Pole piece, roll core and battery
By setting a reinforcement layer at the root of the pole ear and pre-folding and curing during winding, the problems of pole ear collapse and folding are solved, improving the reliability of the pole sheet and the yield of the core, reducing material waste and Manufacturing cost.
Patent Information
- Application Number
- CN202323671291.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-31
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2033-12-31
AI Technical Summary
During the winding of the battery pole, the ears are prone to collapse or fold, resulting in poor reliability of the pole, reduced yield and waste of material.
A pole sheet is designed, including a current collector, an active material layer and a reinforcement layer, which is arranged at one end of the pole ear close to the main body, and increases the strength by increasing the thickness at the root of the pole ear, and pre-folding and curing the reinforcement layer during winding. To prevent collapse and folding.
Effectively prevent the collapse and folding of the extreme ears, improve the reliability of the electrode sheet and the yield of the core, and control the manufacturing cost of the winding assembly.
Smart Images

Figure CN221994498U_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of battery technology, and in particular to a pole piece, a winding core and a battery. Background Art
[0002] In the related art, the battery cell includes a shell and a positive electrode sheet, a separator and a negative electrode sheet that are stacked or wound. The electrode sheet includes a current collector and an active material layer arranged on the main body of the current collector. One side of the current collector is a blank area where the active material layer is not arranged. Usually, the blank area serves as the pole ear of the pole sheet, and the pole ear includes a pole ear body and a pole ear root that connects the pole ear body to the main body. Due to the thin thickness of the current collector, during the process of winding the pole sheet to make a winding core, it is easy for the pole ear to collapse and fold at the pole ear root, resulting in poor reliability of the pole sheet. The folding of the pole ear will cause the yield of the winding core to decrease, resulting in material waste. Utility Model Content
[0003] The embodiments of the present application provide a pole piece, a winding core and a battery, which can improve the problem of poor reliability of the pole piece.
[0004] In a first aspect, an embodiment of the present application provides a pole piece. The pole piece includes a current collector, an active material layer and a reinforcement layer. The current collector includes a pole ear and a body, one side of the pole ear is connected to the body; the active material layer is arranged on the body; and the reinforcement layer is arranged on one end of the pole ear close to the body.
[0005] In one embodiment, a winding center is defined, and the pole piece has an A surface facing the winding center and a B surface away from the winding center; both the A surface and the B surface are provided with a strengthening layer and an active material layer.
[0006] In one embodiment, along the width direction of the pole piece, the strengthening layer on the A side has a width dimension L1, the strengthening layer on the B side has a width dimension L2, and the pole ear has a width dimension H1, satisfying: 15% H1≤L1≤50% H1, 15% H1≤L2≤50% H1.
[0007] In one embodiment, L1<L2.
[0008] In one embodiment, 50% L2 ≤ L1 ≤ 90% L2.
[0009] In one embodiment, 15% H1≤L1≤45% H1.
[0010] In one embodiment, along the thickness direction of the pole piece, the strengthening layer on the A side has a thickness dimension D1, and the strengthening layer on the B side has a thickness dimension D2, satisfying: D1>D2.
[0011] In one embodiment, the electrode is a positive electrode, and 30% H1≤L2≤50% H1.
[0012] In one embodiment, a side of the strengthening layer on the A surface facing away from the active material layer on the A surface is coplanar with a side of the strengthening layer on the B surface facing away from the active material layer on the B surface.
[0013] In one embodiment, in surface A, the strengthening layer is spaced apart from the edge of the main body, and the distance between the strengthening layer and the edge of the main body is L4; in surface B, the strengthening layer is spaced apart from the edge of the main body, and the distance between the strengthening layer and the edge of the main body is L5, satisfying: L4>L5.
[0014] In one embodiment, along the width direction of the pole piece, the strengthening layer on the A surface has a width dimension L1, which satisfies: 15% L1≤L4≤27% L1.
[0015] In one embodiment, 0.25 mm ≤ L5 < L4 ≤ 1.5 mm.
[0016] In one embodiment, along the thickness direction of the pole piece, the pole piece has a thickness dimension D4 at the active material layer; the pole piece has a thickness dimension D0 at the strengthening layer, satisfying: 50% D4≤D0≤90% D4.
[0017] In one embodiment, the strengthening layer includes a first adhesive layer disposed on the tab.
[0018] In one embodiment, the strengthening layer further includes an expansion layer, and the expansion layer is disposed on a side of the first adhesive layer away from the tab.
[0019] In one embodiment, the expansion layer further includes a second adhesive layer and a PI layer, and the PI layer is arranged on a side of the expansion layer away from the first adhesive layer through the second adhesive layer.
[0020] In one embodiment, the first adhesive layer and / or the second adhesive layer is a thermosetting adhesive or a UV curing adhesive or a mixture of a UV curing adhesive and an insulating filler.
[0021] In a second aspect, an embodiment of the present application further provides a winding core, comprising a positive electrode sheet, a separator and a negative electrode sheet stacked and wound, wherein the positive electrode sheet is the aforementioned electrode sheet, or both the positive electrode sheet and the negative electrode sheet are the aforementioned electrode sheets.
[0022] In one embodiment, a winding center is defined, and the surface of the positive electrode sheet facing the winding center is surface A. Along the width direction of the positive electrode sheet, the reinforcement layer on surface A has a first end face of the active material layer facing surface A and a second end face of the active material layer facing away from surface A. The plane parallel to the winding center is taken as the projection plane, and the direction perpendicular to the projection plane is taken as the projection direction. In the projection plane, the orthographic projection of the main edge of the negative electrode sheet is located between the orthographic projection of the first end face and the orthographic projection of the second end face.
[0023] In one embodiment, in the projection plane, the orthographic projection of the edge of the separator is located between the orthographic projection of the second end surface and the orthographic projection of the main body edge of the negative electrode sheet.
[0024] In a third aspect, an embodiment of the present application further provides a battery, comprising the aforementioned winding core.
[0025] Beneficial effects of the embodiments of the present application:
[0026] In an embodiment of the present application, a reinforcement layer is provided at one end of the pole ear close to the main body, so that the thickness of the root of the pole ear can be increased, thereby increasing the strength of the root of the pole ear, and further, when the pole piece is wound, the pole ear can be effectively prevented from collapsing and folding, thereby ultimately improving the reliability of the pole piece. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without creative work.
[0028] Figure 1 is a schematic diagram of the structure provided by an embodiment of the present application as viewed from the cut surface of the pole piece;
[0029] Figure 2 yes Figure 1 The enlarged view of point A in the middle;
[0030] Figure 3 It is a schematic diagram of the positions of the strengthening layer on the A side and the strengthening layer on the B side of the pole piece provided in the embodiment of the present application;
[0031] Figure 4 is a schematic structural diagram of the A surface of the pole piece provided in an embodiment of the present application;
[0032] Figure 5 is a schematic structural diagram of the B surface of the pole piece provided in an embodiment of the present application;
[0033] Figure 6 is a schematic diagram of the structure of the strengthening layer provided in the embodiment of the present application;
[0034] Figure 7 is a schematic structural diagram of another strengthening layer provided in an embodiment of the present application;
[0035] Figure 8 is a schematic structural diagram of a winding core viewed from a cut surface of a pole piece provided in an embodiment of the present application;
[0036] Fig. 9 yes Figure 8 Enlarged view of point C in the middle;
[0037] Fig.10 This is a schematic diagram of the process of preparing a core provided in an embodiment of the present application. Figure 1 ;
[0038] Fig.11 This is a schematic diagram of the process of preparing a core provided in an embodiment of the present application. Figure 2 ;
[0039] Fig.12 This is a schematic diagram of the process of preparing a core provided in an embodiment of the present application. Figure 3 .
[0040] Description of reference numerals:
[0041] 001-pole piece;
[0042] 011-current collector; 111-ear; 112-body;
[0043] 012-active material layer; 013-strengthening layer; 131-first adhesive layer; 132-expansion layer; 134-second adhesive layer; 135-PI layer;
[0044] 002-positive electrode sheet; 003-diaphragm; 004-negative electrode sheet. DETAILED DESCRIPTION
[0045] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of this application.
[0046] In addition, it should be understood that the specific embodiments described herein are only used to illustrate and explain the present application and are not used to limit the present application. In the present application, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present application, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined.
[0047] In the description of this application, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0048] The terms "comprises," "comprising," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that includes a list of elements includes not only those elements but also other elements not explicitly listed, or also includes elements inherent to such process, method, article, or apparatus.
[0049] In the description of the embodiments of the present application, words such as "example" or "for example" are used to indicate examples, illustrations or descriptions. Any embodiment or design described as "example" or "for example" in the embodiments of the present application is not to be interpreted as being more preferred or having more advantages than another embodiment or design. The use of words such as "example" or "for example" is intended to present relative concepts in a clear manner.
[0050] Before introducing a pole piece, winding core and battery of the present application, the related technology of the present application is first introduced.
[0051] In the related art, since the thickness of the current collector of the pole piece is relatively thin, the pole ear is easily folded during the process of winding the pole piece with the pole ear and then undergoing multiple steps to form a finished battery cell, thereby reducing the yield of the pole piece and causing waste of materials.
[0052] Based on this, a smoothing plate is usually provided to smooth the pole piece to prevent the pole ear from folding. However, the smoothing plate needs to be provided at different positions for different pole pieces, which has poor versatility and is prone to cracking and other damage to the pole piece when used.
[0053] As multi-tab and full-tab solutions become more and more popular, coating with an insulating layer has become a necessary measure to improve the reliability of the pole piece. However, in the full-tab solution, the coating process is limited and it is impossible to coat insulating layers of different widths, which limits the ability of the insulating layer to protect the pole piece and still poses the risk of tab folding.
[0054] Based on this, the embodiments of the present application provide a pole piece, a winding core and a battery to solve the problem of poor reliability of the pole piece. The present application describes the pole piece, the winding core and the battery respectively through the following embodiments.
[0055] See also Figure 1 , Figure 1It is a schematic diagram of the structure provided by the embodiment of the present application as viewed from the cut surface of the pole piece 001. The embodiment of the present application provides a pole piece 001, which is applied to a winding core. The pole piece 001 includes a current collector 011, an active material layer 012 and a reinforcement layer 013. The current collector 011 includes a pole ear 111 and a main body 112. One side of the pole ear 111 is connected to the main body 112. The active material layer 012 is arranged on the main body 112. The reinforcement layer 013 is arranged at one end of the pole ear 111 close to the main body 112.
[0056] It can be understood that the active material layer 012 covers the main body 112. The tab 111 includes a tab main body and a tab root connecting the tab main body to the main body 112. The strengthening layer 013 is arranged at one end of the tab 111 close to the main body 112, and it can be arranged only at the tab root, or part of it can be located at the tab root and part of it can be located at the tab main body 112.
[0057] The strengthening layer 013 is used to strengthen the strength of the end of the tab 111 close to the main body 112. The strengthening layer 013 has insulating properties. The strengthening layer 013 includes but is not limited to an insulating layer and an adhesive layer.
[0058] In this embodiment, by providing a strengthening layer 013 at one end of the pole ear 111 close to the main body 112, the thickness of the pole ear root can be increased, thereby increasing the strength of the pole ear root, and further effectively preventing the pole ear from collapsing and folding when the pole piece 001 is wound, and ultimately improving the reliability of the pole piece 001. As a result, the yield rate of the winding core using the pole piece 001 can be improved, and the manufacturing cost of the winding core can be controlled.
[0059] In addition, a material with a strength greater than that of the current collector 011 may be selected as the strengthening layer 013 , so that the strengthening layer 013 can improve the strength of the base of the electrode tab with a smaller thickness.
[0060] See also Figure 2 , Figure 2 yes Figure 1 In one embodiment, the winding center is defined, and the pole piece 001 has an A surface facing the winding center and a B surface away from the winding center. Both the A surface and the B surface are provided with a strengthening layer 013 and an active material layer 012, such as Figure 4 and Figure 5 As shown, Figure 4 is a schematic structural diagram of the A surface of the pole piece 001 provided in an embodiment of the present application, Figure 5 It is a schematic structural diagram of the B side of the pole piece 001 provided in an embodiment of the present application.
[0061] In this embodiment, by providing a strengthening layer 013 on both sides of the tab 111 , both sides of the tab can be strengthened at the same time, thereby improving the symmetry of the strengthening on both sides of the tab root, thereby improving reliability.
[0062] See also Figure 2 In one embodiment, along the width direction of the pole piece 001, the strengthening layer 013 on the A side has a width dimension L1. The strengthening layer 013 on the B side has a width dimension L2. The pole tab 111 has a width dimension H1, which satisfies: 15% H1≤L1≤50% H1, 15% H1≤L2≤50% H1.
[0063] It can be understood that L1 and L2 include but are not limited to 15% H1, 20% H1, 30% H1, 40% H1, 45% H1, 50% H1. For example, when H1 is 6.5 mm, L1 and L2 include but are not limited to 0.975 mm, 1.3 mm, 1.95 mm, 2.6 mm, 2.925 mm, and 3.25 mm.
[0064] In addition, L1 may be equal to L2, or L1 and L2 may be unequal. When L1 and L2 are equal, they may be arranged in alignment on both sides of the pole ear, or they may be arranged in a staggered manner. When L1 and L2 are unequal, in the width direction of the pole piece 001, one end face of the strengthening layer 013 on the A side may be flush with one end face of the strengthening layer 013 on the B side.
[0065] In this embodiment, by making the above-mentioned limitations on L1 and L2, on the one hand, it can be avoided that L1 and L2 are too small to support the tabs, and on the other hand, it can be avoided that L1 and L2 are too large to be conducive to winding and electrical connection with the busbar.
[0066] In one embodiment, the following is satisfied: L1<L2, and further, 30%H1≤L2≤50%H1.
[0067] Illustratively, 50% L2 ≤ L1 ≤ 90% L2.
[0068] It can be understood that L1 includes but is not limited to 50% L2, 60% L2, 70% L2, 80% L2, 86% L2, 90% L2. For example, when L2 is 2.5 mm, L1 includes but is not limited to 1.25 mm, 1.5 mm, 1.75 mm, 2 mm, 2.15 mm, 2.25 mm.
[0069] Accordingly, in combination with the previous embodiment, 15% H1≤L1≤45% H1, 30% H1≤L2≤50% H1. Among them, L1 includes but is not limited to 15% H1, 20% H1, 30% H1, 40% H1, 45% H1. L2 includes but is not limited to 30% H1, 36% H1, 38% H1, 40% H1, 45% H1, 50% H1. For example, when H1 is 6.5mm, L1 includes but is not limited to 0.975mm, 1.3mm, 1.95mm, 2.6mm, 2.925mm, and L2 includes but is not limited to 1.95mm, 2.34mm, 2.47mm, 2.6mm, 2.925mm, 3.25mm.
[0070] It can be understood that since the A surface faces the winding center, it is in an extruded state when winding the pole piece 001; the B surface faces away from the winding center, and it is in a stretched state when winding the pole piece 001. Therefore, in this embodiment, the width dimension L1 of the strengthening layer 013 on the A surface is set to be smaller than the width dimension L2 of the strengthening layer 013 on the B surface, so that the connection surface area between the A surface and the strengthening layer 013 is smaller, so that when winding the pole piece 001, the obstacle of the strengthening layer 013 on the A surface to the bending of the pole piece 001 can be reduced, which is conducive to the smooth winding of the pole piece 001.
[0071] See also Figure 2 In one embodiment, along the thickness direction of the pole piece 001 , the strengthening layer 013 on the A side has a thickness dimension D1 , and the strengthening layer 013 on the B side has a thickness dimension D2 , satisfying: D1>D2 .
[0072] Illustratively, 40% D1≤D2≤80% D1.
[0073] It can be understood that D2 includes but is not limited to 40% D1, 50% D1, 60% D1, 70% D1, 75% D1, 80% D1. For example, when D1=0.05mm, D0 includes but is not limited to 0.02mm, 0.025mm, 0.03mm, 0.035mm, 0.04mm.
[0074] Since L1 is smaller than L2, the support effect of the strengthening layer 013 on the A side on the tab is weaker than the strengthening effect of the strengthening layer 013 on the B side on the tab. Based on this, in this embodiment, by setting the thickness dimension D1 of the strengthening layer 013 on the A side to be greater than the thickness dimension D2 of the strengthening layer 013 on the B side, the thickness of the strengthening layer 013 on the A side can be increased, thereby improving the strengthening effect of the strengthening layer 013 on the A side on the tab, and finally achieving stable support of the strengthening layer 013 on the A side on the base of the tab.
[0075] In one embodiment, the electrode 001 is a positive electrode, and the side of the strengthening layer 013 on the A side facing away from the active material layer 012 on the A side is coplanar with the side of the strengthening layer 013 on the B side facing away from the active material layer 012 on the B side. Figure 3 As shown, Figure 3 It is a schematic diagram of the positions of the strengthening layer 013 on the A side and the strengthening layer 013 on the B side of the pole piece 001 provided in the embodiment of the present application.
[0076] In this embodiment, through the above arrangement, the strengthening layers 013 on the A side 013 and the B side of the pole piece 001 can share a positioning reference, thereby improving the convenience of setting the strengthening layer 013 and further improving the manufacturing efficiency of the pole piece 001.
[0077] See also Figure 3 In one embodiment, in surface A, the strengthening layer 013 is spaced apart from the edge of the main body 112, and the distance between the strengthening layer 013 and the edge of the main body 112 is L4; in surface B, the strengthening layer 013 is spaced apart from the edge of the main body 112, and the distance between the strengthening layer 013 and the edge of the main body 112 is L5, satisfying: L4>L5.
[0078] In this embodiment, through the above-mentioned limitation, the distance between the reinforcement layer 013 on the A side of the pole piece 001 and the edge of the main body 112 is larger than that on the B side, so that the support of the reinforcement layer 013 on the A side for the pole ear on the A side is weaker than the support of the reinforcement layer 013 on the B side for the pole ear on the B side. As a result, when winding the pole piece 001, the pole ear can be more easily bent toward the center of the winding core to achieve directional bending of the pole ear, which can ultimately facilitate the subsequent connection of the pole ear with the busbar.
[0079] See also Figure 2 In one embodiment, along the width direction of the pole piece 001 , the strengthening layer 013 on the A surface has a width dimension L1 , satisfying: 15% L1 ≤ L4 ≤ 27% L1 .
[0080] Exemplarily, 0.25mm≤L5<L4≤1.5mm, for example, L4=0.7mm, L5=0.5mm; L4=0.5mm, L5=0.3mm; L4=0.38mm, L5=0.2mm.
[0081] In this embodiment, by limiting the distance L4 between the reinforcement layer 013 on the A side and the edge of the main body 112, on the one hand, it can avoid the distance between the reinforcement layer 013 and the edge of the main body 112 being too small, thereby avoiding the active material layer 012 and the reinforcement layer 013 under compression in the A side from interfering with each other due to deformation; on the other hand, it can avoid the distance between the reinforcement layer 013 and the edge of the main body 112 being too large, thereby failing to strengthen the root of the pole ear.
[0082] In addition, by limiting the minimum value of L4, the minimum value of the distance between the reinforcement layer 013 on the A side and the edge of the main body 112 can be limited, thereby ensuring that the pole piece has guidance when winding, thereby improving the smoothness of winding.
[0083] See also Figure 2 In one embodiment, along the thickness direction of the pole piece 001, the pole piece 001 has a thickness dimension D4 at the active material layer 012. The pole piece 001 has a thickness dimension D0 at the strengthening layer 013, satisfying: 50% D4≤D0≤90% D4.
[0084] It can be understood that in the art, along the thickness direction of the pole piece 001, the distance between the surface of the active material layer 012 on one side of the current collector 011 and the surface of the active material layer 012 on the other side of the current collector 011 is the thickness dimension D4 of the pole piece 001 at the active material layer 012. In addition, the distance between the surface of the reinforcement layer 013 on one side of the current collector 011 and the surface of the reinforcement layer 013 on the other side of the current collector 011 is the thickness dimension D0 of the pole piece 001 at the reinforcement layer 013.
[0085] Wherein, D0 includes but is not limited to 50% D4, 60% D4, 70% D4, 80% D4, 90% D4. For example, when D4=0.124mm, D0 includes but is not limited to 0.062mm, 0.08mm, 0.09mm, 0.10mm, 0.116mm.
[0086] In one embodiment, the reinforcement layer 013 includes a first adhesive layer 131 disposed on the tab 111. Specifically, the first adhesive layer 131 is a thermosetting adhesive or a UV curing adhesive or a mixture of a UV curing adhesive and an insulating filler.
[0087] It can be understood that the thermosetting adhesive is a thermosetting resin, and the thermosetting resin can be at least one of phenolic resin, urea-formaldehyde resin, melamine-formaldehyde resin, epoxy resin, silicone resin, polyurethane, and polyimide. The UV curable adhesive is a UV curable resin. The UV curable resin is at least one of epoxy acrylate, polyacrylic acid, polyester acrylate, acrylate containing olefin functional groups, and silicone / fluorine light curing resin. Thermosetting adhesives or UV curable adhesives usually have a faster curing time, so that the strengthening layer 013 can be quickly cured and strongly bonded to the tab, thereby saving the waiting time for the glue to cure, thereby improving production efficiency.
[0088] In this embodiment, by using the above-mentioned adhesive, on the one hand, the tab of the pole piece 001 can be pre-folded during winding, and the reinforcing layer 013 can be cured, thereby improving the supporting effect of the reinforcing layer 013 on the tab, and then effectively preventing the tab from collapsing and folding, thereby improving the yield rate of the winding assembly and controlling the manufacturing cost of the winding assembly; on the other hand, the first adhesive layer 131 can have a faster curing time, so that the first adhesive layer 131 can be quickly cured and strongly bonded to the tab. In this way, not only the connection process between the curing layer and the tab is more convenient, but also the time required for curing the first adhesive layer 131 can be saved, and the production efficiency can be improved.
[0089] See also Figure 6 , Figure 6 013 is a schematic diagram of the structure of the strengthening layer 013 provided in an embodiment of the present application. In one embodiment, the strengthening layer 013 further includes an expansion layer 132 , and the expansion layer 132 is disposed on a side of the first adhesive layer 131 away from the tab 111 .
[0090] It can be understood that the expansion layer 132 is an expansion tape.
[0091] In this embodiment, when the battery cell is assembled and injected, the expansion layer 132 expands to fill the gap at the edge between the positive electrode sheet 002 and the negative electrode sheet 004. In this way, the positive electrode sheet 002 and the negative electrode sheet 004 can be insulated and isolated, and the edge of the tab and the diaphragm 003 can be pressed tightly to form a whole, thereby increasing the vibration resistance of the tab to reduce the shaking amplitude of the tab during impact, thereby effectively reducing the possibility of internal short circuit caused by external impact, and ultimately improving the safety and reliability of the battery.
[0092] See also Figure 7 , Figure 7 1 is a schematic diagram of the structure of another strengthening layer 013 provided in an embodiment of the present application. In one embodiment, along the direction away from the pole ear, the strengthening layer 013 includes a first adhesive layer 131, an expansion layer 132, a second adhesive layer 134 and a PI (Polyimide) layer 135 arranged in sequence. The PI layer 135 is arranged on the side of the expansion layer 132 away from the first adhesive layer 131 through the second adhesive layer 134. The second adhesive layer 134 includes but is not limited to UV curable resin and acrylic glue. Specifically, the second adhesive layer 134 is a thermosetting adhesive or a UV curable adhesive or a mixture of a UV curable adhesive and an insulating filler.
[0093] In this embodiment, through the above configuration, on the one hand, the insulation of the strengthening layer 013 can be improved, thereby improving the reliability; on the other hand, the strength of the strengthening layer 013 can be improved to prevent the strengthening layer 013 from being scratched by the burrs at the tab.
[0094] In one embodiment, taking a 4680 cylindrical battery cell and the electrode 001 as the positive electrode as an example, the dimensions and values mentioned above are as follows:
[0095]
[0096] Table 1. Dimensions and values
[0097] In Table 1, the width L3 of the cut pole lug on the A side = the width H1 of the pole lug 111 - the width L1 of the strengthening layer 013 on the A side - the distance L4 between the strengthening layer 013 on the A side and the edge of the main body 112; the width L3 of the cut pole lug on the B side = the width H1 of the pole lug 111 - the width L2 of the strengthening layer 013 on the B side - the distance L5 between the strengthening layer 013 on the B side and the edge of the main body 112.
[0098] In addition, the width of the cut tab in Table 1 refers to the cutting size of the tab formed by cutting the blank area of the current collector.
[0099] Correspondingly, an embodiment of the present application further provides a winding core, comprising a positive electrode sheet 002, a separator 003 and a negative electrode sheet 004 that are wound together, wherein the positive electrode sheet 002 is the aforementioned electrode sheet 001, or the positive electrode sheet 002 and the negative electrode sheet 004 are both the aforementioned electrode sheet 001.
[0100] It can be understood that, based on the battery design, the negative electrode sheet 004 should completely wrap the positive electrode sheet 002. In order to prevent the tab of the positive electrode sheet 002 from bending, at least the structure of the positive electrode sheet 002 should be the structure of the aforementioned electrode sheet 001.
[0101] In this embodiment, by adopting the aforementioned electrode sheet 001 as the positive electrode sheet 002 of the winding core, the thickness of the root of the electrode ear can be increased, thereby increasing the strength of the root of the electrode ear. Furthermore, when the positive electrode sheet 002 is wound, the electrode ear of the positive electrode sheet 002 can be prevented from bending at the root of the electrode ear to avoid folding of the electrode ear, thereby ultimately improving the yield rate of the winding core and controlling the manufacturing cost of the winding core.
[0102] See also Figure 8 and Fig. 9 , Figure 8 is a schematic diagram of the structure of the winding core viewed from the cut surface of the pole piece 001 provided in an embodiment of the present application, Fig. 9 yes Figure 8Enlarged view of C in the middle. In one embodiment, the winding core has a winding center, and the surface of the positive electrode sheet 002 facing the winding center is surface A. Along the width direction of the positive electrode sheet 002, the strengthening layer 013 on surface A has a first end face of the active material layer 012 facing surface A and a second end face of the active material layer 012 away from surface A. With the plane parallel to the winding center as the projection plane and the direction perpendicular to the projection plane as the projection direction, in the projection plane, the orthographic projection of the edge of the negative electrode sheet 004 is located between the orthographic projection of the first end face and the orthographic projection of the second end face.
[0103] Fig. 9 In the embodiment, the edge of the negative electrode sheet 004 exceeds the edge of the main body 112 of the positive electrode sheet 002 by a dimension H3, and the distance between the first end surface and the edge of the main body 112 of the positive electrode sheet 002 is L4. Correspondingly, L4<H3.
[0104] Exemplarily, L4 is 0.7 mm and H3 is 1 mm.
[0105] In this embodiment, through the above-mentioned limitations, the strengthening layer 013 can not only protect the ear of the positive electrode sheet 002 from folding, but also prevent the edge of the negative electrode sheet 004 from being stuck in the gap between the first end face and the edge of the main body 112 of the positive electrode sheet 002, thereby preventing the edge of the negative electrode sheet from being stuck in the gap and causing a short circuit, thereby improving the reliability of the winding core.
[0106] See also Fig. 9 In one embodiment, in the projection plane, the orthographic projection of the edge of the diaphragm 003 is located between the orthographic projection of the second end surface and the orthographic projection of the edge of the main body 112 of the negative electrode sheet 004 .
[0107] It can be understood that the tabs of the positive electrode sheet 002 and the tabs of the negative electrode sheet 004 are respectively located at the two ends of the winding center, and the edge of the negative electrode sheet 004 close to the tabs of the positive electrode sheet 002 is the edge of the body of the negative electrode sheet 004. Therefore, the distance between the second end surface and the edge of the body 112 of the negative electrode sheet 004 is arranged opposite to the edge of the separator 003, so that the insulation isolation between the negative electrode sheet 004 and the positive electrode sheet 002 can be achieved.
[0108] The surface of the positive electrode sheet 002 facing away from the winding center is the B surface. In the B surface, Fig. 9As shown, along the width direction of the positive electrode sheet 002, the distance between the second end face and the edge of the main body 112 of the positive electrode sheet 002 = the width dimension L2 of the strengthening layer 013 on the B surface + the distance L5 between the strengthening layer 013 on the B surface and the edge of the main body 112 on the B surface. Along the width direction of the positive electrode sheet 002, the edge of the diaphragm 003 exceeds the edge of the main body 112 of the positive electrode sheet 002 by a dimension H2. The orthographic projection of the edge of the diaphragm 003 is located between the orthographic projection of the second end face and the orthographic projection of the edge of the main body 112 of the negative electrode sheet 004, and correspondingly, L5<H2<L5+L2.
[0109] Exemplarily, L5 is 0.3 mm, L2 is 2.5 mm, and correspondingly, 0.3 mm<H2<2.8 mm, for example, H2=2 mm.
[0110] In this embodiment, through the above-mentioned limitation, the edge of the diaphragm 003 is arranged opposite to the reinforcement layer 013, so that in the wound core, the gaps between the pole ears of the positive electrode sheet 002, the edge of the diaphragm 003 and the edge of the negative electrode sheet 004 can be filled with the reinforcement layer 013, so that the edges of these three components are integrated, thereby improving the structural stability of the core.
[0111] In addition, when the strengthening layer 013 includes an expansion layer, the expansion layer can expand when the battery cell is assembled and injected, so that the gap between the tab of the positive electrode sheet 002 and the edge of the negative electrode sheet 004 can be filled, so as to squeeze the edge of the diaphragm 002, the edge of the negative electrode sheet 004, the tab of the positive electrode sheet 002 and the relative position of the expansion layer 132 into one. In this way, the positive electrode sheet 002 and the negative electrode sheet 004 can be insulated and isolated, and the tab of the positive electrode sheet 002, the edge of the negative electrode sheet 004 and the edge of the diaphragm 003 can be pressed together to form a whole, so that the vibration resistance at the tab is increased to reduce the shaking amplitude between them during impact, and then the possibility of internal short circuit caused by external impact can be effectively prevented, and finally the safety and reliability of the battery can be improved.
[0112] Accordingly, an embodiment of the present application further provides a battery, which includes the aforementioned winding core.
[0113] It can be understood that the battery further includes a battery box and a cell shell disposed in the battery box. The winding core is disposed in the cell shell, and electrolyte is injected into the cell shell.
[0114] In this embodiment, by adopting the aforementioned winding core, the yield rate of the battery is improved, thereby controlling the manufacturing cost of the battery.
[0115] Correspondingly, an embodiment of the present application further provides a winding core preparation method, which comprises: obtaining the aforementioned pole piece 001 for winding, or obtaining the aforementioned winding core.
[0116] In this embodiment, by adopting the aforementioned pole piece 001 or winding core, the pole ear 111 of the pole piece 001 can be prevented from collapsing or folding during winding, thereby improving the yield of the winding assembly and controlling the manufacturing cost of the winding assembly.
[0117] In one embodiment, the reinforcement layer 013 includes a first adhesive layer 131 disposed on the pole piece, and the method includes: disposing the first adhesive layer 131 on one end of the pole ear 111 of the pole piece 001 close to the main body 112; when winding, pre-folding the pole ear 111 of the pole piece 001, and curing the first adhesive layer 131 on the pre-folded pole ear 111 of the pole piece 001.
[0118] Exemplarily, the first adhesive layer 131 is a thermosetting adhesive or a UV curing adhesive or a mixture of a UV curing adhesive and an insulating filler, wherein the insulating filler may be ceramic powder.
[0119] In this way, the tab of the positive electrode sheet 002 can be bent and shaped in a preset direction, thereby improving the strength of the tab and preventing the tab of the positive electrode sheet 002 from collapsing or folding.
[0120] Among them, when the first adhesive layer 131 is a thermosetting adhesive, the reinforcing layer 013 is cured by heating the reinforcing layer 013; when the first adhesive layer 131 is a UV curing adhesive or a mixture of a UV curing adhesive and an insulating filler, the reinforcing layer 013 is cured by irradiating it with external rays through a UV curing device.
[0121] In one embodiment, before pre-folding the tab 111 of the electrode sheet 001 , the method further includes: baking the strengthening layer 013 .
[0122] In this embodiment, the strengthening layer 013 is baked to be initially solidified, so as to control the adhesion of the strengthening layer 013 and prevent it from being randomly bonded to other components, thereby facilitating the smooth preparation of the winding core.
[0123] In one embodiment, the reinforcement layer 013 further includes an expansion layer 132 . After the first adhesive layer 131 is disposed on one end of the pole ear 111 of the pole piece 001 close to the main body 112 , the method further includes: disposing the expansion layer 132 on a side of the first adhesive layer 131 away from the pole ear 111 .
[0124] In this embodiment, by providing the expansion layer 132, when the battery cell is assembled and injected, the expansion layer expands, so that the gap between the tab of the positive electrode sheet 002 and the edge of the negative electrode sheet 004 can be filled, so that the edge of the diaphragm 002, the edge of the negative electrode sheet 004, and the tab of the positive electrode sheet 002 relative to the expansion layer 132 are squeezed into one. In this way, the positive electrode sheet 002 and the negative electrode sheet 004 can be insulated and isolated, and the tab of the positive electrode sheet 002, the edge of the negative electrode sheet 004 and the edge of the diaphragm 003 can be pressed together to form a whole, so that the vibration resistance at the tab is increased, so as to reduce the shaking amplitude between them during impact, and then the possibility of internal short circuit caused by external impact can be effectively prevented, and finally the safety and reliability of the battery can be improved.
[0125] In one embodiment, the strengthening layer 013 also includes a second viscose layer 134 and a PI layer 135. After the expansion layer 134 is disposed on the side of the first viscose layer 131 away from the tab 111, the method further includes: disposing the second viscose layer 134 on the side of the expansion layer 132 away from the first viscose layer 131; and disposing the PI layer 135 on the side of the second viscose layer 134 away from the expansion layer 132.
[0126] In this embodiment, through the above configuration, on the one hand, the insulation of the strengthening layer 013 can be improved, thereby improving the reliability; on the other hand, the strength of the strengthening layer 013 can be improved to prevent the strengthening layer 013 from being scratched by the burrs at the tab.
[0127] In one embodiment, the method further includes: preparing and baking a strengthening layer 013; setting the baked strengthening layer 013 at one end of the pole ear 111 of the pole piece 001 close to the main body 112; when winding, pre-folding the pole ear 111 of the pole piece 001, and curing the strengthening layer 013 on the pre-folded pole ear 111.
[0128] The strengthening layer 013 includes a first adhesive layer 131 , an expansion layer 132 , a second adhesive layer 134 and a PI layer 135 which are stacked in sequence.
[0129] In this embodiment, the strengthening layer 013 is prepared and then disposed on the pole ear 111 of the pole piece 001 , so that the strengthening layer 013 and the active material can be separately manufactured and coated on the current collector 011 , thereby improving the manufacturing efficiency of the pole piece 011 .
[0130] Based on the above embodiments, the preparation of the winding core is described in detail as follows.
[0131] 1. When the strengthening layer 013 includes the first adhesive layer 131, and the first adhesive layer 131 is a mixture of a UV curable adhesive and an insulating filler, as Fig.10 As shown, Fig.10This is a schematic diagram of the process of preparing a core provided in an embodiment of the present application. Figure 1 , the preparation method of the core comprises:
[0132] S100, preparing glue: mixing a UV curable adhesive and an insulating filler to prepare glue;
[0133] S200, preparing the positive electrode sheet 002: obtaining the electrode body, applying glue to the base of the electrode ear of the electrode body, and drying the glue to form a strengthening layer 013, that is, a first adhesive layer 131; it can be understood that when the strengthening layer 013 only has the first adhesive layer 131, drying the strengthening layer 013 is equivalent to drying the first adhesive layer 131;
[0134] S300, forming a winding core: winding the positive electrode sheet 002, and during the winding, pre-folding the tab of the positive electrode sheet 002, and curing the reinforcing layer 013 on the tab of the pre-folded positive electrode sheet 002 by a UV curing device.
[0135] 2. When the strengthening layer 013 includes the first adhesive layer 131 and the expansion layer 132, and the first adhesive layer 131 is a mixture of a UV curable adhesive and an insulating filler, Fig.11 As shown, Fig.11 This is a schematic diagram of the process of preparing a core provided in an embodiment of the present application. Figure 2 , the preparation method of the core comprises:
[0136] S100, preparing glue: mixing a UV curable adhesive and an insulating filler to prepare glue;
[0137] S200, preparing the positive electrode sheet 002: obtaining the electrode body, applying glue to the base of the electrode ear of the electrode body, and drying the glue to form a first adhesive layer 131;
[0138] S300, disposing the expansion layer 132 on the first adhesive layer 131 to form a strengthening layer 013;
[0139] S400, forming a winding core: winding the positive electrode sheet 002, and during the winding, pre-folding the tab of the positive electrode sheet 002, and curing the reinforcing layer 013 on the tab of the pre-folded positive electrode sheet 002 by a UV curing device.
[0140] 3. When the strengthening layer 013 includes the first adhesive layer 131, the expansion layer 132, the second adhesive layer 134 and the PI layer 135, and the first adhesive layer 131 is a mixture of a UV curable adhesive and an insulating filler, as Fig.12 As shown, Fig.12 This is a schematic diagram of the process of preparing a core provided in an embodiment of the present application. Figure 3 , the preparation method of the core comprises:
[0141] S100, preparing an adhesive tape: coating a mixture of a UV curable adhesive and an insulating filler on both surfaces of the expansion layer 132 to form a first adhesive layer 131 and a second adhesive layer 134 respectively; then arranging a PI layer 135 on a side of the second adhesive layer 134 away from the expansion layer 132; and then baking the second adhesive layer 134 to obtain a strengthening layer 013;
[0142] S200, preparing the positive electrode sheet 002: obtaining the electrode sheet body, and setting the strengthening layer 013 at the root of the electrode ear of the electrode sheet body;
[0143] S300, forming a winding core: winding the positive electrode sheet 002, and during the winding, pre-folding the tab of the positive electrode sheet 002, and curing the reinforcing layer 013 on the tab of the pre-folded positive electrode sheet 002 by a UV curing device.
[0144] The embodiments of the present application are introduced in detail above. Specific examples are used in this article to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method and core idea of the present application. At the same time, for technical personnel in this field, according to the idea of the present application, there will be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.
Claims
1. A pole piece, characterized in that: The pole piece comprises: A current collector, comprising a tab and a main body, wherein one side of the tab is connected to the main body; An active material layer, disposed on the main body; The strengthening layer is arranged at one end of the tab close to the main body.
2. The pole piece according to claim 1, characterized in that: A winding center is defined, and the pole piece has an A surface facing the winding center and a B surface away from the winding center; the A surface and the B surface are both provided with the strengthening layer and the active material layer.
3. The pole piece according to claim 2, characterized in that: Along the width direction of the pole piece, the strengthening layer of the A surface has a width dimension L1, the strengthening layer of the B surface has a width dimension L2, and the pole ear has a width dimension H1, satisfying: 15% H1≤L1≤50% H1, 15% H1≤L2≤50% H1.
4. The pole piece according to claim 3, characterized in that: L1<L2.
5. The pole piece according to claim 4, characterized in that: 50%L2≤L1≤90%L2.
6. The pole piece according to claim 5, characterized in that: 15%H1≤L1≤45%H1.
7. The pole piece according to claim 4, characterized in that: Along the thickness direction of the pole piece, the strengthening layer on the A surface has a thickness dimension D1, and the strengthening layer on the B surface has a thickness dimension D2, satisfying: D1>D2.
8. The pole piece according to claim 4, characterized in that: The electrode sheet is a positive electrode sheet, and 30% H1≤L2≤50% H1.
9. The pole piece according to claim 4, characterized in that: A side of the reinforcement layer on the A surface facing away from the active material layer on the A surface is coplanar with a side of the reinforcement layer on the B surface facing away from the active material layer on the B surface.
10. The pole piece according to claim 2, characterized in that: In the A surface, the strengthening layer is spaced apart from the edge of the main body, and the distance between the strengthening layer and the edge of the main body is L4; in the B surface, the strengthening layer is spaced apart from the edge of the main body, and the distance between the strengthening layer and the edge of the main body is L5, satisfying: L4>L5.
11. The pole piece according to claim 10, characterized in that: Along the width direction of the pole piece, the strengthening layer of the A surface has a width dimension L1, which satisfies: 15% L1≤L4≤27% L1.
12. The pole piece according to claim 11, characterized in that: 0.25mm≤L5<L4≤1.5mm.
13. The pole piece according to claim 1, characterized in that: Along the thickness direction of the pole piece, the pole piece has a thickness dimension D4 at the active material layer, and the pole piece has a thickness dimension D0 at the reinforcement layer, satisfying: 50% D4≤D0≤90% D4.
14. The pole piece according to any one of claims 1 to 13, characterized in that: The strengthening layer includes a first adhesive layer disposed on the tab.
15. The pole piece according to claim 14, characterized in that: The strengthening layer further includes an expansion layer, and the expansion layer is arranged on a side of the first adhesive layer away from the pole ear.
16. The pole piece according to claim 15, characterized in that: The strengthening layer further includes a second adhesive layer and a PI layer. The PI layer is arranged on a side of the expansion layer away from the first adhesive layer through the second adhesive layer.
17. The pole piece according to claim 16, characterized in that: The first adhesive layer and / or the second adhesive layer is a thermosetting adhesive or a UV curing adhesive or a mixture of a UV curing adhesive and an insulating filler.
18. A winding core, characterized in that: It comprises a positive electrode sheet, a separator and a negative electrode sheet which are wound together, wherein the positive electrode sheet is the electrode sheet according to any one of claims 1 to 17, or the positive electrode sheet and the negative electrode sheet are both the electrode sheets according to any one of claims 1 to 17.
19. The winding core according to claim 18, characterized in that: A winding center is defined, the surface of the positive electrode sheet facing the winding center is surface A, and along the width direction of the positive electrode sheet, the strengthening layer on surface A has a first end surface of the active material layer facing the surface A and a second end surface of the active material layer away from the surface A; A plane parallel to the winding center is taken as a projection plane, and a direction perpendicular to the projection plane is taken as a projection direction. In the projection plane, the orthographic projection of the main edge of the negative electrode sheet is located between the orthographic projection of the first end face and the orthographic projection of the second end face.
20. The winding core according to claim 19, characterized in that In the projection plane, the orthographic projection of the edge of the diaphragm is located between the orthographic projection of the second end surface and the orthographic projection of the main body edge of the negative electrode sheet.
21. A battery, characterized in that: Comprising the winding core according to any one of claims 18 to 20.
Citation Information
Cited By
Pole piece, roll core, battery and roll core preparation method
CN117976802A
Electrode sheet, jelly roll, battery and preparation method for jelly roll
EP4618218A1
Electrode sheet, jelly roll, battery and preparation method for jelly roll