of the Ni-Ce-Si multi-component synergistic system, the two achieve synergistic effects through sharing Ni, thereby suppressing the precipitation of brittle phases in the high Cu matrix and balancing the contradiction between low melting point and toughness.
[0015] The present invention constructs a synergistic design system with multi-element functionalized precise coordination through the above-mentioned method. This system can reduce the melting point of the brazing filler metal while maintaining good amorphous formation ability, wettability and toughness, thereby meeting the low-temperature brazing requirements of micron or nano-scale ultrathin copper and copper alloy pipes.
[0016] In a further example of the present invention, the copper-based amorphous solder comprises the following elemental composition by mass percentage: P: 6.0%~6.5%, Sn: 10.0%~11.5%, Ni: 6.0%~7.0%, Si: 0.3%~0.4%, Ce: 0.04%~0.05%, Ga: 0.4%~0.5%, In: 0.10%~0.20%, Cu: 73%~78%; Wherein, the mass ratio of P to Sn is 1:(1.6~1.8), the mass ratio of Ga to In is (2~5):1, and the mass ratio of the total mass of Ni and Ce to the mass of Si is (16~25):1; more preferably, the mass ratio of P to Sn is 1:(1.6~1.8), the mass ratio of Ga to In is (3~5):1, and the mass ratio of the total mass of Ni and Ce to the mass of Si is (19~24):1.
[0017] Secondly, the present invention also provides a method for preparing the copper-based amorphous solder described in any of the above examples, comprising the following steps: (1) Based on the mass percentage of each element in the copper-based amorphous brazing filler metal, calculate and weigh the corresponding raw materials according to the actual element content of each element and / or intermediate alloy raw material, and then perform pretreatment. (2) Place each of the raw materials in a smelting furnace and heat it at 6.0 × 10⁻⁶ ℃. -4 ~9.0×10 -4 Staged gradient heating melting under high vacuum conditions; (3) After all raw materials have melted, adjust the pressure inside the furnace to 1.0 × 10⁻⁶. -3 ~3.0×10 -3 Pa, then fill with high-purity argon gas to atmospheric pressure, and then cast into a water-cooled copper mold to obtain an alloy ingot; (4) The alloy ingot is heat-treated and crushed, then placed into a quartz tube with a nozzle, vacuumed and heated to melt, then argon gas is injected into the quartz tube and sprayed onto a copper roller rotating at a gradient speed for rapid cooling, and then separated by compressed air to obtain copper-based amorphous brazing filler metal.
[0018] The preparation method of this invention, through a combination of graded gradient heating, pressure adjustment, and gradient speed belt spinning, is adapted to the aforementioned multi-element synergistic composition system. Specifically, the graded gradient heating, through variations in multiple temperature ranges, allows dehydration and impurity removal, pre-melting of high-melting-point components, and final alloying to be completed in stages. This avoids directly exposing low-melting-point components (such as Ga and In) to the highest melting temperature environment, thereby reducing their volatility tendency, minimizing component segregation, and increasing the microstructure uniformity of the alloy ingot. Regarding pressure adjustment, under high vacuum conditions (6.0 × 10⁻⁶), -4 ~9.0×10 -4 Under high vacuum conditions, oxygen in the melt mainly exists in two forms: dissolved oxygen and oxide inclusions. While high vacuum conditions can reduce the equivalent partial pressure of dissolved oxygen in the melt, it is difficult to effectively remove oxide inclusions (such as Cu₂O and SnO₂) already formed inside the melt using only high vacuum conditions. This is because the interfacial energy between oxide inclusions and the melt is high, making them difficult to spontaneously float; secondly, the diffusion and mass transfer rate of dissolved oxygen is limited, resulting in slow deoxidation kinetics under high vacuum conditions. The furnace pressure was adjusted to 1.0 × 10⁻⁶ Pa. -3 ~3.0×10 -3 After Pa, this process condition promotes melt purification and compositional stability in several ways: 1.0 × 10 -3 ~3.0×10 -3 High-purity argon gas (purity ≥99.999%, oxygen content << 5ppm) is introduced at a pressure of Pa to create a slight airflow agitation, promoting convection within the melt and accelerating the floating and escape of oxide inclusions. Within this pressure range, the equivalent partial pressure of dissolved oxygen in the melt is slightly higher than under high vacuum conditions (6.0 × 10⁻⁶). -4 ~9.0×10 -4 The pressure of 1.0 × 10⁻⁶ Pa can create a suitable oxygen concentration gradient driving force, avoiding insufficient mass transfer driving force due to excessively low equivalent partial pressure of dissolved oxygen in the melt. Trace carbon impurities in the melt (from raw materials or crucibles) react with dissolved oxygen to generate CO. This pressure is conducive to the nucleation and growth of CO bubbles, which are then carried upwards and discharged through a bubble flotation mechanism, carrying oxygen inclusions. Simultaneously, 1.0 × 10⁻⁶ Pa… -3 ~3.0×10 -3 The pressure range maintains a certain deoxidation driving force without causing excessive volatilization of low-melting-point elements such as Ga and In due to excessively low pressure, nor inhibiting bubble escape due to excessively high pressure. Gradient speed strip spinning dynamically adjusts the copper roller speed during strip preparation to regulate the cooling rate. Compared to constant speed methods, this helps improve the thickness uniformity and dimensional accuracy of amorphous strips. Through the above process combination, this method can obtain copper-based amorphous solders with uniform composition, high purity, and good strip dimensional accuracy, thus stably realizing the performance advantages of the aforementioned composition system.
[0019] It should be noted that the purity of each raw material is not particularly limited in the preparation method of this invention. The actual weighing can be calculated based on the actual elemental content of the raw materials. For example, high-purity electrolytic copper with a purity ≥99.99% can be used as the Cu source; Sn, Ni, Ga, and In particles with a purity ≥97% can be used to provide the corresponding elements; P, Si, and Ce can be introduced through intermediate alloys, such as copper-phosphorus (85Cu-15P) intermediate alloys, copper-silicon (80Cu-20Si) intermediate alloys, and copper-cerium (80Cu-20Ce) intermediate alloys with Fe ≤0.1wt%.
[0020] It should be noted that in the preparation method of the present invention, the pretreatment of raw materials is a conventional pretreatment method, which can be exemplarily adopted as follows: sequentially polished with 2000-grit sandpaper, ultrasonically cleaned with acetone for 30 minutes, and vacuum dried at 80°C for 2 hours.
[0021] It should be noted that the present invention can be carried out using a vacuum induction melting furnace crucible. The melting equipment used here is only an example. Those skilled in the art can select other furnace types that can achieve vacuum melting according to actual conditions, and are not limited to the specific equipment mentioned above.
[0022] In a further example of the present invention, the graded gradient heating in step (2) includes three stages: First stage: Heat to 400-450℃ at a rate of 8-10℃ / min, and hold for 5-10 minutes; Second stage: Increase the temperature to 800-850℃ at a rate of 8-10℃ / min, and hold for 8-15 minutes; Third stage: Increase the temperature to 1100~1200℃ at a rate of 3~5℃ / min, and hold for 15~20min.
[0023] In the preparation method of the present invention, the first two stages of the graded gradient heating process in the melting process are completed at a lower temperature to remove water and impurities and pre-melt high-melting-point components, so as to avoid low-melting-point elements (Ga, In) being exposed to high-temperature environment too early; the third stage heats up to the final temperature at a slower rate and extends the holding time to make the whole component melt uniformly.
[0024] In a further example of the present invention, the heat treatment in step (4) is to place the alloy ingot in a vacuum muffle furnace and sequentially perform heating, heat preservation and furnace air cooling; The heating rate is 3~5℃ / min, and the temperature is raised to 560~590℃; the holding time is 4~6h.
[0025] This homogenization heat treatment can eliminate component segregation inside the ingot, optimize the dendritic structure, and improve the uniformity of the alloy structure, thereby enhancing the ability of amorphous phases to form during the subsequent strip spinning process, and providing a basis for ensuring the consistency of the brazing filler strip performance.
[0026] In a further example of the present invention, the vacuum level after vacuuming in step (4) is less than 5 × 10⁻⁶. -3 Pa; And / or, the heating and melting temperature in step (4) is 780~820℃ and the time is 5min.
[0027] In a further example of the present invention, the gradient rotation speed of the copper roller in step (4) includes two levels: First stage: Control the rotation speed at 25~26m / s and continue for 1~5 seconds for pre-cooling; Second stage: Increase the rotation speed to 30~32m / s for high-speed cooling.
[0028] In a further example of the present invention, the rapid cooling rate in step (4) is 6 × 10⁻⁶. 6 K / s ~3×10 7 K / s.
[0029] The rapid cooling rate is mainly related to the rotational speed of the copper roller; that is, the higher the rotational speed of the copper roller, the greater the cooling rate. Based on this principle, this invention controls the rotational speed of the copper roller within a specific range, so that the rapid cooling rate reaches 6 × 10⁻⁶. 6 K / s ~3×10 7 K / s.
[0030] In a further example of the present invention, the distance between the nozzle and the copper roller in step (4) is 1.2~1.4 mm; And / or, the pressure of the argon gas introduced in step (4) is 0.3~0.5MPa.
[0031] Thirdly, the present invention also provides an application of copper-based amorphous brazing filler metal as described in any example of the first aspect in the brazing of ultrathin copper and copper alloy pipe fittings, wherein the brazing temperature is 570~610℃.
[0032] In the application of this invention, the brazing temperature is 570~610℃. Compared to existing Cu-P-Sn-Ni based amorphous brazing filler metals, which generally require brazing temperatures above 600℃, the brazing filler metal provided by this invention can lower the brazing window to around 570℃. This lower brazing temperature is mainly achieved through the precise ratio of P to Sn in the aforementioned composition system, the melting point reduction of Ga and In through compounding, and the contribution of Ni-Ce-Si multi-component synergy to the microstructure stability. The lower brazing temperature helps reduce the tendency of ultrathin copper tube substrates to coarsen and soften at high temperatures, reducing the risk of damage to the microstructure of the base material, thereby better maintaining the mechanical properties and dimensional accuracy of the tube fittings. Simultaneously, the wetting and spreading behavior of the filler metal remains good within this temperature range, forming dense, high-strength brazed joints. Therefore, the filler metal of this invention is particularly suitable for brazing connections of micron- or nano-scale ultrathin copper and copper alloy tube fittings that are sensitive to heat input and require high dimensional accuracy.
[0033] In a further example of the present invention, when vacuum brazing is performed using the copper-based amorphous brazing filler metal, no additional flux is required, and the vacuum level during the brazing process is controlled at 5 × 10⁻⁶. -3 For temperatures below 10 Pa, the heat preservation time is 10-15 minutes.
[0034] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0035] (1) The copper-based amorphous brazing filler metal of the present invention can simultaneously improve the melting point, toughness, wettability, and amorphous formation capability of the filler metal through the functionalized synergistic coordination among multiple components. In terms of melting point reduction, the coupled ratio of P and Sn can exert the melting point reduction and self-fluxing effect of P, while using Sn to assist in melting point reduction and suppress excessive precipitation of Cu3P brittle phase, which helps to balance low melting point and high toughness. In terms of strengthening and toughening, breaking through conventional understanding, the Ni content is increased and a synergistic system is formed with Ce and Si. By utilizing the interface purification effect of Ce and the microstructure refinement effect of Si, the continuous precipitation of brittle phases such as Ni3P can be suppressed and the amorphous structure can be stabilized, thereby improving wettability and joint strength. In terms of amorphous formation, Ga and In are compounded in proportion. By utilizing the atomic size matching of the two, the melting point can be further reduced while mitigating the tendency of strip embrittlement that may be caused by single addition. Thus, the above component combination enables the filler metal to maintain good toughness, wettability, and amorphous formation capability at a lower melting point.
[0036] (2) The copper-based amorphous brazing filler metal preparation method of the present invention, through graded gradient heating, pressure adjustment, and gradient speed strip spinning, helps to obtain high-quality amorphous brazing filler metal with uniform composition, high purity, and consistent size. Graded gradient heating can complete dehydration and impurity removal, pre-melting of high-melting-point components, and final alloying in stages, which helps to reduce the high-temperature volatilization of low-melting-point elements such as Ga and In, thereby reducing component segregation. Pressure adjustment after melting can promote the floating and removal of oxide inclusions inside the melt, reduce heterogeneous nucleation cores, help stabilize amorphous formation ability, and improve the wetting and mechanical properties of the brazing filler metal. The gradient speed dynamic adjustment of the cooling rate during the strip spinning stage can improve the uniformity of strip thickness. The above process combination helps to fully reflect the potential performance of the composition system in the final product, thereby providing high-quality copper-based amorphous brazing filler metal with high strip size consistency for precision brazing.
[0037] (3) The copper-based amorphous brazing filler metal provided by the present invention can be used for brazing of ultra-thin copper and copper alloy pipes, and the required brazing temperature is low, and good brazing effect can be achieved in the range of 570~610℃. Attached Figure Description
[0038] The accompanying drawings, which form part of this application, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an undue limitation of the invention. In the drawings: Figure 1 The DSC curve of the copper-based amorphous solder of Embodiment 1 of the present invention is shown; Figure 2 The XRD patterns of copper-based brazing filler metals from Example 1 and Comparative Example 7 of the present invention are shown. Figure 3 The XRD patterns of copper-based brazing filler metals from Example 1 and Comparative Example 8 of the present invention are shown. Figure 4 The images show comparative photographs of copper-based brazing filler metals from Embodiment 8 of the present invention and Comparative Examples 1 and 3 after a 180° bending test. Figure 5 The metallographic structure of copper-based brazing filler metal in Example 8 of the present invention is shown in comparison with that in Comparative Example 4. Detailed Implementation
[0039] To facilitate understanding of the present invention, a more comprehensive description will be provided below, along with preferred embodiments. However, it should be understood that these embodiments are merely for more detailed explanation and should not be construed as limiting the invention in any way, i.e., not intended to limit the scope of protection of the invention.
[0040] Unless otherwise defined, all technical terms used in the following examples have the same meanings as commonly understood by those of ordinary skill in the art to which the present invention pertains. The chemical raw materials involved in the following examples are all conventional chemical raw materials unless otherwise specified; the experimental methods are all conventional methods unless otherwise specified.
[0041] It should be noted that, in order to verify the comprehensive properties of the copper-based amorphous brazing fillers obtained in the examples and comparative examples of the present invention, the following test methods are adopted to test six core indicators of the samples, namely amorphous forming ability, melting point, toughness, wettability, brazing shear strength and strip dimensional accuracy. The test methods are as follows: Amorphous forming ability test: An X-ray diffractometer (XRD, Cu target Kα ray) is used to analyze the structure of the brazing strip, with a scanning range of 2θ = 20° to 80° and a scanning speed of 5° / min. The amorphous forming ability of the brazing strip is judged according to whether there are sharp crystalline diffraction peaks in the XRD pattern: if the pattern shows a typical diffuse scattering peak without obvious sharp peaks, it indicates that the sample has an amorphous structure; if sharp crystalline diffraction peaks are superimposed on the background of the typical amorphous diffuse scattering peak, partial crystallization occurs.
[0042] Melting point and solidus / liquidus test: A high-low temperature differential scanning calorimeter (DSC) is used for the test, with a heating rate of 20°C / min, a test temperature range from room temperature to 1000°C, and a crucible made of high-temperature resistant Al₂O₃. The characteristic temperatures of the brazing filler are determined according to the DSC heating curve: the onset temperature of the first endothermic peak is defined as the solidus temperature, the end temperature of the last endothermic peak is defined as the liquidus temperature, and the melting point range of the brazing filler is expressed as from the solidus to the liquidus.
[0043] Toughness test: The flat plate bending method is used to qualitatively evaluate the toughness of the copper-based amorphous brazing strip. During the test, the distance between two parallel flat plates is set to twice the thickness of the strip, and the brazing strip is placed between the two flat plates for 180° bending. The judgment is graded according to the appearance state of the strip after bending: if there are no visible cracks on the surface of the strip after bending, no fracture on the side, and no delamination or spalling at the bend, it is judged as qualified; if microcracks appear on the surface (the crack length is less than 10% of the width of the strip) but the strip is not completely broken, it is judged as micro-cracked; if the strip is completely broken or through cracks appear during or after bending, it is judged as fractured.
[0044] Wettability test: The spread area method is used to evaluate the wettability of the brazing filler on the copper-based base material. The specific steps are as follows: a copper plate with a size of 50mm×50mm is prepared in advance as the base material, which is sequentially ground with 2000-mesh sandpaper and ultrasonically cleaned for 30min for later use. 100mg of the brazing strip to be tested is weighed, cut into pieces and stacked in the center of the copper plate. The copper plate is placed in a crucible in a high-temperature vacuum furnace, and the vacuum is pumped to a vacuum degree of no less than 5×10 -3Heating was started after Pa, with a test temperature of 680℃ and a holding time of 10 minutes. After cooling, the spreading area of the solder on the copper plate was measured, and the wettability was evaluated based on the size of the spreading area.
[0045] Brazing Shear Strength Test: The shear strength of the brazed joint was tested using a universal testing machine. Brazed specimens were prepared using an lap joint method: a 2mm thick copper plate was used as the base material, and the lap length was set to three times the plate thickness (6mm). Before brazing, the copper plate was polished and cleaned with 2000-grit sandpaper. 80mg of the copper-based amorphous brazing tape to be tested was placed at the lap joint, and a 100g crucible was placed in the overlapping area as a counterweight for fixation. The brazing temperature was 680℃, and the holding time was 10min. During the shear test, the shear rate was set to 1mm / min. Each group of samples was tested five times, and the average value was taken as the final shear strength.
[0046] Strip dimensional accuracy test: The thickness and width of the prepared brazing strip were measured using a digital micrometer (accuracy 0.001 mm). Ten test points were randomly selected on the strip, and the thickness and width values of each point were recorded to evaluate the dimensional uniformity and processing accuracy of the strip.
[0047] Example 1
[0048] This embodiment provides a copper-based amorphous solder, which, by mass percentage, comprises the following elemental composition: P: 6.0%, Sn: 10.0%, Ni: 6.0%, Si: 0.3%, Ce: 0.04%, Ga: 0.4%, In: 0.10%, with the balance being Cu: 77.16%. The mass ratio of P to Sn is 1:1.67, the mass ratio of Ga to In is 4:1, and the total mass ratio of Ni and Ce to Si is 20.13:1.
[0049] This embodiment prepares the copper-based amorphous solder with the above-mentioned composition according to the following steps: (1) Based on the mass percentage of each element in the copper-based amorphous solder, calculate and weigh the corresponding raw materials according to the actual element content of each element and / or intermediate alloy raw material. Specifically, high-purity electrolytic copper with a purity ≥99.99% is used as the Cu source; Sn, Ni, Ga, and In particles with a purity ≥97% are used to provide the corresponding elements; P, Si, and Ce are provided by copper-phosphorus (85Cu-15P) intermediate alloy, copper-silicon (80Cu-20Si) intermediate alloy, and copper-cerium (80Cu-20Ce) intermediate alloy with an Fe impurity content of 0.08wt%. The weighed raw materials are pretreated by grinding with 2000-mesh sandpaper, ultrasonic cleaning with acetone for 30 min, and vacuum drying at 80℃ for 2 h. (2) Place the pretreated raw material in the crucible of the vacuum induction melting furnace, seal it, and then evacuate it to 7×10⁻⁶.-4 Pa. A graded gradient heating melting process was carried out under high vacuum conditions. The specific procedure was as follows: the first stage involved heating to 450℃ at a rate of 10℃ / min and holding for 5 min; the second stage involved heating to 850℃ at a rate of 8℃ / min and holding for 8 min; the third stage involved heating to 1150℃ at a rate of 5℃ / min and holding for 15 min. (3) After all the raw materials have completely melted, adjust the pressure inside the furnace to 2.0 × 10⁻⁶. -3 Pa, maintain for 3 min. Then, introduce high-purity argon gas to atmospheric pressure, stir for 2 min, and then pour into a water-cooled copper mold to obtain an alloy ingot; (4) The obtained alloy ingot was placed in a vacuum muffle furnace for homogenization heat treatment: heated to 560°C at a heating rate of 5°C / min, held for 4 hours, and then air-cooled with the furnace. The heat-treated ingot was crushed into particles of φ5~10mm, loaded into a quartz tube with a boron nitride nozzle of 0.8mm aperture, and evacuated to 5×10⁻⁶. -3 After heating to 780℃ and holding for 5 minutes, 0.3 MPa argon gas was introduced into the quartz tube, and the melt was sprayed onto a copper roller rotating at a gradient speed for rapid cooling: the copper roller was first pre-cooled at 25 m / s for 1 second, and then increased to 30 m / s for high-speed cooling, while 0.2 MPa compressed air was used to detach the strip. The resulting amorphous brazing filler metal strip had a thickness of 0.03 mm and a width of 4 mm.
[0050] The solder strip obtained in this embodiment was subjected to performance testing using the aforementioned test method, and the results are as follows: DSC curve as shown. Figure 1 As shown, the solidus temperature was measured to be 565℃, the liquidus temperature to be 583℃, and the melting point range was 565~583℃. After the 180° flat plate bending test, the strip surface showed no cracks or fractures, and its toughness was deemed acceptable. The wetting area on the copper plate was 86 mm². 2 The shear strength of the brazed joint is 285 MPa; the strip thickness deviation is ±0.004 mm; the XRD pattern is as follows. Figure 2 As shown, it exhibits typical diffuse scattering peaks and no sharp crystalline peaks, indicating that the strip has an amorphous structure.
[0051] Example 2
[0052] This embodiment provides a copper-based amorphous solder, which, by mass percentage, comprises the following elemental composition: P: 6.2%, Sn: 11.0%, Ni: 6.5%, Si: 0.35%, Ce: 0.045%, Ga: 0.45%, In: 0.15%, with the balance being Cu: 75.205%. The mass ratio of P to Sn is 1:1.77, the mass ratio of Ga to In is 3:1, and the total mass ratio of Ni and Ce to Si is 18.7:1.
[0053] This embodiment prepares the copper-based amorphous solder with the above composition according to the following steps. The steps that are the same as in Example 1 will not be described again, and will only be noted as "same as Example 1": (1) Calculate and weigh each raw material according to the composition of this embodiment. The source, specifications and pretreatment methods of the raw materials are the same as in Example 1; (2) Place the pretreated raw materials in a vacuum induction melting furnace, seal it, and then evacuate it to 8×10⁻⁶. -4 Pa, the graded gradient heating procedure is the same as in Example 1; (3) After the raw materials are completely melted, adjust the pressure inside the furnace to 1.5 × 10⁻⁶. -3 Pa, maintain for 3 minutes. Subsequent operations are the same as in Example 1; (4) The homogenization heat treatment conditions were the same as in Example 1. The parameters for ingot crushing, tube loading, vacuuming, heating to 780℃ and holding for 5 min were the same as in Example 1. During the strip spinning, the copper roller gradient speed was first pre-cooled at 25.5 m / s for 1 s, and then increased to 31 m / s for high-speed cooling. The remaining parameters were the same as in Example 1. The resulting amorphous brazing filler metal strip had a thickness of 0.05 mm and a width of 6 mm.
[0054] The brazing filler metal strip obtained in this embodiment was tested using the same testing method as in Example 1. The results are as follows: DSC measured the solidus temperature to be 568℃, the liquidus temperature to be 585℃, and the melting point range to be 568~585℃; after the 180° flat plate bending test, the strip surface showed no cracks or fractures, and the toughness was qualified; the wetting area was 88mm². 2 Shear strength 292 MPa; thickness deviation ±0.005 mm; XRD pattern shows amorphous diffuse scattering peaks, indicating that the strip has an amorphous structure.
[0055] Example 3
[0056] This embodiment provides a copper-based amorphous solder, which, by mass percentage, comprises the following elemental composition: P: 6.5%, Sn: 11.5%, Ni: 7.0%, Si: 0.4%, Ce: 0.05%, Ga: 0.5%, In: 0.20%, with the balance being Cu: 73.85%. The mass ratio of P to Sn is 1:1.77, the mass ratio of Ga to In is 2.5:1, and the total mass ratio of Ni and Ce to Si is 17.6:1.
[0057] This embodiment prepares the copper-based amorphous solder with the above composition according to the following steps. The parts that are the same as in Example 1 will not be repeated, and will only be noted as "same as Example 1": (1) Calculate and weigh each raw material according to the composition of this embodiment. The source, specifications and pretreatment methods of the raw materials are the same as in Example 1; (2) Evacuate to 6.5×10 -4 Pa, the graded gradient heating procedure is the same as in Example 1; (3) After the raw materials are melted, adjust the temperature to 2.5×10. -3 Pa, maintain for 3 minutes, and then follow the same procedure as in Example 1; (4) Homogenization heat treatment is the same as in Example 1. During the strip spinning process, the copper roller gradient speed is first pre-cooled at 26 m / s for 1 s, and then increased to 32 m / s for high-speed cooling. The other parameters are the same as in Example 1. The resulting amorphous brazing wire strip has a thickness of 0.08 mm and a width of 8 mm.
[0058] The performance of the brazing filler metal strip obtained in this embodiment was tested using the same testing method as in Example 1. The results are as follows: the solidus temperature was 570℃, the liquidus temperature was 588℃, and the melting point range was 570~588℃, as measured by DSC; after the 180° flat plate bending test, there were no cracks or fractures on the surface of the strip, and the toughness was qualified; the wetting area was 87mm²; the shear strength was 288MPa; the thickness deviation was ±0.005mm; the XRD pattern showed amorphous diffuse scattering peaks, indicating that the strip has an amorphous structure.
[0059] Example 4
[0060] This embodiment provides a copper-based amorphous solder, which, by mass percentage, comprises the following elemental composition: P: 5.8%, Sn: 9.8%, Ni: 5.8%, Si: 0.25%, Ce: 0.03%, Ga: 0.3%, In: 0.08%, with the balance being Cu: 77.94%. The mass ratio of P to Sn is 1:1.69, the mass ratio of Ga to In is 3.75:1, and the total mass ratio of Ni and Ce to Si is 23.3:1.
[0061] This embodiment prepares the copper-based amorphous solder with the above composition according to the following steps. The steps that are the same as in Example 1 will not be described again, and will only be noted as "same as Example 1": (1) Calculate and weigh each raw material according to the composition of this embodiment. The source, specifications and pretreatment methods of the raw materials are the same as in Example 1; (2) Place the pretreated raw materials in a vacuum induction melting furnace, seal it, and then evacuate it to 7.5 × 10⁻⁶. -4 Pa, the graded gradient heating procedure is the same as in Example 1; (3) After the raw materials are completely melted, adjust the pressure inside the furnace to 2.0 × 10⁻⁶. -3 Pa, maintain for 3 minutes. Subsequent operations are the same as in Example 1; (4) The homogenization heat treatment conditions were the same as in Example 1. The parameters for ingot crushing, tube loading, vacuuming, heating to 780℃ and holding for 5 min were the same as in Example 1. During strip spinning, the gradient speed of the copper roller was first pre-cooled at 25 m / s for 1 s, and then increased to 30 m / s for high-speed cooling. The remaining parameters were the same as in Example 1. The thickness of the prepared amorphous brazing filler metal strip was 0.04 mm and the width was 5 mm.
[0062] The solder strip obtained in this embodiment was subjected to performance tests using the same testing methods as in Example 1. The results are as follows: DSC measured the solidus temperature to be 566℃, the liquidus temperature to be 584℃, and the melting point range to be 566~584℃; after the 180° flat plate bending test, the strip surface showed no cracks or fractures, and the toughness was qualified; the wetting area was 85mm². 2 Shear strength 283 MPa; thickness deviation ±0.004 mm; XRD pattern shows amorphous diffuse scattering peaks, indicating that the strip has an amorphous structure.
[0063] Example 5
[0064] This embodiment provides a copper-based amorphous solder, which, by mass percentage, comprises the following elemental composition: P: 7.0%, Sn: 12.0%, Ni: 7.5%, Si: 0.45%, Ce: 0.06%, Ga: 0.5%, In: 0.22%, with the balance being Cu: 72.27%. The mass ratio of P to Sn is 1:1.71, the mass ratio of Ga to In is 2.27:1, and the total mass ratio of Ni and Ce to Si is 16.8:1.
[0065] This embodiment prepares the copper-based amorphous solder with the above composition according to the following steps. The steps that are the same as in Example 1 will not be described again, and will only be noted as "same as Example 1": (1) Calculate and weigh each raw material according to the composition of this embodiment. The source, specifications and pretreatment methods of the raw materials are the same as in Example 1; (2) Evacuate to 8×10 -4 Pa, the graded gradient heating procedure is the same as in Example 1; (3) After the raw materials are melted, adjust the temperature to 2.0×10. -3 Pa, maintain for 3 minutes, and then follow the same procedure as in Example 1; (4) Homogenization heat treatment is the same as in Example 1. During the strip spinning process, the copper roller gradient speed is first pre-cooled at 25 m / s for 1 s, and then increased to 30 m / s for high-speed cooling. The other parameters are the same as in Example 1. The resulting amorphous brazing wire strip has a thickness of 0.04 mm and a width of 5 mm.
[0066] The brazing filler metal strip obtained in this embodiment was tested using the same testing method as in Example 1. The results are as follows: DSC measured a solidus temperature of 570℃, a liquidus temperature of 590℃, and a melting point range of 570~590℃; after the 180° flat plate bending test, the strip surface showed no cracks or fractures, and the toughness was qualified; the wetting area was 86mm². 2 Shear strength 286 MPa; thickness deviation ±0.005 mm; XRD pattern shows amorphous diffuse scattering peaks, indicating that the strip has an amorphous structure.
[0067] Example 6
[0068] This embodiment provides a copper-based amorphous solder, which, by mass percentage, comprises the following elemental composition: P: 6.2%, Sn: 10.5%, Ni: 6.5%, Si: 0.35%, Ce: 0.045%, Ga: 0.35%, In: 0.20%, with the balance being Cu: 75.855%. The mass ratio of P to Sn is 1:1.69, the mass ratio of Ga to In is 1.75:1, and the total mass ratio of Ni and Ce to Si is 18.7:1.
[0069] This embodiment prepares the copper-based amorphous solder with the above composition according to the following steps. The steps that are the same as in Example 1 will not be described again, and will only be noted as "same as Example 1": (1) Calculate and weigh each raw material according to the composition of this embodiment. The source, specifications and pretreatment methods of the raw materials are the same as in Example 1; (2) Place the pretreated raw materials in a vacuum induction melting furnace, seal it, and then evacuate it to 7×10⁻⁶. -4 Pa, the graded gradient heating procedure is the same as in Example 1; (3) After the raw materials are completely melted, adjust the pressure inside the furnace to 1.5 × 10⁻⁶. -3 Pa, maintain for 3 minutes. Subsequent operations are the same as in Example 1; (4) The homogenization heat treatment conditions were the same as in Example 1. The parameters for ingot crushing, tube loading, vacuuming, heating to 780℃ and holding for 5 min were the same as in Example 1. During the strip spinning, the copper roller gradient speed was first pre-cooled at 25.5 m / s for 1 s, and then increased to 31 m / s for high-speed cooling. The remaining parameters were the same as in Example 1. The resulting amorphous brazing filler metal strip had a thickness of 0.05 mm and a width of 6 mm.
[0070] The solder strip obtained in this embodiment was subjected to performance tests using the same testing methods as in Example 1. The results are as follows: DSC measured a solidus temperature of 567℃, a liquidus temperature of 586℃, and a melting point range of 567~586℃; after the 180° flat plate bending test, the strip surface showed no cracks or fractures, and the toughness was qualified; the wetting area was 87mm². 2 Shear strength 290 MPa; thickness deviation ±0.005 mm; XRD pattern shows amorphous diffuse scattering peaks, indicating that the strip has an amorphous structure.
[0071] Example 7
[0072] This embodiment provides a copper-based amorphous solder, which, by mass percentage, comprises the following elemental composition: P: 6.3%, Sn: 11.0%, Ni: 6.8%, Si: 0.35%, Ce: 0.045%, Ga: 0.5%, In: 0.10%, with the balance being Cu: 74.905%. The mass ratio of P to Sn is 1:1.75, the mass ratio of Ga to In is 5:1, and the total mass ratio of Ni and Ce to Si is 19.6:1.
[0073] This embodiment prepares the copper-based amorphous solder with the above composition according to the following steps. The steps that are the same as in Example 1 will not be described again, and will only be noted as "same as Example 1": (1) Calculate and weigh each raw material according to the composition of this embodiment. The source, specifications and pretreatment methods of the raw materials are the same as in Example 1; (2) Evacuate to 7.5×10 -4 Pa, the graded gradient heating procedure is the same as in Example 1; (3) After the raw materials are melted, adjust the temperature to 2.0×10. -3 Pa, maintain for 3 minutes, and then follow the same procedure as in Example 1; (4) The homogenization heat treatment was the same as in Example 1. During the strip spinning, the gradient speed of the copper roller was first pre-cooled at 25.5 m / s for 1 s, and then increased to 31 m / s for high-speed cooling. The other parameters were the same as in Example 1. The resulting amorphous brazing wire strip had a thickness of 0.05 mm and a width of 6 mm.
[0074] The brazing filler metal strip obtained in this embodiment was subjected to performance tests using the same testing methods as in Example 1. The results are as follows: DSC measured a solidus temperature of 565℃, a liquidus temperature of 583℃, and a melting point range of 565~583℃; after the 180° flat plate bending test, the strip surface showed no cracks or fractures, and the toughness was qualified; the wetting area was 88mm². 2 Shear strength 291 MPa; thickness deviation ±0.005 mm; XRD pattern shows amorphous diffuse scattering peaks, indicating that the strip has an amorphous structure.
[0075] Example 8
[0076] This embodiment provides a copper-based amorphous solder, which, by mass percentage, comprises the following elemental composition: P: 6.2%, Sn: 11.0%, Ni: 6.5%, Si: 0.35%, Ce: 0.045%, Ga: 0.45%, In: 0.15%, with the balance being Cu: 75.205%. The mass ratio of P to Sn is 1:1.77, the mass ratio of Ga to In is 3:1, and the total mass ratio of Ni and Ce to Si is 18.7:1.
[0077] This embodiment prepares the copper-based amorphous solder with the above composition according to the following steps. The steps that are the same as in Example 1 will not be described again, and will only be noted as "same as Example 1": (1) Calculate and weigh each raw material according to the composition of this embodiment. The source, specifications and pretreatment methods of the raw materials are the same as in Example 1; (2) Place the pretreated raw materials in a vacuum induction melting furnace, seal it, and then evacuate it to 7×10⁻⁶. -4 Pa, the graded gradient heating procedure is the same as in Example 1; (3) After the raw materials are completely melted, adjust the pressure inside the furnace to 2.0 × 10⁻⁶. -3 Pa, maintain for 3 minutes. Subsequent operations are the same as in Example 1; (4) The homogenization heat treatment conditions were the same as in Example 1. The parameters for ingot crushing, tube loading, vacuuming, heating to 780℃ and holding for 5 min were the same as in Example 1. During the strip spinning, the copper roller gradient speed was first pre-cooled at 25.5 m / s for 1 s, and then increased to 31 m / s for high-speed cooling. The remaining parameters were the same as in Example 1. The resulting amorphous brazing filler metal strip had a thickness of 0.05 mm and a width of 6 mm.
[0078] The brazing filler metal strip obtained in this embodiment was tested using the same testing method as in Example 1. The results are as follows: DSC measured a solidus temperature of 566℃, a liquidus temperature of 584℃, and a melting point range of 566~584℃; after the 180° flat plate bending test, the strip surface showed no cracks or fractures, and its toughness was satisfactory. Figure 4 As shown; wetting area 89mm 2 Shear strength 293 MPa; thickness deviation ±0.004 mm; XRD pattern shows amorphous diffuse scattering peaks, indicating that the strip has an amorphous structure.
[0079] Comparative Example 1
[0080] This comparative example provides a copper-based solder, the elemental composition of which differs from that of Example 8 in that In is not added. By mass percentage, the copper-based solder comprises the following elements: P: 6.2%, Sn: 11.0%, Ni: 6.5%, Si: 0.35%, Ce: 0.045%, Ga: 0.45%, with the balance being Cu: 75.355%. The mass ratio of P to Sn is 1:1.77, and the total mass ratio of Ni and Ce to Si is 18.7:1.
[0081] The preparation method of the copper-based solder in this comparative example is the same as that in Example 8.
[0082] The brazing filler metal strip obtained in this embodiment was tested using the same testing method as in Example 1. The results are as follows: DSC measured the solidus temperature to be 580℃, the liquidus temperature to be 605℃, and the melting point range to be 580~605℃; the strip fractured after a 180° flat plate bending test. Figure 4As shown; wetting area 71mm 2 Shear strength 241 MPa; thickness deviation ±0.012 mm; XRD pattern shows localized crystallization.
[0083] Comparative Example 2
[0084] This comparative example provides a copper-based solder, the elemental composition of which differs from that of Example 8 in that Ga is not added. By mass percentage, the copper-based solder comprises the following elements: P: 6.2%, Sn: 11.0%, Ni: 6.5%, Si: 0.35%, Ce: 0.045%, In: 0.15%, with the balance being Cu: 75.505%. The mass ratio of P to Sn is 1:1.77, and the total mass ratio of Ni and Ce to Si is 18.7:1.
[0085] The preparation method of the copper-based solder in this comparative example is the same as that in Example 8.
[0086] The performance of the brazing filler metal strip obtained in this comparative example was tested using the same test method as in Example 1. The results are as follows: DSC measured solidus temperature of 582℃, liquidus temperature of 608℃, and melting point range of 582~608℃; the strip broke after a 180° flat plate bending test; wetted area of 69mm²; shear strength of 237MPa; thickness deviation of ±0.013mm; XRD pattern showed local crystallization.
[0087] Comparative Example 3
[0088] This comparative example provides a copper-based solder, the elemental composition of which differs from that of Example 8 in that Ce is not added. By mass percentage, the copper-based solder comprises the following elements: P: 6.2%, Sn: 11.0%, Ni: 6.5%, Si: 0.35%, Ga: 0.45%, In: 0.15%, with the balance being Cu: 75.25%. The mass ratio of P to Sn is 1:1.77, and the mass ratio of Ga to In is 3:1.
[0089] The preparation method of the copper-based solder in this comparative example is the same as that in Example 8.
[0090] The brazing filler metal strip obtained in this comparative example was tested using the same testing method as in Example 1. The results are as follows: DSC measured the solidus temperature to be 578℃, the liquidus temperature to be 602℃, and the melting point range to be 578~602℃; after the 180° flat plate bending test, microcracks appeared on the surface of the strip, which were determined to be microcracks. Figure 4 As shown; wetting area 73 mm²; shear strength 246 MPa; thickness deviation ±0.011 mm; XRD pattern shows localized crystallization.
[0091] Comparative Example 4
[0092] This comparative example provides a copper-based solder with the same elemental composition as Example 8 (P: 6.2%, Sn: 11.0%, Ni: 6.5%, Si: 0.35%, Ce: 0.045%, Ga: 0.45%, In: 0.15%, with the balance being Cu: 75.205%). The difference lies in the melting stage of the preparation method, where a single-stage heating melting is used instead of a graded gradient heating. The specific process is as follows: the raw material is placed in a vacuum induction melting furnace, and a vacuum of 7 × 10⁻⁶ is applied. -4 After Pa, the temperature is directly increased from room temperature to 1150℃ at a rate of 5℃ / min and held for 15min; after the raw material is completely melted, the furnace pressure is adjusted to 2.0×10 -3 Pa, hold for 3 minutes, and the subsequent argon filling, stirring, casting, homogenization heat treatment and strip spinning steps are the same as in Example 8.
[0093] The brazing filler metal strip obtained in this comparative example was tested using the same testing method as in Example 1. The results are as follows: DSC measured the solidus temperature to be 575℃, the liquidus temperature to be 598℃, and the melting point range to be 575~598℃; after the 180° flat plate bending test, there were no cracks or fractures on the surface of the strip, and the toughness was qualified; the wetting area was 78mm²; the shear strength was 262MPa; the thickness deviation was ±0.010mm; and the XRD pattern showed local crystallization.
[0094] Comparative Example 5
[0095] This comparative example provides a copper-based solder with the same elemental composition as Example 8 (P: 6.2%, Sn: 11.0%, Ni: 6.5%, Si: 0.35%, Ce: 0.045%, Ga: 0.45%, In: 0.15%, with the balance being Cu: 75.205%). The difference lies in the preparation method, where no pressure adjustment is performed. The specific process is as follows: graded gradient heating melting is used (same as Example 8). After the raw material is completely melted, the pressure is not adjusted and is set at 7 × 10⁻⁶. -4 Pa, directly fill with high-purity argon gas to atmospheric pressure, stir for 2 minutes and then cast; the remaining steps (homogenization heat treatment, gradient speed belt spinning) are the same as in Example 8.
[0096] The brazing filler metal strip obtained in this comparative example was tested using the same testing method as in Example 1. The results are as follows: DSC measured the solidus temperature to be 574℃, the liquidus temperature to be 596℃, and the melting point range to be 574~596℃; after the 180° flat plate bending test, there were no cracks or fractures on the surface of the strip, and the toughness was qualified; the wetting area was 76mm²; the shear strength was 258MPa; the thickness deviation was ±0.009mm; and the XRD pattern showed local crystallization.
[0097] Comparative Example 6
[0098] This comparative example provides a copper-based brazing filler metal with the same elemental composition as Example 8 (P: 6.2%, Sn: 11.0%, Ni: 6.5%, Si: 0.35%, Ce: 0.045%, Ga: 0.45%, In: 0.15%, with the balance being Cu: 75.205%). The difference lies in the use of a constant rotation speed instead of a gradient rotation speed during the spinning stage. Specifically, the copper roller runs at a constant speed of 30 m / s without a pre-cooling stage. The remaining spinning parameters (nozzle distance 1.2 mm, argon pressure 0.3 MPa, compressed air 0.2 MPa, quartz tube heated to 780°C and held for 5 min) and the melting and heat treatment steps are the same as in Example 8.
[0099] The performance of the brazing filler metal strip obtained in this comparative example was tested using the same test method as in Example 1. The results are as follows: DSC measured solidus temperature of 580℃, liquidus temperature of 610℃, and melting point range of 580~610℃; the strip broke after a 180° flat plate bending test; wetted area of 68mm²; shear strength of 235MPa; thickness deviation of ±0.014mm; XRD pattern showed local crystallization.
[0100] Comparative Example 7
[0101] This comparative example provides a copper-based solder whose elemental composition differs from that of Example 1 in that the mass ratio of P to Sn is not within the 1:1.6~1.9 range specified in this invention. By mass percentage, the copper-based solder comprises the following elements: P: 6.5%, Sn: 9.0%, Ni: 6.0%, Si: 0.3%, Ce: 0.04%, Ga: 0.4%, In: 0.10%, with the balance being Cu: 77.66%. The mass ratio of P to Sn is 1:1.38, the mass ratio of Ga to In is 4:1, and the total mass ratio of Ni and Ce to Si is 20.13:1.
[0102] The preparation method of the copper-based solder in this comparative example is the same as that in Example 1.
[0103] The brazing filler metal strip obtained in this comparative example was tested using the same test method as in Example 1. The results are as follows: DSC measured solidus temperature of 560℃, liquidus temperature of 595℃, and melting point range of 560~595℃; the strip fractured after a 180° flat plate bending test; the wetting area was 62mm². 2 Shear strength 218 MPa; thickness deviation ±0.014 mm; XRD pattern as shown. Figure 2 As shown, it exhibits localized crystallization.
[0104] Comparative Example 8
[0105] This comparative example provides a copper-based solder whose elemental composition differs from that of Example 1 in that the mass ratio of Ga to In is not within the range of (1.2-6.25):1 limited by this invention. By mass percentage, the copper-based solder comprises the following elements: P: 6.0%, Sn: 10.0%, Ni: 6.0%, Si: 0.3%, Ce: 0.04%, Ga: 0.2%, In: 0.20%, with the balance being Cu: 77.46%. The mass ratio of P to Sn is 1:1.67, the mass ratio of Ga to In is 1:1, and the total mass ratio of Ni and Ce to Si is 20.13:1.
[0106] The preparation method of the copper-based solder in this comparative example is the same as that in Example 1.
[0107] The performance of the brazing filler metal strip obtained in this comparative example was tested using the same test method as in Example 1. The results are as follows: DSC measured solidus temperature of 558℃, liquidus temperature of 592℃, and melting point range of 558~592℃; the strip fractured after a 180° flat plate bending test; wetting area of 65mm²; shear strength of 225MPa; thickness deviation of ±0.013mm; XRD pattern as shown. Figure 3 As shown, it exhibits localized crystallization.
[0108] Comparative Example 9
[0109] This comparative example is prepared and formulated according to the optimal embodiment (Example 3) of the prior art CN108381058A. By mass percentage, the copper-based brazing filler metal includes the following elemental composition: P: 6.5%, Sn: 6.5%, Ni: 2.5%, Si: 0.3%, with the balance being Cu: 84.2%. The preparation process adopts traditional vacuum induction melting and constant speed strip spinning: the raw material is placed in a vacuum induction melting furnace, heated to 1100℃ in one go, held at that temperature for 15 minutes, and then cast; after the ingot is broken, it is loaded into a quartz tube, heated and melted, and then sprayed onto a copper roller rotating at a constant speed of 30m / s for rapid cooling.
[0110] The performance of the brazing filler metal strip obtained in this comparative example was tested using the same test method as in Example 1. The results are as follows: DSC measured solidus temperature of 620℃, liquidus temperature of 645℃, and melting point range of 620~645℃; the strip broke after a 180° flat plate bending test; wetted area of 58mm²; shear strength of 195MPa; thickness deviation of ±0.018mm; XRD pattern showed local crystallization.
[0111] The performance test results of Examples 1-8 and Comparative Examples 1-9 are summarized in Table 1: Table 1 Summary of performance test results for Examples 1-8 and Comparative Examples 1-9
[0112] The performance test results of Examples 1-8 show that the copper-based amorphous brazing filler metal provided by this invention has a solidus temperature between 565 and 570°C and a liquidus temperature between 583 and 590°C, achieving a low-temperature brazing process window below 600°C. Simultaneously, the obtained strips all passed the 180° flat plate bending test, exhibiting good toughness; the wetting area on the copper plate was ≥85 mm², the shear strength of the brazed joint was ≥283 MPa, the strip thickness deviation was controlled within ±0.005 mm, and the XRD patterns all showed typical amorphous diffuse scattering peaks. This proves that the multi-component system of this invention, through precise coordination, successfully achieves low melting point, high toughness, strong wetting, and excellent amorphous forming ability, meeting the low-temperature brazing requirements of micron or nano-scale ultrathin copper and copper alloy tubing.
[0113] Comparing Example 8 with Comparative Example 1 (without In) and Comparative Example 2 (without Ga), it can be seen that when Ga or In is missing alone, the solid-liquid phase temperature of the alloy increases significantly (e.g., the solidus temperature of Comparative Example 1 is as high as 580℃, and that of Comparative Example 2 is 582℃), which is much higher than the 566℃ of Example 8. At the same time, all of them fractured in the bending test, the wetting area and shear strength decreased significantly, and XRD showed that the strip had local crystallization. This confirms the necessity of using Ga and In in combination. Although Ga can significantly reduce the melting point, it is easy to cause embrittlement when used alone. The introduction of In not only helps to reduce the melting point, but more importantly, through its good atomic size matching with Ga, it synergistically improves the problem of toughness reduction caused by Ga introduction and jointly promotes the stability of the amorphous structure. In Examples 1 to 8, the mass ratio of Ga to In within the range of 2: (1 to 3) defined in this invention has achieved excellent comprehensive performance. However, in Comparative Example 8, when the Ga content relative to In content is too low, the synergistic balance is broken, resulting in a downward trend in amorphous formation ability or processing performance.
[0114] Comparing Example 8 with Comparative Example 3 (without Ce), it can be seen that without Ce, the solidus temperature of the alloy increased from 566°C to 578°C, microcracks appeared in the bending test, and the wetting area and shear strength decreased to 73 mm². 2 The pressure reached 246 MPa, and local crystallization occurred. This verifies that Ce plays an irreplaceable role in the high Ni content (6.5%) system: it purifies the alloy interface, reduces oxide inclusions, and synergistically inhibits the continuous network precipitation of the Ni3P brittle phase with Ni.
[0115] Comparative Example 9, using existing technology, controlled the Ni content at 2.5%. Although the resulting solder had a different composition, its solidus temperature reached 620℃, indicating that conventional low-Ni routes struggle to maintain a low melting point. This invention breaks through the conventional understanding that "Ni should not exceed 3%." It increases the Ni content to 5.8%~8.0% to strengthen the matrix and improve wettability and joint strength. Addressing the potential problem that high Ni content might exacerbate the precipitation of brittle phases like Ni3P and impair amorphous formation ability, this invention simultaneously introduces Ce and Si to form a synergistic system: Ce can purify the alloy interface, reduce oxide inclusions, and synergistically suppress the continuous network precipitation of Ni3P with Ni; Si, as an amorphous modifier, can refine the microstructure, and the composite modification system formed by Ce and Si also helps suppress the precipitation of crystalline phases during rapid cooling. By controlling the total mass ratio of Ni and Ce to Si within the range of (15~20):(1~2), the synergistic effect of the three is fully realized, thus maintaining excellent amorphous formation ability and strip toughness even at higher Ni contents.
[0116] Comparative Example 7, with a P to Sn mass ratio of 1:1.38, which is lower than the 1:(1.6~1.9) range of this invention, resulted in strip fracture and a sharp deterioration in performance. This indicates that when the Sn content is relatively insufficient compared to P, it is impossible to effectively suppress the continuous precipitation of the Cu3P brittle phase generated due to the high P content, which seriously impairs the toughness of the solder, proving the necessity of controlling the P to Sn ratio within a specific range.
[0117] Compared with Comparative Example 4, Comparative Example 4, due to a one-time direct heating to the maximum temperature, resulted in a large amount of volatilization of the low-melting-point components Ga and In, causing the actual composition to deviate from the designed ratio. The alloy liquidus temperature rose from 584°C to 598°C, and localized crystallization occurred in the strip. Simultaneously, oxide inclusions inside the melt were difficult to remove effectively, and obvious dendritic segregation and inclusions were visible in the metallographic structure. Figure 5 As shown, the aforementioned structural defects directly degraded the brazing performance: the shear strength of Comparative Example 4 decreased to 262 MPa compared to 293 MPa in Example 8, and the wetting area also declined significantly. This comparison fully demonstrates that the graded gradient heating process of the present invention reduces the volatilization loss of low-melting-point components through staged temperature control and achieves deep melt purification in conjunction with pressure adjustment, ensuring the complete realization of the multi-component system design. This is the key process guarantee for the stable performance advantage of the component system of the present invention.
[0118] Comparing Example 8 with Comparative Example 5 (without pressure adjustment in the preparation method), when the pressure adjustment process was not performed, the alloy liquidus temperature rose from 584°C to 596°C, and local crystallization also occurred, resulting in a decrease in wetting and mechanical properties. This is because although the high vacuum in the early stage eliminated free oxygen in the furnace, oxide inclusions still remained inside the melt. The airflow stirring and bubble flotation mechanism introduced after pressure adjustment can deeply remove oxide inclusions such as Cu2O and SnO2, improving the purity of the melt. The performance degradation of Comparative Example 5 directly proves the key role of this step in reducing heterogeneous nucleation sites, improving amorphous formation ability, and ensuring wetting and strength.
[0119] Comparing Example 8 with Comparative Example 6 (constant rotation speed spinning in the preparation method), the strip performance deteriorated sharply after adopting a constant rotation speed, with the liquidus temperature rising to 610°C and directly breaking and failing. This indicates that, compared to the traditional constant rotation speed, the gradient rotation speed spinning process of the present invention (pre-cooling at a lower speed first, then increasing to high speed for cooling) is more conducive to improving the thickness uniformity and dimensional accuracy of amorphous strips by dynamically adjusting the cooling rate, and is an important guarantee for achieving high-quality, high-precision amorphous solder strip preparation.
[0120] Application examples
[0121] The copper-based amorphous brazing filler metal prepared in Example 1 was used for brazing ultrathin T2 copper tubes (outer diameter Φ6mm, wall thickness 0.2mm). The brazing steps are as follows: (1) Joint preparation: Before brazing, the ends of the two copper pipes are processed into 45° V-shaped bevels, the assembly gap is controlled at 0.05mm, and the area to be welded is polished with 2000 grit sandpaper. Then, it is ultrasonically cleaned in acetone for 15 minutes and dried in hot air at 80℃. (2) Placing of brazing filler metal: Cut the copper-based amorphous brazing filler metal strip (thickness 0.03 mm, width 4 mm) prepared in Example 1 into 15 mm long segments, wrap around and press tightly onto the joint bevel to ensure that the strip is fully attached to the surface of the base material; (3) Loading into the furnace: Place the assembled joint into the vacuum brazing furnace, and place process gaskets of the same material around the joint to prevent high-temperature deformation. After closing the furnace door, evacuate the furnace until the pressure inside the furnace is ≤5×10. -3 Pa; (4) Heating and brazing: Increase the temperature to 580℃ at 10℃ / min (this temperature is about 15℃ higher than the solidus of the brazing filler metal in Example 1, which is 565℃), and hold for 10 min; during the holding period, maintain the vacuum degree at ≤5×10 -3 Pa; The brazing temperature must be strictly controlled to not exceed 600℃ to avoid the performance degradation of the ultra-thin copper tube wall due to grain coarsening (the grain growth rate of T2 copper increases sharply above 600℃). At the same time, the holding time should not exceed 15 min to prevent the brazing filler metal from spreading too much and causing insufficient filling of the joint gap. (5) Cooling: After brazing, cool the furnace to below 200°C, then fill with high-purity nitrogen to break the vacuum, remove the joint, and finally wipe the surface residue of the joint with anhydrous ethanol.
[0122] The brazing results show that the joint shear strength reaches 285MPa, the brazing seam is fully and continuously filled, and there are no defects such as pores or cracks. Furthermore, no visible deformation occurs in the copper tube base material, indicating that the brazing filler metal has excellent low-temperature brazing adaptability to ultra-thin copper tubes.
[0123] It should be noted that the above description is a further detailed explanation of the present invention in conjunction with specific embodiments, and should not be construed as limiting the specific implementation of the present invention to these descriptions; the dimensional data in this embodiment do not necessarily limit the technical solution, but merely illustrate one specific working condition. For those skilled in the art, various simple improvements and modifications can be made without departing from the concept of the present invention, and all such improvements and modifications should be considered to fall within the scope of protection of the present invention.
Claims
1. A copper-based amorphous solder, characterized in that, The copper-based amorphous solder comprises the following elemental components by weight percentage: P: 5.8%~7.2%, Sn: 9.5%~12.0%, Ni: 5.8%~8.0%, Si: 0.2%~0.5%, Ce: 0.03%~0.06%, Ga: 0.3%~0.5%, In: 0.08%~0.25%, with the balance being Cu and mass percentage ≥71%; Wherein, the mass ratio of P to Sn is 1:(1.6~1.9), the mass ratio of Ga to In is (1.2~6.25):1, and the total mass ratio of Ni and Ce to Si is (15~25):(1~2).
2. The copper-based amorphous solder according to claim 1, characterized in that, The copper-based amorphous solder comprises the following elemental components by mass percentage: P: 6.0%~6.5%, Sn: 10.0%~11.5%, Ni: 6.0%~7.0%, Si: 0.3%~0.4%, Ce: 0.04%~0.05%, Ga: 0.4%~0.5%, In: 0.10%~0.20%, Cu: 73%~78%; Wherein, the mass ratio of P to Sn is 1:(1.6~1.8), the mass ratio of Ga to In is (2~5):1, and the total mass ratio of Ni and Ce to Si is (16~25):
1.
3. A method for preparing a copper-based amorphous solder as described in any one of claims 1-2, characterized in that, Includes the following steps: (1) Based on the mass percentage of each element in the copper-based amorphous brazing filler metal, calculate and weigh the corresponding raw materials according to the actual element content of each element and / or intermediate alloy raw material, and then perform pretreatment. (2) Place each of the raw materials in a smelting furnace and heat it at 6.0 × 10⁻⁶ ℃. -4 ~9.0×10 -4 Staged gradient heating melting under high vacuum conditions; (3) After all raw materials have melted, adjust the pressure inside the furnace to 1.0 × 10⁻⁶. -3 ~3.0×10 -3 Pa, then fill with high-purity argon gas to atmospheric pressure, and then cast into a water-cooled copper mold to obtain an alloy ingot; (4) The alloy ingot is heat-treated and crushed, then placed into a quartz tube with a nozzle, vacuumed and heated to melt, then argon gas is injected into the quartz tube and sprayed onto a copper roller rotating at a gradient speed for rapid cooling, and then separated by compressed air to obtain copper-based amorphous brazing filler metal.
4. The preparation method according to claim 3, characterized in that, The graded gradient heating described in step (2) includes three stages: First stage: Heat to 400-450℃ at a rate of 8-10℃ / min, and hold for 5-10 minutes; Second stage: Increase the temperature to 800-850℃ at a rate of 8-10℃ / min, and hold for 8-15 minutes; Third stage: Increase the temperature to 1100~1200℃ at a rate of 3~5℃ / min, and hold for 15~20min.
5. The preparation method according to claim 3, characterized in that, The heat treatment in step (4) involves placing the alloy ingot in a vacuum muffle furnace and sequentially heating, holding, and air cooling. The heating rate is 3~5℃ / min, and the temperature is raised to 560~590℃; the holding time is 4~6h.
6. The preparation method according to claim 3, characterized in that, The vacuum level after evacuation in step (4) is less than 5 × 10⁻⁶. -3 Pa; And / or, the heating and melting temperature in step (4) is 780~820℃ and the time is 5~10min.
7. The preparation method according to claim 3, characterized in that, The gradient rotation speed of the copper roller in step (4) includes two levels: First stage: Control the rotation speed at 25~26m / s and continue for 1~5 seconds for pre-cooling; Second stage: Increase the rotation speed to 30~32m / s for high-speed cooling.
8. The preparation method according to claim 3, characterized in that, The rapid cooling rate described in step (4) is 6 × 10⁻⁶. 6 K / s ~3×10 7 K / s.
9. The preparation method according to claim 3, characterized in that, In step (4), the distance between the nozzle and the copper roller is 1.2~1.4mm; And / or, the pressure of the argon gas introduced in step (4) is 0.3~0.5MPa.
10. The application of a copper-based amorphous brazing filler metal as described in any one of claims 1-2 in the brazing of ultra-thin copper and copper alloy pipe fittings, characterized in that, The brazing temperature is 570~610℃.
Citation Information
Patent Citations
Boracic Cu-P-based amorphous brazing filler metal and method for preparing same
CN101530952A
Ga-containing low-sliver copper based high-performance brazing filler metal and preparation method thereof
CN108381058A
Preparation method of tungsten-copper composite contact
CN117038368A