Zirconium oxide ceramic bead forming die
Through the multi-layer mold plate structure and overflow hole docking hole design, the problems of easy damage of high-pressure equipment and poor sphericity in the production of large-size zirconia ceramic beads are solved, and high-quality, low-cost zirconia ceramic bead molding is achieved. Improved product sphericity and production efficiency.
Patent Information
- Application Number
- CN202323259567.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-01
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2033-12-01
AI Technical Summary
The existing production method of large-sized zirconia ceramic beads has problems such as high-pressure equipment being easily damaged, mold demoulding being difficult, uneven powder addition leading to poor sphericity, low efficiency, and high maintenance costs.
It adopts a multi-layer mold plate set structure, forming a temporary flow channel through the overflow hole and butt hole to facilitate material overflow and collection, ensuring that the material is completely formed in the ball cavity, and ensuring the stable stacking and stabilization of the mold plate set through limiting fixed angles and handles. separation to reduce production pressure.
It achieves high-quality molding of large-size zirconia ceramic beads, reduces production costs and equipment maintenance requirements, improves the sphericity and qualification rate of the product, and achieves flexible production.
Smart Images

Figure CN221834576U_ABST
Abstract
Description
Technical Field
[0001] The utility model belongs to the technical field of zirconium oxide preparation, in particular to a zirconium oxide ceramic bead forming mold and a method for preparing the zirconium oxide ceramic bead by using the mold. Background Art
[0002] As an excellent grinding medium, zirconia ceramic beads have the advantages of high melting point, high hardness, low wear rate, high grinding efficiency, etc., and have been widely used in industries such as coatings, inks, and lithium battery materials. With the development of the grinding industry, zirconia ceramic beads are gradually developing towards miniaturization, but large-sized zirconia ceramic beads are still widely used in certain industries. For example, large rolling ball mills are required in the grinding process of gold mines, which inevitably require large-sized zirconia ceramic beads, such as 20mm, 40mm, etc.
[0003] At present, the production method of large-sized zirconia ceramic beads generally adopts isostatic pressing. This method requires adding powder into the mold cavity and obtaining the zirconia ceramic bead green body after being pressed by the machine. However, this method has some problems. First, the press requires very high pressure, the hydraulic device is easily damaged, and the maintenance is frequent. Secondly, it is difficult to demold the mold and requires a lot of manpower. In addition, if too much powder is added during the pressing process, a very thick cap will be formed, which is difficult to remove by the later green body polishing and the final sintered ball polishing; if the amount of powder added is too little, the sphericity of the pressed zirconia ceramic bead green body will be very poor, and even if an automated powder adding device is added, stable production cannot be achieved due to changes in powder fluidity, looseness, softness and hardness. Therefore, most of the production is still manually operated, which is inefficient and cannot guarantee that the appropriate amount of powder is added each time to obtain zirconia ceramic beads with good sphericity. The mold after demolding is difficult to clean due to the hard adhesion of powder caused by high pressure. Utility Model Content
[0004] In order to overcome the shortcomings of the prior art, the utility model provides a zirconia ceramic bead forming mold which is convenient for demoulding a green body of a product and ensures the production quality of the product.
[0005] In order to achieve the above object, the present invention adopts the following technical scheme: a zirconia ceramic bead forming mold, comprising a plurality of mold plate groups, wherein the mold plate group is composed of an upper cover plate, a middle cavity plate and a lower cavity plate;
[0006] A plurality of lower cavities are arranged on the lower cavity plate;
[0007] A plurality of upper cavities are arranged on the middle cavity plate, an overflow hole is opened on the top of the upper cavity, and a docking hole is provided between the overflow hole and the inner cavity of the upper cavity;
[0008] A plurality of cover bodies are arranged on the upper cover plate, a pressing platform is provided at the bottom of the cover body, a docking platform is provided at the bottom thereof, and a spherical concave cavity is provided on the bottom surface of the docking platform;
[0009] The lower cavity plate, the middle cavity plate and the upper cover plate are stacked from bottom to top and covered accordingly, each upper cavity is docked on the corresponding lower cavity, the extrusion platform is engaged with the overflow hole, the docking platform is plugged into the docking hole, and the lower cavity, the upper cavity and the spherical concave cavity surround to form a spherical cavity for forming products;
[0010] During the process of the extrusion platform being inserted into the overflow hole and the docking platform not yet being fully docked with the docking hole, a temporary flow channel is formed between the outer wall of the extrusion platform and the wall of the overflow hole, and part of the excess material can overflow along the temporary flow channel. When the docking platform begins to be plugged into and mated with the docking hole and is fully mated, the material that cannot be discharged along the temporary flow channel will be collected in the spherical concave cavity until the temporary flow channel is closed and the docking platform and the docking hole are fully mated, and the material that cannot be discharged along the temporary flow channel will all enter the spherical concave cavity.
[0011] Preferably, the top aperture of the overflow hole is larger than the bottom aperture, and the extrusion platform is a frustum structure with a larger top and a smaller bottom that corresponds to the overflow hole.
[0012] Preferably, the bottom edge of the overflow hole and the top edge of the docking hole are connected and arranged, and the bottom edge of the extrusion platform and the top edge of the docking platform are connected and arranged.
[0013] Preferably, the bottom surface of the middle cavity plate is provided with a plurality of grooves, and the top surface of the lower cavity plate is provided with a plurality of bosses, and when the middle cavity plate and the lower cavity plate are covered, the bosses and the grooves are plug-fitted correspondingly.
[0014] Preferably, the grooves are annular grooves respectively surrounding the circumference of the corresponding upper cavities, and the bosses are annular bosses respectively surrounding the circumference of the corresponding lower cavities.
[0015] Preferably, the lower cavity plate, the middle cavity plate and the upper cover plate are respectively provided with handles.
[0016] Preferably, a first arc chamfer is provided on the bottom outer edge of the handle of the lower cavity plate, and a second arc chamfer is provided on the top outer edge of the handle of the middle cavity plate, and when the middle cavity plate is covered on the lower cavity plate, the first arc chamfer and the second arc chamfer directly constitute an arc bevel.
[0017] Preferably, a limiting fixing angle is provided on the top surface of the upper cover plate, and a fixing foot is provided on the bottom surface of the lower cavity plate. When multiple layers of mold plate groups are stacked, the fixing feet of the lower cavity plate of the upper layer can be engaged with the limiting fixing angle of the upper cover plate of the next layer to limit the slippage of the adjacent layers of mold plate groups.
[0018] Preferably, when multiple layers of mold plate groups are stacked, the outer bottom surface of the lower cavity of an upper layer abuts against the top surface of the upper cover plate of a lower layer.
[0019] Preferably, a method for preparing zirconia ceramic beads using any one of the molds described above,
[0020] Step S1, assembling the middle cavity plate and the lower cavity plate of a layer of mold plate group to form a main cavity assembly;
[0021] Step S2, pouring the gel zirconia ceramic slurry into each cavity of the main cavity assembly from the overflow hole, until the liquid level of the gel zirconia ceramic slurry is higher than the docking hole;
[0022] Step S3, closing the upper cover body onto the middle cavity plate, and draining the excess gel zirconia ceramic slurry;
[0023] Step S4, placing a lower cavity plate on the upper cover plate of the current layer;
[0024] Step S5, repeating steps S1 to S4 to stack several layers of mold plate groups in sequence;
[0025] Step S6, placing a pressing plate on the upper cover plate at the top layer, applying a certain pressure to the mold plate group so that each layer of the mold plate group will not loosen;
[0026] Step S7, standing for a period of time to allow the gel zirconium oxide ceramic slurry in each layer of the spherical cavity to solidify into a gel sphere;
[0027] Step S8, opening the upper cover plate of each layer of the mold plate group in turn, and placing the main cavity assembly of the middle cavity plate and the lower cavity plate of each layer into an oven for drying;
[0028] Step S9, after the gel sphere is completely dried, the middle cavity and the lower cavity are separated, and the formed green sphere is taken out for subsequent processing;
[0029] Step S10, cleaning the mold plate set with pure water and drying it for reuse.
[0030] The technical effect of the utility model is as follows: through the structural setting of the present invention, the gel slurry is poured into the mold plate group for solidification to form large-sized zirconia ceramic beads, without the need for large-cost equipment investment, and only a normal pressure-resistant mold is needed as a production device, which can effectively reduce the production cost; and the zirconia ceramic beads prepared by this mold have few surface defects, high sphericity, high product qualification rate, and flexible production can be achieved in output, without excessive equipment maintenance costs, and while facilitating production, product quality is guaranteed. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 It is a structural schematic diagram of the utility model.
[0032] Figure 2 It is a schematic diagram of the structure of a single mold plate group.
[0033] Figure 3 Schematic diagram of an exploded view of a single mold plate group.
[0034] Figure 4 A schematic side view of the upper cover.
[0035] Figure 5 for Figure 4 Local schematic diagram of point H in the middle.
[0036] Figure 6 It is a structural schematic diagram of the upper cover.
[0037] Figure 7 It is a bottom view schematic diagram of the upper cover.
[0038] Figure 8 for Figure 7 Partial schematic diagram of point F in the middle.
[0039] Fig. 9 Schematic diagram of the top view of the middle cavity plate.
[0040] Fig.10 for Fig. 9 Local schematic diagram at point M in the middle.
[0041] Fig.11 It is a bottom view schematic diagram of the middle cavity plate.
[0042] Fig.12 for Fig.11 Local schematic diagram at point N in the figure.
[0043] Fig.13 Schematic diagram of the side view of the middle cavity plate.
[0044] Fig.14 It is a schematic diagram of the structure of a single mold plate group.
[0045] Fig.15 Schematic diagram of the structure of the middle cavity plate.
[0046] Fig.16 Schematic diagram of the side view of the lower cavity plate.
[0047] Fig.17 for Fig.16 Local schematic diagram at P in the middle.
[0048] Fig.18 Schematic diagram of the top view of the lower cavity plate.
[0049] Fig.19 for Fig.18 Partial schematic diagram at Q in the middle.
[0050] Fig. 20 A schematic side view of a single mold plate assembly.
[0051] Fig.21 for Fig. 20 Schematic cross-sectional view of area C in the middle.
[0052] Fig. 22 for Fig.21 Partial schematic diagram at point E in the middle.
[0053] The main technical features in the figure are marked as follows: 1. upper cover plate; 2. middle cavity plate; 3. lower cavity plate; 1-1. spherical concave cavity; 1-2. limit fixing angle; 1-3. handle; 1-5. cover body; 1-6. extrusion table; 1-7. docking table; 2-1. docking hole; 2-2. square ring groove; 2-3. overflow hole; 2-6. upper cavity; 3-1. fixed foot; 3-4. square ring table; 3-5. lower cavity. Implementation
[0054] The present invention will be further described below through specific implementation modes and accompanying drawings.
[0055] like Figures 1 to 22 As shown, a zirconia ceramic bead forming mold includes multiple layers of mold plate groups stacked in sequence, and each layer of the mold plate group is composed of an upper cover plate 1, a middle cavity plate 2 and a lower cavity plate 3.
[0056] Specifically, a plurality of rows of lower cavities 3-5 are evenly arranged in a square shape along the length of the lower cavity plate 3, and the lower cavity 3-5 is a hemispherical body, and its bottom protrudes from the bottom surface of the lower cavity plate 3;
[0057] Specifically, a plurality of rows of upper cavities 2-6 are evenly arranged in a square along the length of the middle cavity plate 2. The upper cavity 2-6 is a hemispherical body with an overflow hole 2-3 on the top. A docking hole 2-1 is provided between the overflow hole 2-3 and the inner cavity of the upper cavity 2-6. The overflow hole 2-3 is an inverted truncated cone-shaped conical hole. The docking hole 2-1 is a circular hole with the same aperture as the bottom aperture of the overflow hole 2-3, and its upper and lower ends are respectively adjacently joined to the hole wall of the overflow hole 2-3 and the cavity wall of the upper cavity 2-6.
[0058] Specifically, a plurality of cover bodies 1-5 are arranged on the upper cover plate 1. The cover body 1-5 is hemispherical, and an extrusion platform 1-6 is fixedly connected to its bottom. The extrusion platform 1-6 is an inverted frustum structure, and a docking platform 1-7 is fixedly connected to its bottom. The docking platform 1-7 is a frustum with the same diameter as the bottom of the extrusion platform 1-6, and a spherical concave cavity 1-1 is opened on its bottom surface.
[0059] Specifically, the lower cavity plate 3, the middle cavity plate 2 and the upper cover plate 1 are stacked from bottom to top and covered accordingly, each upper cavity 2-6 is docked on the corresponding lower cavity 3-5, the extrusion platform 1-6 is engaged with the overflow hole 2-3, the docking platform 1-7 is engaged and inserted into the docking hole 2-1, and the lower cavity 3-5, the upper cavity 2-6 and the spherical concave cavity 1-1 surround and form a spherical cavity for molding products.
[0060] Specifically, when the extrusion platform 1-6 is inserted into the overflow hole 2-3 and the docking platform 1-7 has not yet been fully docked with the docking hole 2-1, a temporary flow channel is formed between the outer wall of the extrusion platform 1-6 and the wall of the overflow hole 2-3, and some excess material can overflow along the temporary flow channel. When the docking platform 1-7 begins to be plugged and matched with the docking hole 2-1 and is fully matched, the material that cannot be discharged along the temporary flow channel will be collected in the spherical concave cavity 1-1 until the temporary flow channel is closed and the docking platform 1-7 and the docking hole 2-1 are fully matched, and the material that cannot be discharged along the temporary flow channel all enters the spherical concave cavity 1-1; ensuring that the material forms a complete spherical feature when being molded in the spherical cavity, and there is no excess part of the molded sphere due to the inability to discharge excess material, resulting in the inability to close the mold, or missing part due to too little material after closing, thereby ensuring the molding quality of the product.
[0061] Furthermore, the middle cavity plate 2 is provided with a square annular groove 2-2 in the circumference of each upper cavity 2-6, and the lower cavity 3-5 is provided with a square annular platform 3-4 in the circumference of the lower cavity 3-5. When the middle cavity plate 2 and the lower cavity plate 3 are covered, the square groove and the square annular platform 3-4 are respectively plugged in and matched.
[0062] Furthermore, both ends of the lower cavity plate 3, the middle cavity plate 2 and the upper cover plate 1 are respectively fixed with handles 3-2, wherein a first arc chamfer is provided on the bottom outer edge of the handle 3-2 of the lower cavity plate 3, and a second arc chamfer is provided on the top outer edge of the handle 3-2 of the middle cavity plate 2, and when the middle cavity plate 2 is covered on the lower cavity plate 3, the first arc chamfer and the second arc chamfer directly constitute an arc bevel, which is convenient for the separation processing of the mold during use.
[0063] Furthermore, a limited fixing angle 1-2 is fixedly connected to the top surface of the upper cover plate 1, and the limited fixing angle 1-2 is a right-angle platform respectively arranged in each top corner area of the upper cover plate 1, and a fixed foot 3-1 is provided on the bottom surface of the lower cavity plate 3, and the fixed foot 3-1 is a square platform respectively located in each top corner area of the lower cavity plate 3. When multiple layers of mold plate groups are stacked, the fixed feet 3-1 of the lower cavity plate 3 of the upper layer can be engaged with and clamped to the inner side of the limited fixing angle 1-2 of the upper cover plate 1 of the next layer to limit the relative slippage of the mold plate groups of adjacent layers, thereby ensuring that the upper cavity 2-6 and the lower cavity 3-5 are tightly combined into a spherical cavity.
[0064] Furthermore, when multiple layers of mold plate groups are stacked, the outer bottom surface of the lower cavity 3-5 of the upper layer abuts against the top surface of the upper cover plate 1 of the lower layer, ensuring force balance of the mold during the stacking process.
[0065] A method for preparing zirconia ceramic beads using the mold:
[0066] Step S1, assembling the middle cavity plate and the lower cavity plate of a layer of mold plate group to form a main cavity assembly;
[0067] Step S2, pouring the gel zirconia ceramic slurry into each cavity of the main cavity assembly from the overflow hole, until the liquid level of the gel zirconia ceramic slurry is higher than the docking hole;
[0068] Step S3, closing the upper cover body onto the middle cavity plate, and draining the excess gel zirconia ceramic slurry;
[0069] Step S4, placing a lower cavity plate on the upper cover plate of the current layer;
[0070] Step S5, repeating steps S1 to S4 to stack several layers of mold plate groups in sequence;
[0071] Step S6, placing a pressing plate on the upper cover plate at the top layer, applying a pressure of 1-1.5 MPa to the mold plate group so that each layer of the mold plate group will not loosen;
[0072] Step S7, standing for more than 1 day to allow the gel zirconia ceramic slurry in each layer of the spherical cavity to solidify into a gel sphere;
[0073] Step S8, opening the upper cover plate of each layer of the mold plate group in turn, placing the main cavity assembly of the middle cavity plate and the lower cavity plate of each layer into an oven, and slowly air-drying at a temperature of 20-30° C. for 0.5-1 day;
[0074] Step S9, after the gel sphere is completely dried, the middle cavity and the lower cavity are separated, and the formed green sphere is taken out for subsequent processing;
[0075] Step S10, cleaning the mold plate set with pure water and drying it for reuse.
[0076] Furthermore, when assembling each layer of the mold plate group, it is necessary to check whether there is a gap. If there is a gap, it should be reassembled and placed flat on the corresponding platform or the upper cover plate of the next layer.
[0077] The above description is only a specific embodiment of the present invention, but the technical features of the present invention are not limited thereto. The present invention can be used in similar products or methods. Any changes or modifications made by any technician in the field of the present invention are covered by the patent scope of the present invention.
Claims
1. A zirconia ceramic bead forming mold, characterized in that: It includes several layers of mold plate groups, and the mold plate group consists of an upper cover plate, a middle cavity plate and a lower cavity plate; A plurality of lower cavities are arranged on the lower cavity plate; A plurality of upper cavities are arranged on the middle cavity plate, an overflow hole is opened on the top of the upper cavity, and a docking hole is provided between the overflow hole and the inner cavity of the upper cavity; A plurality of cover bodies are arranged on the upper cover plate, a pressing platform is provided at the bottom of the cover body, a docking platform is provided at the bottom thereof, and a spherical concave cavity is provided on the bottom surface of the docking platform; The lower cavity plate, the middle cavity plate and the upper cover plate are stacked from bottom to top and covered accordingly, each upper cavity is docked on the corresponding lower cavity, the extrusion platform is engaged with the overflow hole, the docking platform is plugged into the docking hole, and the lower cavity, the upper cavity and the spherical concave cavity surround to form a spherical cavity for forming products; During the process of the extrusion platform being inserted into the overflow hole and the docking platform not yet being fully docked with the docking hole, a temporary flow channel is formed between the outer wall of the extrusion platform and the wall of the overflow hole, and part of the excess material can overflow along the temporary flow channel. When the docking platform begins to be plugged into and mated with the docking hole and is fully mated, the material that cannot be discharged along the temporary flow channel will be collected in the spherical concave cavity until the temporary flow channel is closed and the docking platform and the docking hole are fully mated, and the material that cannot be discharged along the temporary flow channel will all enter the spherical concave cavity.
2. A zirconia ceramic bead forming mold according to claim 1, characterized in that: The top aperture of the overflow hole is larger than the bottom aperture, and the extrusion platform is a frustum structure with a larger top and a smaller bottom that matches the overflow hole.
3. A zirconia ceramic bead forming mold according to claim 2, characterized in that: The bottom edge of the overflow hole and the top edge of the docking hole are connected and arranged, and the bottom edge of the extrusion platform and the top edge of the docking platform are connected and arranged.
4. The zirconia ceramic bead forming mold according to claim 1, characterized in that: The bottom surface of the middle cavity plate is provided with a plurality of grooves, and the top surface of the lower cavity plate is provided with a plurality of bosses. When the middle cavity plate and the lower cavity plate are covered, the bosses and the grooves are plugged and matched with each other.
5. A zirconia ceramic bead forming mold according to claim 4, characterized in that: The grooves are annular grooves respectively surrounding the circumference of the corresponding upper cavity, and the bosses are annular platforms respectively surrounding the circumference of the corresponding lower cavity.
6. The zirconia ceramic bead forming mold according to claim 1, characterized in that: The lower cavity plate, the middle cavity plate and the upper cover plate are respectively provided with handles.
7. A zirconia ceramic bead forming mold according to claim 6, characterized in that: A first arc chamfer is provided on the bottom outer edge of the handle of the lower cavity plate, and a second arc chamfer is provided on the top outer edge of the handle of the middle cavity plate. When the middle cavity plate is covered on the lower cavity plate, an arc bevel is formed between the first arc chamfer and the second arc chamfer.
8. The zirconia ceramic bead forming mold according to claim 1, characterized in that: A limiting fixing angle is provided on the top surface of the upper cover plate, and a fixing foot is provided on the bottom surface of the lower cavity plate. When multiple layers of mold plate groups are stacked, the fixing feet of the lower cavity plate of the upper layer can be engaged with the limiting fixing angle of the upper cover plate of the next layer to limit the slippage of the mold plate groups of adjacent layers.
9. The zirconia ceramic bead forming mold according to claim 1, characterized in that: When multiple layers of mold plate groups are stacked, the outer bottom surface of the lower cavity of the upper layer abuts against the top surface of the upper cover plate of the lower layer.