Slow-effect/release-controllable silica-potassic-magnesium fertilizer
A technology of silicon-potassium and magnesium fertilizers, applied in magnesium fertilizers, potash fertilizers, inorganic fertilizers, etc., can solve the problems of adverse side effects, small market share, low potassium content, etc. Effect
Patent Information
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Publication Date
- 2007-06-20
- Estimated Expiration
- Not applicable · inactive patent
Abstract
Description
technical field
[0001] The invention belongs to the field of mineral potassium fertilizer production, and in particular relates to a slow-acting / controlled-release citrate-soluble (water-insoluble) silicon-potassium-magnesium fertilizer. Background technique
[0002] In the past, the order of using soil fertilizers in my country was nitrogen, phosphorus, and potassium. By the late 1990s, potassium deficiency in agricultural production had become a serious problem. The relevant state departments began to implement the "potassium supplement project". Pay attention to. The main raw material for the traditional production of potash fertilizers is the water-soluble potassium salt resources that are lacking in my country. Therefore, the potash fertilizers needed in China in the early stage mainly relied on imports, mainly potassium chloride and potassium sulfate, which belong to chemical fertilizers. These potash fertilizers are water-soluble quick-acting fertilizers. Characterized...
Examples
Embodiment 1
[0012] The calorific value of coal used as fuel is 6600 kcal. Potassium feldspar contains 12.5% potassium oxide. The raw material ratio is 66% potassium feldspar, 20% limestone, 6% potassium chloride, and 8% magnesium oxide. Kiln, calcined for 40 minutes, calcined at 1200°C, cooled and ball-milled into 120-mesh powder, and then granulated to obtain the finished product. The effective potassium oxide content in the finished product is 8.66%, the effective silicon oxide content is 32.6%, and the effective magnesium content is 8.2%.
Embodiment 2
[0014] The calorific value of coal used as fuel is 6600 kcal. Potassium feldspar contains 12.5% potassium oxide. Raw material ratio is 54% potassium feldspar, 18% limestone, 18% potassium chloride, and 10% magnesium oxide. Kiln, calcined for 40 minutes, calcined at 1150°C, cooled and ball-milled into 120-mesh powder, and then granulated to obtain the finished product.
Embodiment 3
[0016] The calorific value of coal used as fuel is 6600 kcal. Potassium feldspar contains 12.5% potassium oxide. The raw material ratio is 69% potassium feldspar, 15% limestone, 7% potassium chloride, and 9% magnesium oxide. Kiln, calcination for 40 minutes, calcination temperature 1300 ℃, cooling ball mill into 120 mesh powder, and then granulation is the finished product.