Anodic oxidation tool for thin-walled parts with holes
By using the barbed structure of the hanger body and conductive hooks in the anodizing tooling, the problems of thin-walled aluminum parts falling off and poor conductivity during the anodizing process are solved, and stable clamping and high-quality processing of the parts are achieved.
Patent Information
- Application Number
- CN202323507158.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-21
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2033-12-21
AI Technical Summary
The existing flat clamping or cylindrical clamping methods can easily lead to problems such as parts falling off, poor conductivity, and oversized clamping marks during the anodizing process of thin-walled aluminum parts.
Anodized tooling using thin-walled parts with holes, including an aluminum alloy or titanium alloy hanger body with a barbed structure and a conductive hook, is fixed through the inclined hanging rod of the hanger body through the center hole of the part, and the hanging rod is used The elastic structure and conductive ring achieve stable clamping and conduction.
It effectively avoids parts falling off and poor conductivity during the anodizing process, reduces fixture imprints, ensures the processing quality and appearance flatness of parts, reduces tooling costs, and improves the versatility of the process.
Smart Images

Figure CN221918286U_ABST
Abstract
Description
Technical Field
[0001] The utility model relates to but is not limited to the technical field of metal surface treatment, in particular to an anodic oxidation tool for thin-walled parts with holes. Background Art
[0002] Anodizing technology for aluminum and aluminum alloys is an important technology for corrosion protection of aviation products. It can improve the corrosion resistance of materials and increase the adhesion of paint films.
[0003] For thin-walled aluminum alloy gasket parts with a thickness of no more than 0.3mm, a plane clamping or outer circle clamping method is usually used to achieve conductivity of the parts during the anodizing process. However, the existing plane clamping or outer circle clamping method generally has problems such as easy falling off, poor conductivity, and excessive clamping marks during the anodizing process of thin-walled aluminum parts. Utility Model Content
[0004] Purpose of the utility model: In order to solve the above-mentioned technical problems, the embodiment of the utility model provides an anodizing tool and an anodizing method for thin-walled parts with holes, so as to solve the existing plane clamping or outer circle clamping method. During the anodizing process of thin-walled aluminum parts, there are generally problems such as easy falling off, poor conductivity, and excessive clamp print.
[0005] Technical solution of the utility model: The embodiment of the utility model provides an anodizing tool for thin-walled parts with holes, comprising: a hanger body 3 and a conductive hook 1, wherein the hanger body 3 is configured as an aluminum alloy or titanium alloy hanger with a barb structure;
[0006] Wherein, a plurality of upwardly inclined hanging rods are arranged on both sides of the hanger body 3, each hanging rod is formed by bending a rod wall on both sides of an alloy wire, a single-side hanging rod forms a barb structure, and the hanging rods with barb structures on both sides form a hanger with a fishbone-shaped barb structure, so that the hanging rods on both sides of the hanger body pass through the central hole of the thin-walled part with holes, thereby fixing the part on each hanging rod;
[0007] The end of the conductive hook 1 is provided with a conductive ring 2 for connecting with the hanger body 3 through the conductive ring 2, so that during the anodizing process, the conductive hook 1 and the conductive ring 2 conduct electricity to the entire hanger body 3, thereby performing anodizing treatment on the perforated thin-walled parts on each hanging rod of the hanger body 3.
[0008] Optionally, in the anodizing tooling for thin-walled parts with holes as described above,
[0009] Each hanging rod arranged on both sides of the hanger body 3 is an elastic structure, which is used to compress the end of the hanging rod by applying external force before hanging the thin-walled part with a hole, so that the thin-walled part with a hole can be inserted into the compressed hanging rod through the center hole, and the external force used for compression can be released. The hanging rod's own elastic force makes its structure rebound to clamp and fix the thin-walled part with a hole.
[0010] Optionally, in the anodizing tooling for thin-walled parts with holes as described above,
[0011] The hanger body 3 is formed by bending an alloy wire of aluminum alloy or titanium alloy in a preset structure in a dragon-tail-like manner, and one end of the alloy wire is connected to the conductive ring 2 .
[0012] Optionally, in the anodizing tooling for thin-walled parts with holes as described above,
[0013] After the alloy wire is bent to form an end of a hanging rod, when it extends along the hanging rod arm to the boundary position of the hanging rods on both sides, it is bent obliquely upward to the other hanging rod at a certain angle to form the hanging rod on the other side by bending, so that the two hanging rods formed by the bending of the alloy wire form a boundary line in the middle; or,
[0014] After the alloy wire is bent in an arc form to form a hanging rod end, it is extended along the curvature trend of the hanging rod arm to the position of the hanging rod end on the other side and then bent to form the other hanging rod end on the other side, and then continues to extend and bend along the curvature trend of the hanging rod arm formed by the current bending, so that the outer contour formed by the bending of the alloy wire in an arc form is a hanger main body 3 with a fan-shaped structure.
[0015] Optionally, in the anodizing tooling for thin-walled parts with holes as described above,
[0016] The hanger body 3 is formed by bending two aluminum alloy or titanium alloy alloy wires, wherein the first alloy wire is bent to form a hanger rod with a barb structure on one side of the hanger body, and the second alloy wire is bent to form a hanger rod with a barb structure on the other side of the hanger body;
[0017] One end of the first alloy wire is connected to the conductive ring 2 , and at least one end of the second alloy wire is connected to the first alloy wire; or, after one end of the first alloy wire and one end of the second alloy wire are connected, the extended end is connected to the conductive ring 2 .
[0018] Optionally, in the anodizing tooling for thin-walled parts with holes as described above, the conductive hook 1 and the conductive ring 2 are made of copper material.
[0019] The present invention also provides an anodizing method for thin-walled parts with holes, comprising:
[0020] Step 1, multiple thin-walled parts with holes are sleeved on a plastic tube, and the multiple parts are evenly dispersed, and the parts are cleaned by ultrasonic wave;
[0021] Step 2, after cleaning, remove the parts from the plastic tube, and install each part on each hanging rod of the hanger body 3 with a barb structure of the anodized tooling as described in any of the above items, and hang a part on the end of each hanging rod;
[0022] Step 3, anodizing the thin-walled parts with holes mounted on the anodizing tooling.
[0023] Optionally, in the anodizing method for a porous thin-walled part as described above, step 1 comprises:
[0024] Step 11, sleeve a plurality of thin-walled parts with holes on a plastic tube whose inner hole diameter is smaller than the plastic tube, and evenly disperse the plurality of parts;
[0025] Step 12, adjacent parts sleeved on the plastic tube are isolated by buckles to prevent accumulation between the parts;
[0026] Step 13, using ARDROX 5503 organic solvent to pre-clean the parts, with an ultrasonic frequency of 20KHZ-28KHZ, a power of 1.5kW, and a cleaning time of 5min-10min;
[0027] Step 14, use a neutral water-based cleaning agent to clean the parts, with an ultrasonic frequency of 28KHZ, a power of 3kW, and a cleaning time of 10min-30min; after cleaning, the water film on the surface of the parts is continuous for at least 30s;
[0028] Step 15, after cleaning, immerse the cleaned parts in anhydrous ethanol solution and dry them.
[0029] Optionally, in the above-mentioned anodizing method for thin-walled parts with holes, the part hanging method in step 2 is:
[0030] Before hanging the thin-walled part with a hole, the elastic deformation property of the hanging rod is utilized to compress the end of the hanging rod by applying an external force, so that the thin-walled part with a hole is inserted into the compressed hanging rod through the center hole, and the external force used for compression is released. The hanging rod's own elastic force makes its structure rebound to clamp and fix the thin-walled part with a hole.
[0031] Optionally, in the anodizing method for thin-walled parts with holes as described above, step 3 comprises:
[0032] The parts are processed through the processes of alkali washing → hot water washing → cold water washing → deoxidation → cold water washing → anodizing → cold water washing → filling → drying;
[0033] Among them, the process control conditions are: the alkali washing temperature is controlled at 40℃-60℃, and the time is 6s-30s; the anodizing process is prohibited from using strong compressed air stirring, and slight compressed air stirring or mechanical stirring is used.
[0034] Beneficial effects of the utility model: In order to improve the problems of detachment, poor conductivity, and excessive clamping points of anodized thin-walled parts with holes, the utility model embodiment combines the size, morphology and characteristics of the parts, and provides an anodizing tool for aluminum alloy thin-walled parts, and proposes an anodizing process method using the anodizing tool. On the one hand, the anodizing tool provided by the utility model embodiment is formed by a hanger body 3 and a conductive hook 1. The hanger body 3 is configured as an alloy hanger with a barb structure, and a plurality of inclined upward hanging rods are arranged on both sides thereof. Each hanging rod is formed by bending out two side rod walls from an alloy wire, and the single-side hanging rod forms a barb structure, and the hanging rods with barb structures on both sides form a hanger with a fishbone-shaped barb structure, so that the hanging rods on both sides of the hanger body pass through the central hole of the thin-walled parts with holes, thereby fixing the parts on each hanging rod; on the other hand, in view of the characteristics of thin-walled parts with holes, such as light weight, thin material wall, and inner hole, a method for anodizing thin-walled parts with holes using the above-mentioned tool is provided. The technical solution provided by the utility model has the following beneficial effects:
[0035] First, the hanger body 3 of the barbed structure provided by the embodiment of the utility model has a simple structure, low cost, and is easy to produce;
[0036] Secondly, the hanger body 3 with the barbed structure provided in the embodiment of the utility model can utilize the elastic deformation performance of the hanging rod itself to hang the parts, and utilize the inner hole of the thin-walled part itself to constrain the hanging rod, thereby ensuring that the thin-walled parts are clamped and fastened and convenient for assembly and disassembly, and can also ensure that the thin-walled parts do not fall off, have poor conductivity, or have too large a clamp print during processing;
[0037] Thirdly, the principle of the anodizing treatment method provided by the utility model is simple, and the anodizing tooling used can be reused, thereby reducing costs;
[0038] Fourthly, anodizing is performed after the thin-walled parts are hung with the anodizing tooling provided in the embodiment of the utility model. Based on the tooling structure and the hanging effect, the process of the parts can meet the process requirements of anodizing, and ultimately the product performance is uniform and the qualified rate is high.
[0039] In summary, the process method for anodizing aluminum alloy thin-walled parts with holes provided by the embodiment of the utility model can achieve the whole process of parts processing without deformation, no falling off, small fixture marks, and the finished parts meet the requirements of parts appearance and flatness. In addition, in conjunction with the process method, a special tooling is made to solve the problems of part deformation and difficult clamping in the processes of degreasing, alkali washing, oxidation, etc., and improve the product quality of aluminum alloy thin-walled small parts.
[0040] The tooling provided in the embodiment of the utility model has been successfully applied to the anodizing treatment of a certain type of gasket parts. If there are other specifications of thin-walled small parts in the future, it is only necessary to use aluminum wire to wind the corresponding specification device according to the drawing. This method can meet the anodizing treatment of general thin-walled parts, ensure that the parts do not fall off, conduct electricity poorly, and the fixture prints too large, etc., and has strong versatility. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] The accompanying drawings are used to provide a further understanding of the technical solution of the utility model and constitute a part of the specification. Together with the embodiments of the present application, they are used to explain the technical solution of the utility model and do not constitute a limitation on the technical solution of the utility model.
[0042] Figure 1 A schematic structural diagram of an anodizing tool for thin-walled parts with holes provided in an embodiment of the utility model;
[0043] Figure 2 A schematic structural diagram of another anodizing tool for thin-walled parts with holes provided in an embodiment of the utility model;
[0044] Figure 3 A schematic structural diagram of another anodizing tooling for thin-walled parts with holes provided in an embodiment of the utility model. DETAILED DESCRIPTION
[0045] In order to make the purpose, technical solution and advantages of the utility model more clear, the embodiments of the utility model will be described in detail with reference to the accompanying drawings. It should be noted that the embodiments and features in the embodiments of the present application can be combined with each other arbitrarily without conflict.
[0046] As described in the above background technology, the conventional conductive method for thin-walled aluminum alloy gaskets during anodizing is to adopt a planar clamping method or an outer circle clamping method.
[0047] Among them, the plane clamping method usually uses a cylindrical spring clamp, inserting the parts directly into the spring, and achieving the purpose of conduction and clamping through the clamping force of the spring. This clamping method is prone to various problems during the clamping process, such as the parts are easily deformed due to force extrusion, the large clamping contact area of the spring clamp affects the surface oxidation quality, the clamp is easy to loosen after use, and the clamping force is insufficient, which often leads to no current when the thin-walled small parts of aluminum alloy are oxidized, and the parts fall off into the electroplating solution.
[0048] In addition, the external circle clamping adopts a clamping fixture to clamp the parts between the clamps, and fix the parts by the clamping force between the upper and lower clamps to achieve conductivity and fastening. This clamping method is easy to cause deformation of the parts. When clamping, the contact surface between the parts and the clamps is relatively small, and it is easy to fall off in the stirred solution.
[0049] In order to improve the problems of anodizing shedding, poor conductivity, and excessive clamping points of thin-walled small parts, the utility model embodiment designs an anodizing tool for aluminum alloy thin-walled parts in combination with product size and morphology, and an anodizing process method using the anodizing tool, that is, provides an anodizing tool and an anodizing method for thin-walled parts with holes.
[0050] The utility model provides the following specific embodiments which can be combined with each other, and the same or similar concepts or processes may not be described in detail in some embodiments.
[0051] Figure 1 The schematic diagram of the structure of an anodizing tool for thin-walled parts with holes provided by the embodiment of the utility model. Figure 1 As shown, the main structure of the anodizing tool includes: a hanger body 3 and a conductive hook 1, and the hanger body 3 is configured as an aluminum alloy or titanium alloy hanger with a barb structure.
[0052] like Figure 1 In the structure of the anodizing tooling shown, a plurality of upwardly inclined hanging rods are arranged on both sides of the hanger body 3, and the hanging rod on one side forms a barb structure, and the hanging rods of the barb structure on both sides form a hanger with a fishbone-shaped barb structure, so that the hanging rods on both sides of the hanger body pass through the central hole of the perforated thin-walled part to fix the part on each hanging rod.
[0053] In the embodiment of the utility model, the end of the conductive hook 1 is provided with a conductive ring 2, which is used to connect with the hanger body 3 through the conductive ring 2, so that during the anodizing process, the conductive hook 1 and the conductive ring 2 conduct electricity to the entire hanger body 3, thereby performing anodizing treatment on the perforated thin-walled parts on each hanging rod of the hanger body 3. The conductive hook 1 and the conductive ring 2 in the embodiment of the utility model can be made of copper material.
[0054] It should be noted that each of the hanging rods arranged on both sides of the hanger body 3 of the embodiment of the utility model is an elastic structure, and the operation process of using the hanger body 3 to hang the thin-walled parts with holes is as follows:
[0055] Before hanging the thin-walled part with a hole, the end of the hanging rod is compressed by applying external force based on its elastic deformation performance, so that the thin-walled part with a hole is inserted into the hanging rod in a compressed state through the center hole, and the external force used for compression is released, thereby releasing the compression amount, and the structure of the hanging rod rebounds through its own elastic force to fix the thin-walled part with a hole.
[0056] In one implementation of the present utility model, Figure 1 As shown, the hanger body 3 is formed by bending an alloy wire of aluminum alloy or titanium alloy in a dragon-tail-like manner in a preset structure, and one end of the alloy wire is connected to the conductive ring 2 .
[0057] In another embodiment of this implementation, Figure 1 As shown, after the alloy wire is bent to form an end of a hanging rod, it extends along the hanging rod arm to the boundary position of the hanging rods on both sides, and then bends obliquely upward to the other hanging rod at a certain angle to form the hanging rod on the other side, so that the two hanging rods formed by the bending of the alloy wire form a dividing line in the middle, as shown in FIG. Figure 1 The structure of the hanger body 3 is shown.
[0058] In another embodiment of this implementation, Figure 2 The figure is a schematic diagram of the structure of another anodizing tooling for thin-walled parts with holes provided by an embodiment of the utility model. In this embodiment, after the alloy wire is bent in an arc to form a hanging rod end, it is extended along the arc trend of the hanging rod arm to the position of the hanging rod end on the other side and then bent to form the hanging rod end on the other side, and then continues to extend and bend along the arc trend of the hanging rod arm formed by the current bending to the position of the previous hanging rod end, so that the outer contour formed by the bending of the alloy wire in the arc form is a fan-shaped structure of the hanger body 3.
[0059] In another implementation of the embodiment of the utility model, a structure of the hanger body 3 is provided, such as Figure 3 FIG. 1 is a schematic diagram of the structure of another anodizing tooling for thin-walled parts with holes provided by an embodiment of the utility model. In this implementation, the hanger body 3 is no longer formed by bending one alloy wire, but is formed by bending two aluminum alloy or titanium alloy alloy wires. The first alloy wire is bent to form a hanger rod with a barb structure on one side of the hanger body, and the second alloy wire is bent to form a hanger rod with a barb structure on the other side of the hanger body. Figure 3 The structure shown.
[0060] In this implementation, one end of the first alloy wire is connected to the conductive ring, and at least one end of the second alloy wire is connected to the first alloy wire; or, after one end of the first alloy wire is connected to one end of the second alloy wire, the extended end is connected to the conductive ring 2. It should be noted that when two alloy wires are bent to form a hanging rod with barbed structures on both sides, it is required that the alloy wires forming the barbed structures on both sides can be conductive through the conductive hook 1 and the conductive ring 2, so that the parts hung on the ends of the hanging rod can be anodized.
[0061] Based on the anodizing method for thin-walled parts with holes provided in the above embodiments of the utility model, the embodiments of the utility model also provide an anodizing method for thin-walled parts with holes. The main implementation process of the anodizing method is: first, the thin-walled parts with holes are sleeved on a plastic tube smaller than the diameter of its inner hole, and multiple parts are evenly dispersed by shaking, and the parts are cleaned by ultrasonic waves. The cleaned parts are installed on an aluminum alloy or titanium alloy hanger with a barbed structure, and then the parts are anodized. The specific method includes the following implementation steps:
[0062] Step 1: sleeve a plurality of thin-walled parts with holes on a plastic tube whose inner hole diameter is smaller than the plastic tube, evenly disperse the plurality of parts, and clean the parts by ultrasonic wave.
[0063] This step is for cleaning the parts to be anodized. On the one hand, for batch cleaning, the thin-walled parts with holes are threaded together with plastic tubes smaller than their inner holes. On the other hand, to prevent accumulation between parts, the thin-walled parts with holes can be isolated with buckles and arranged horizontally.
[0064] The cleaning operation process includes: using ARDROX 5503 organic solvent to pre-clean the parts, ultrasonic frequency 20KHZ-28KHZ, power 1.5kW, cleaning 5min-10min.
[0065] Use a neutral water-based cleaning agent to clean the parts, ultrasonic frequency 28KHZ, power 3kW, cleaning 10min-30min. After cleaning, the water film on the surface of the parts will last for at least 30s.
[0066] After cleaning, immerse the cleaned parts in anhydrous ethanol solution and let them dry.
[0067] Step 2: After cleaning, remove the parts from the plastic tube and install them in Figures 1 to 3 On each hanging rod of the hanger body 3 with a barb structure in the anodizing tool shown.
[0068] In this step, only one part is allowed to be hung on each end of the hanging rod, and the part hanging method is: before hanging the thin-walled part with a hole, the elastic deformation performance of the hanging rod is used to compress the end of the hanging rod by applying an external force, so that the thin-walled part with a hole is inserted into the hanging rod in a compressed state through the center hole, and the external force used for compression is released. The hanging rod's own elastic force makes its structure rebound to clamp and fix the thin-walled part with a hole.
[0069] Step 3, anodizing the thin-walled parts with holes mounted on the anodizing tooling.
[0070] In this step, the parts are processed through alkali washing → hot water washing → cold water washing → deoxidation → cold water washing → anodizing → cold water washing → filling → drying. To ensure that the parts do not fall off the hanging rod during the anodizing operation, the process control conditions are: the alkali washing temperature is controlled at 40℃-60℃, and the time is 6s-30s; strong compressed air stirring is not allowed during the oxidation process, and only slight compressed air stirring or mechanical stirring is allowed.
[0071] In order to improve the problems of detachment, poor conductivity, and excessive clamping points of anodized thin-walled parts with holes, the embodiment of the utility model designs an anodizing tool for aluminum alloy thin-walled parts in combination with the size, morphology and characteristics of the parts, and proposes a process method for anodizing treatment using the anodizing tool. On the one hand, the anodizing tool provided by the embodiment of the utility model is formed by a hanger body 3 and a conductive hook 1. The hanger body 3 is configured as an alloy hanger with a barb structure, and a plurality of inclined upward hanging rods are arranged on both sides thereof. Each hanging rod is formed by bending out two side rod walls from an alloy wire, and the single-side hanging rod forms a barb structure, and the hanging rods with barb structures on both sides form a hanger with a fishbone-shaped barb structure, so that the hanging rods on both sides of the hanger body pass through the central hole of the thin-walled parts with holes, thereby fixing the parts on each hanging rod; on the other hand, in view of the characteristics of thin-walled parts with holes, such as light weight, thin material wall, and inner hole, a method for anodizing thin-walled parts with holes using the above-mentioned tool is provided. The technical solution provided by the utility model has the following beneficial effects:
[0072] First, the hanger body 3 of the barbed structure provided by the embodiment of the utility model has a simple structure, low cost, and is easy to produce;
[0073] Secondly, the hanger body 3 with the barbed structure provided in the embodiment of the utility model can utilize the elastic deformation performance of the hanging rod itself to hang the parts, and utilize the inner hole of the thin-walled part itself to constrain the hanging rod, thereby ensuring that the thin-walled parts are clamped and fastened and convenient for assembly and disassembly, and can also ensure that the thin-walled parts do not fall off, have poor conductivity, or have too large a clamp print during processing;
[0074] Thirdly, the principle of the anodizing treatment method provided by the utility model is simple, and the anodizing tooling used can be reused, thereby reducing costs;
[0075] Fourthly, anodizing is performed after the thin-walled parts are hung with the anodizing tooling provided in the embodiment of the utility model. Based on the tooling structure and the hanging effect, the process of the parts can meet the process requirements of anodizing, and ultimately the product performance is uniform and the qualified rate is high.
[0076] The process method for anodizing aluminum alloy thin-walled parts with holes provided in the embodiment of the utility model can achieve the whole process of parts processing without deformation, no falling off, small fixture mark, and the finished parts meet the requirements of parts appearance and flatness. In addition, with the process method, a special tooling is made to solve the problems of part deformation and difficult clamping in the processes of degreasing, alkali washing, oxidation, etc., and improve the product quality of aluminum alloy thin-walled small parts.
[0077] The tooling provided in the embodiment of the utility model has been successfully applied to the anodizing treatment of a certain type of gasket parts. If there are other specifications of thin-walled small parts in the future, it is only necessary to use aluminum wire to wind the corresponding specification device according to the drawing. This method can meet the anodizing treatment of general thin-walled parts, ensure that the parts do not fall off, conduct electricity poorly, and the fixture prints too large, etc., and has strong versatility.
[0078] The following is a schematic illustration of the implementation of the anodizing tooling and anodizing method for thin-walled parts with holes provided in the embodiments of the utility model through some implementation examples.
[0079] Implementation Example 1
[0080] In this implementation example 1, a certain type of gasket is subjected to sulfuric acid anodizing treatment, and the inner diameter of the part is 12 mm, the outer diameter is 44 mm, and the thickness is 0.3 mm.
[0081] Step 1: Use Φ8 plastic tubes to thread thin-walled parts together, separate them with plastic buckles, and arrange them horizontally;
[0082] Step 2: Pre-clean the parts with ARDROX 5503 organic solvent, ultrasonic frequency 20KHZ, power 1.5kW, cleaning for 10 minutes.
[0083] Step 3: Use a neutral water-based cleaning agent to clean the parts, with an ultrasonic frequency of 28KHZ, a power of 3kW, and a cleaning time of 10 minutes. After cleaning, the water film on the surface of the parts will remain for 30 seconds.
[0084] Step 4: Immerse the cleaned parts in anhydrous ethanol solution and dry them.
[0085] Step 5: Wear clean gloves to remove the parts from the plastic tube and hang them on the hanging rod of the hanger body with a barbed structure. Only one part is allowed to be hung on each hanging rod of the hanger body.
[0086] Step 6: Alkaline washing (40℃, 30s) → hot water washing → cold water washing → deoxidation → cold water washing → anodizing (slightly stirring the tank liquid) → cold water washing → filling → drying and other steps to complete the parts processing.
[0087] Implementation Example 2
[0088] In this implementation example 2, a certain type of gasket is subjected to sulfuric acid anodizing treatment, and the inner diameter of the part is 10 mm, the outer diameter is 35 mm, and the thickness is 0.2 mm.
[0089] Step 1: Use Φ8 plastic tubes to thread thin-walled parts together, separate them with plastic buckles, and arrange them horizontally;
[0090] Step 2: Pre-clean the parts with ARDROX 5503 organic solvent, ultrasonic frequency 28KHZ, power 1.5kW, cleaning for 5 minutes.
[0091] Step 3: Use a neutral water-based cleaning agent to clean the parts, with an ultrasonic frequency of 28KHZ, a power of 3kW, and a cleaning time of 30 minutes. After cleaning, the water film on the surface of the parts will remain for 30 seconds.
[0092] Step 4: Immerse the cleaned parts in anhydrous ethanol solution and dry them.
[0093] Step 5: Remove the parts from the plastic tube and hang them on the hanging rod of the hanger body with a barbed structure. Only one part is allowed to be hung on each hanging rod of the hanger body.
[0094] Step 6: Complete the parts processing through the steps of alkali washing (60℃, 6s) → hot water washing → cold water washing → deoxidation → cold water washing → anodizing (slightly stirring) → cold water washing → filling → drying.
[0095] Implementation Example 3
[0096] In this implementation example 3, a certain type of gasket is subjected to chromic acid anodizing treatment, and the inner diameter of the part is 8 mm, the outer diameter is 22 mm, and the thickness is 0.3 mm.
[0097] Step 1: Use Φ6 plastic tubes to thread thin-walled parts together, separate them with plastic buckles, and arrange them horizontally;
[0098] Step 2: Pre-clean the parts with ARDROX 5503 organic solvent, ultrasonic frequency 28KHZ, power 1.5kW, cleaning for 6 minutes.
[0099] Step 3: Use a neutral water-based cleaning agent to clean the parts, with an ultrasonic frequency of 28KHZ, a power of 3kW, and a cleaning time of 20 minutes. After cleaning, the water film on the surface of the parts will remain for 30 seconds.
[0100] Step 4: Immerse the cleaned parts in anhydrous ethanol solution and dry them.
[0101] Step 5: Remove the parts from the plastic tube and hang them on the hanging rod of the hanger body with a barbed structure. Only one part is allowed to be hung on each hanging rod of the hanger body.
[0102] Step 6: Complete the parts processing through the steps of alkaline washing (60℃, 6s) → hot water washing → cold water washing → deoxidation → cold water washing → anodic chromic acid oxidation (slightly stirring) → cold water washing → filling → drying.
[0103] The parts in the above-mentioned implementation examples are processed according to the method provided by the utility model, which can effectively prevent the occurrence of parts falling off, poor conductivity, large fixture marks, etc. during the oxidation process of thin-walled small parts, and the appearance and quality meet the requirements of the drawings.
[0104] Although the implementation methods disclosed in the utility model are as above, the content is only an implementation method adopted to facilitate the understanding of the utility model, and is not used to limit the utility model. Any technician in the field to which the utility model belongs can make any modifications and changes in the form and details of implementation without departing from the spirit and scope disclosed in the utility model, but the scope of patent protection of the utility model shall still be based on the scope defined in the attached claims.
Claims
1. An anodizing tool for thin-walled parts with holes, characterized in that: The anodizing tool comprises: a hanger body (3) and a conductive hook (1); the hanger body (3) is configured as an aluminum alloy or titanium alloy hanger with a barbed structure; Wherein, a plurality of upwardly inclined hanging rods are arranged on both sides of the hanger body (3), each hanging rod is formed by bending a rod wall on both sides of an alloy wire, a single-side hanging rod forms a barb structure, and the hanging rods with barb structures on both sides form a hanger with a fishbone-shaped barb structure, so that the hanging rods on both sides of the hanger body pass through the central hole of the thin-walled part with holes, thereby fixing the part on each hanging rod; The end of the conductive hook (1) is provided with a conductive ring (2) for connecting with the hanger body (3) via the conductive ring (2), so that during the anodizing process, the conductive hook (1) and the conductive ring (2) conduct electricity to the entire hanger body (3), thereby performing anodizing treatment on the perforated thin-walled parts on each hanging rod of the hanger body (3).
2. The anodizing tool for thin-walled parts with holes according to claim 1, characterized in that: Each of the hanging rods arranged on both sides of the hanger body (3) is an elastic structure, which is used to compress the end of the hanging rod by applying external force before hanging the thin-walled part with a hole, so that the thin-walled part with a hole is inserted into the hanging rod in a compressed state through the center hole, and the external force used for compression is released. The hanging rod's own elastic force makes its structure rebound to clamp and fix the thin-walled part with a hole.
3. The anodizing tool for thin-walled parts with holes according to claim 2, characterized in that: The hanger body (3) is formed by bending an alloy wire of aluminum alloy or titanium alloy in a predetermined structure in a dragon-tail-like manner, and one end of the alloy wire is connected to the conductive ring (2).
4. The anodizing tool for thin-walled parts with holes according to claim 3, characterized in that: After the alloy wire is bent to form an end of a hanging rod, when it extends along the hanging rod arm to the dividing position of the hanging rods on both sides, it is bent obliquely upward to the other hanging rod at a certain angle to form the hanging rod on the other side, so that the hanging rods on both sides formed by bending the alloy wire form a dividing line in the middle.
5. The anodizing tool for thin-walled parts with holes according to claim 3, characterized in that: After the alloy wire is bent in an arc form to form a hanging rod end, it is extended along the arc trend of the hanging rod arm to the position of the hanging rod end on the other side and then bent to form the hanging rod end on the other side, and then continues to extend and bend along the arc trend of the hanging rod arm formed by the current bending to the position of the previous hanging rod end, so that the outer contour formed by the bending of the alloy wire in an arc form is a fan-shaped structure of the hanger main body (3).
6. The anodizing tool for thin-walled parts with holes according to claim 2, characterized in that: The hanger body (3) is formed by bending two aluminum alloy or titanium alloy alloy wires, wherein the first alloy wire is bent to form a hanger rod with a barb structure on one side of the hanger body, and the second alloy wire is bent to form a hanger rod with a barb structure on the other side of the hanger body.
7. The anodizing tool for thin-walled parts with holes according to claim 6, characterized in that: One end of the first alloy wire is connected to the conductive ring (2), and at least one end of the second alloy wire is connected to the first alloy wire; or, after one end of the first alloy wire and one end of the second alloy wire are connected, the extended end is connected to the conductive ring (2).