Cathode-supported large-area solid oxide electrolytic cell with reticular stepped pore structure

By adopting a mesh step pore structure in the cathode support layer of a large area high-temperature solid oxide electrolytic cell, the problems of water vapor transmission resistance and battery strength are solved, and the power density and steam conversion rate of the electrolytic cell are improved, and the battery is also improved. Provides better structural strength.

CN222008079UActive Publication Date: 2024-11-15QINGDAO PROTON POWER TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202420564145.3
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2024-03-22
Publication Date
2024-11-15
Estimated Expiration
2034-03-22

AI Technical Summary

Technical Problem

Large-area high-temperature solid oxide electrolytic cells have great resistance during water vapor transmission, resulting in reduced electrochemical performance and increased porosity to alleviate this problem, which will lead to a decrease in battery strength and make it difficult to be suitable for large-area preparation.

Method used

The cathode support layer adopts a mesh step pore structure. By gradually increasing the pore diameter and porosity of the ball holes in the inner and outer layers of the cathode support layer, a mesh gas transmission channel between the ball holes and the communication holes is formed, reducing the water vapor and gas transmission resistance. , while improving the structural strength of the battery.

Benefits of technology

It effectively improves the power density and steam conversion rate of the electrolytic cell, and provides better structural strength. It is suitable for the preparation of large-area electrolytic cells, reducing mass transfer resistance and improving electrolytic performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN222008079U_ABST
    Figure CN222008079U_ABST
Patent Text Reader

Abstract

The utility model discloses a cathode-supported large-area solid oxide electrolytic tank with a net-shaped stepped pore structure. The cathode-supported large-area solid oxide electrolytic tank comprises an anode (10), a barrier layer (20), an electrolyte layer (30), an active cathode (40) and a cathode supporting layer which are sequentially stacked, a ball hole (62) and a communicating hole (61) are formed in the cathode supporting layer, and the cathode supporting layer is divided into a cathode supporting inner layer (51), a cathode supporting middle layer (52) and a cathode supporting outer layer (53); the aperture of the ball holes (62) is larger than that of the communicating holes (61), the aperture of the ball holes (62) is gradually increased in the cathode supporting inner layer (51), the cathode supporting middle layer (52) and the cathode supporting outer layer (53), and the ball holes and the communicating holes jointly form a net-shaped gas transmission channel. The water vapor transmission resistance is small, the improvement of the power density and the steam conversion rate of the electrolytic tank is facilitated, and the cathode supporting layer can provide structural strength for the electrolytic tank while guaranteeing gas transmission.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The utility model relates to the technical field of solid oxide electrolytic cells, in particular to a large-area solid oxide electrolytic cell supported by a cathode with a mesh-like stepped pore structure. Background Art

[0002] High-temperature solid oxide fuel cells (SOECs) produce hydrogen and oxygen by electrolyzing water vapor under applied voltage and high temperature. They can convert electrical energy and thermal energy into chemical energy, providing a new technology for the efficient use of hydrogen energy. SOECs have the advantages of high power generation efficiency, strong fuel adaptability, and high-temperature waste heat recovery. SOECs have broad application prospects in large-scale power generation, distributed power generation and combined heat and power, transportation, peak load storage, and other fields.

[0003] The high efficiency of SOEC is mainly due to two reasons: thermodynamics and kinetics. In terms of thermodynamics, high-temperature electrolysis can reduce the energy consumption of the electrolysis process and can utilize waste heat from power stations or other industrial processes. In terms of kinetics, high-temperature electrolysis can reduce the internal resistance of the battery and increase the current density, thereby improving the electrolysis efficiency. In addition, SOEC has low energy consumption and can use cheap nickel electrodes (Ni-YSZ).

[0004] High-temperature solid oxide electrolyzer (SOEC) is the reverse operation of SOFC fuel cell, but due to the change of working environment and mode, SOEC has special requirements for materials and structures compared with SOFC. Compared with traditional SOFC which uses hydrogen as the main raw material, SOEC uses water vapor as the main raw material. The volume of water molecules is much larger than that of hydrogen, which will produce greater resistance during mass transfer. In addition, in SOEC with fuel pole support structure design, since the fuel pole is relatively thick, its porous characteristics have a huge impact on the mass transfer of water molecules in SOEC, which will directly lead to an increase in the concentration polarization of the electrolyzer and reduce its electrochemical performance. Directly increasing the porosity of the fuel pole will also lead to a decrease in the strength of the battery.

[0005] Some methods can alleviate concentration polarization by changing the battery assembly method and adjusting the gas channel, and are suitable for the preparation of small-sized electrolytic cells (less than 50×50 mm) in the field. However, the change in process increases the cost, and the decrease in strength due to the increase in porosity makes the preparation of large-area electrolytic cells, which are already difficult to prepare, further increased. Summary of the invention

[0006] The utility model aims to provide a large-area solid oxide electrolytic cell with a cathode support having a mesh-like stepped pore structure, which has a small resistance to water vapor transmission, is beneficial to improving the power density and steam conversion rate of the electrolytic cell, and the cathode support layer can provide structural strength for the electrolytic cell while ensuring gas transmission.

[0007] To achieve the above purpose, the present invention provides a large-area solid oxide electrolytic cell with a cathode supporting a mesh-like stepped pore structure, comprising:

[0008] An anode, a barrier layer, an electrolyte layer, an active cathode, and a cathode support layer stacked in sequence;

[0009] The cathode support layer is provided with spherical holes and connecting holes, and is divided into a cathode support inner layer, a cathode support middle layer, and a cathode support outer layer;

[0010] The diameter of the spherical hole is larger than the diameter of the connecting hole, and gradually increases in the cathode support inner layer, the cathode support middle layer, and the cathode support outer layer.

[0011] Furthermore, the distances between adjacent spherical holes are connected by connecting holes, and a mesh-like gas transmission channel is formed between the spherical holes and the connecting holes.

[0012] Furthermore, the cathode support inner layer has a thickness of 100-300 μm, the cathode support middle layer has a thickness of 100-300 μm, and the cathode support outer layer has a thickness of 100-300 μm.

[0013] Furthermore, the cathode support inner layer has a porosity of 10%-20%, wherein the spherical pores have a pore size of 1-10 μm;

[0014] The porosity of the cathode support middle layer is 20%-30%, and the spherical pore diameter is 1-10 μm;

[0015] The porosity of the cathode support outer layer is 30%-40%, and the diameter of the spherical pores is 20-30 μm.

[0016] Further, the cathode support layer is composed of one or more materials selected from NiO and yttria-stabilized zirconia, scandia-stabilized zirconia, and gadolinium-doped cerium oxide;

[0017] And the content of NiO is 45%-60%.

[0018] Compared with the prior art, the cathode support large-area solid oxide electrolytic cell with mesh-like stepped pore structure divides the cathode support layer into a cathode support inner layer, a cathode support middle layer, and a cathode support outer layer, and the spherical pores gradually increase in the corresponding layers. The cathode support structure with such stepped pores has a small resistance to water vapor transmission, which is beneficial to the improvement of the power density and steam conversion rate of the electrolytic cell. Moreover, the cathode support layer with such spherical pore structure can provide better structural strength for the electrolytic cell while ensuring gas transmission. In addition, a mesh-like gas transmission channel is formed between the spherical pores and the connecting pores, which is beneficial to the shortest path transmission of gas and can reduce the mass transfer resistance.

[0019] Since the cathode support middle layer and the cathode support outer layer adopt large pore size and high porosity, it is helpful for the mass transfer process of water molecules; the cathode support inner layer adopts a relatively small pore size and low porosity structure, which is beneficial to improving the structural strength of the electrolytic cell and allowing water molecules to be evenly dispersed to reach the surface of the cathode active layer, which helps to increase the reaction sites, thereby helping to improve the electrolysis performance and steam conversion rate; the pore size and porosity of the cathode support layer gradually decrease from the outside to the inside, so that the mass transfer resistance of water molecules gradually increases and the dispersion is gradually uniform. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 It is an overall schematic diagram of the utility model;

[0021] Figure 2 It is the actual SEM picture of the utility model;

[0022] Figure 3 It is the IV curve diagram of the electrolytic cell operation;

[0023] In the figure: 10, anode, 20, barrier layer, 30, electrolyte layer, 40, active cathode;

[0024] 51, cathode support inner layer, 52, cathode support middle layer, 53, cathode support outer layer;

[0025] 61. Connecting hole, 62. Ball hole. DETAILED DESCRIPTION

[0026] The following will be combined with the drawings in the embodiments of the utility model to clearly and completely describe the technical solutions in the embodiments of the utility model. Obviously, the described embodiments are only part of the embodiments of the utility model, not all of the embodiments. Based on the embodiments in the utility model, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the utility model.

[0027] like Figure 1 , Figure 2 , Figure 3 As shown, the present mesh-like stepped pore structure cathode supports a large-area solid oxide electrolytic cell, comprising:

[0028] An anode 10, a barrier layer 20, an electrolyte layer 30, an active cathode 40, and a cathode support layer stacked in sequence;

[0029] The cathode support layer is provided with a ball hole 62 and a connecting hole 61, and is divided into a cathode support inner layer 51, a cathode support middle layer 52, and a cathode support outer layer 53;

[0030] The diameter of the spherical hole 62 is larger than the diameter of the connecting hole 61, and gradually increases in the cathode support inner layer 51, the cathode support middle layer 52, and the cathode support outer layer 53;

[0031] Specifically, the anode 10 is made of anode liquid slurry, which can be prepared by grinding and mixing anode ceramic powder with an organic solvent, a dispersant, a binder, and a plasticizer. The anode 10 is located at the positive electrode of the electrolytic cell and provides electrons to oxidize the anions in the electrolyte layer 30, thereby promoting the electrolysis process.

[0032] The barrier layer 20 is made of a barrier layer liquid slurry, which can be prepared by grinding and mixing a barrier layer ceramic powder with an organic solvent, a dispersant, a binder, and a plasticizer. The barrier layer 20 is located between the anode 10 and the electrolyte layer 30, and can prevent the anions and cations in the electrolyte layer 30 from directly mixing to maintain the stability of the electrolyte, and prevent the short circuit between the anode 10 and the active cathode 40.

[0033] The electrolyte layer 30 is made of electrolyte liquid slurry, which can be prepared by grinding and mixing electrolyte ceramic powder with organic solvent, dispersant, binder and plasticizer. The electrolyte is a conductive medium in the electrolytic cell, which can transfer ions, maintain the electrolysis process, and transfer charges between the anode 10 and the active cathode 40.

[0034] The active cathode 40 is a cathode liquid slurry, which can be prepared by grinding and mixing the active cathode ceramic powder with an organic solvent, a dispersant, a binder, and a plasticizer. The active cathode 40 is located at the negative electrode of the electrolytic cell and can provide electrons to promote the reduction reaction of the electrolyte cations, thereby completing the electrolysis process.

[0035] The cathode support layer adopts cathode support liquid slurry, and cathode support ceramic powder can be fully ground and mixed with organic solvent, dispersant, binder, plasticizer and pore-forming agent to prepare; the cathode support layer is located on the outside of the active cathode 40, and its function is to support and fix the active cathode 40, as well as mass transfer, which not only improves the structural strength of the electrolytic cell, but also facilitates the smooth discharge of gas; the cathode support layer is evenly arranged with spherical holes 62 and connecting holes 61, and the aperture of the spherical holes 62 gradually increases with the corresponding inner layer, middle layer and outer layer, and the spherical holes 62 and connecting holes 61 can make the gas generated in the electrolysis process be discharged smoothly, and compared with other methods using fiber holes, it can have better structural strength and is suitable for the production and preparation of large-area electrolytic cells;

[0036] In the present large-area solid oxide electrolytic cell with a cathode support having a mesh-like stepped pore structure, the cathode support layer is divided into a cathode support inner layer 51, a cathode support middle layer 52, and a cathode support outer layer 53, and the spherical holes 62 gradually increase in the corresponding layers. This cathode support structure with a gradient gap has a small resistance to water vapor transmission, which is beneficial to the improvement of the power density and steam conversion rate of the electrolytic cell. In addition, the cathode support layer can provide structural strength for the electrolytic cell while ensuring gas transmission.

[0037] Furthermore, the distance between adjacent spherical holes 62 is connected by the connecting holes 61, and a mesh-like gas transmission channel is formed between the spherical holes 62 and the connecting holes 61;

[0038] Specifically, a mesh gas transmission channel is formed between the ball hole 62 and the connecting hole 61, which is conducive to the shortest path transmission of gas. That is, during the electrolysis process of the electrolytic cell, the gas will be transmitted along the shortest path of the mesh channel under the action of gas and pressure, and the mass transfer resistance can be reduced. In some technical solutions, fiber holes are used, which are perpendicular to the gas transmission direction, resulting in an increase in the gas transmission path.

[0039] Further, the cathode support inner layer 51 has a thickness of 100-300 μm, the cathode support middle layer 52 has a thickness of 100-300 μm, and the cathode support outer layer 53 has a thickness of 100-300 μm;

[0040] Furthermore, the porosity of the cathode support inner layer 51 is 10%-20%, and the pore diameter of the spherical pores 62 is 1-10 μm;

[0041] The porosity of the cathode support middle layer 52 is 20%-30%, and the pore diameter of the spherical pores 62 is 1-10 μm;

[0042] The porosity of the cathode support outer layer 53 is 30%-40%, and the diameter of the spherical pores 62 therein is 20-30 μm.

[0043] Specifically, compared with the cathode support inner layer 51, the cathode support middle layer 52 and the cathode support outer layer 53 use large pores and high porosity to facilitate the mass transfer process of water molecules;

[0044] The cathode support inner layer 51 adopts a relatively small pore size and low porosity structure, which is beneficial to improving the structural strength of the electrolytic cell and allowing water molecules to be dispersed evenly to reach the surface of the cathode active layer, which helps to increase the reaction sites, thereby helping to improve the electrolysis performance and steam conversion rate; the pore size and porosity of the cathode support layer gradually decrease from the outside to the inside, so that the mass transfer resistance of water molecules is gradually increased and the dispersion is gradually uniform;

[0045] In addition, when preparing a large-area electrolytic cell, the area size of the electrolytic cell is 100×100mm-200×200mm. The cathode support layer is applied to the preparation method of tape casting-co-firing-screen printing-re-sintering to obtain a large-area electrolytic cell with high yield and high performance.

[0046] Further, the cathode support layer is composed of NiO and one or more materials selected from yttria-stabilized zirconia, scandia-stabilized zirconia, and gadolinium-doped cerium oxide;

[0047] And the content of NiO is 45%-60%.

[0048] Example

[0049] The present invention discloses a method for preparing a large-area solid oxide electrolytic cell with a cathode supported by a mesh-like stepped pore structure, which specifically comprises the following steps:

[0050] S1, preparing anode liquid slurry by fully grinding and mixing anode ceramic powder with an organic solvent, a dispersant, a binder, and a plasticizer;

[0051] The barrier layer ceramic powder is fully ground and mixed with an organic solvent, a dispersant, a binder, and a plasticizer to prepare a barrier layer liquid slurry; preferably, the barrier layer ceramic powder is one or more of yttria-stabilized zirconia, scandia-stabilized zirconia, and doped cerium oxide;

[0052] The active electrolyte liquid slurry is prepared by grinding and mixing the electrolyte ceramic powder with an organic solvent, a dispersant, a binder, and a plasticizer; preferably, the electrolyte ceramic powder is one or more of yttria-stabilized zirconia, scandia-stabilized zirconia, and doped cerium oxide;

[0053] Active cathode ceramic powder is fully ground and mixed with an organic solvent, a dispersant, a binder, and a plasticizer to prepare an active cathode 40 liquid slurry; preferably, the active cathode ceramic powder is one or more of NiO and yttria-stabilized zirconia, scandium oxide-stabilized zirconia, and doped cerium oxide;

[0054] The cathode support ceramic powder is fully ground and mixed with an organic solvent, a dispersant, a binder, a plasticizer and a pore-forming agent to prepare a cathode support layer liquid slurry, that is, the cathode support layer liquid slurry forms a cathode support inner layer 51 liquid slurry, a cathode support middle layer 52 liquid slurry, and a cathode support outer layer 53 liquid slurry, respectively. Preferably, the pore-forming agent is one or two materials selected from spherical organic glass and spherical graphite, and the cathode support ceramic powder is one or more selected from NiO and yttria-stabilized zirconia, scandium oxide-stabilized zirconia, and doped cerium oxide.

[0055] S2, vacuum degassing the cathode support inner layer 51 liquid slurry, the cathode support middle layer 52 liquid slurry, the cathode support outer layer 53 liquid slurry, the active cathode 40 liquid slurry, and the electrolyte liquid slurry;

[0056] First, the cathode support inner layer 51 liquid slurry, the cathode support middle layer 52 liquid slurry, the cathode support outer layer 53 liquid slurry, the active cathode 40 liquid slurry, and the electrolyte slurry are respectively cast on the PET film tape to form corresponding slurry layers;

[0057] Then the cathode support inner slurry layer, cathode support middle slurry layer, cathode support outer slurry layer are separated from PET, and are stacked with the active cathode 40 slurry layer in sequence, and then they are isostatically pressed, and the PET on the active cathode 40 side is separated after isostatic pressing, and finally the electrolyte slurry layer is stacked on the surface of the active cathode 40 slurry layer, and isostatically pressed again to obtain a semi-electrolytic cell blank;

[0058] S3, pre-co-sintering the semi-electrolytic cell blank in step S2 without pressurization, and then pressurizing the cover plate for secondary high-temperature co-sintering to obtain a cathode-supported semi-electrolytic cell with a flat and high-strength gradient pore structure, with a pressurization pressure of 30-60 Pa;

[0059] S4, printing the barrier layer liquid slurry on the half electrolytic cell in step S3 by screen printing, and then sintering the barrier layer 20 at high temperature;

[0060] The anode liquid slurry is screen-printed on the semi-electrolytic cell with the firing barrier layer 20, and then the anode 10 is sintered at a high temperature to obtain the present large-area solid oxide electrolytic cell with a cathode supporting a mesh-like stepped pore structure;

[0061] Furthermore, the anode ceramic powder is a barrier layer ceramic powder and (La 0.8 Sr 0.2 ) 0.95 MnO 3-δ (LSM), La 0.6 Sr 0.4 FeO 3-δ (LSF) or La 0.6 Sr 0.4 Cr 0.2 Fe 0.8 O 3-δ One of the (LSCF);

[0062] The organic solvent is one or more of xylene, ethanol, butyl acetate and acetone;

[0063] The dispersant is one or more of polyethylene glycol, acrylic resin, herring oil, and polyvinyl butyral;

[0064] The binder is one or more of acrylic resin, ethyl cellulose and polyethylene;

[0065] The plasticizer is one or more of dibutyl phthalate, dioctyl phthalate and acrylic resin;

[0066] Further, in step S3, the temperature rise and fall system of the pre-co-sintering is firstly raised from room temperature to 500-700°C at a rate of 0.5-3°C / min, and kept at this temperature for 90-180min, then raised to 900-1200°C at a rate of 1-2°C / min, and kept at this temperature for 40-120min, and then naturally cooled to room temperature;

[0067] The heating and cooling system of the secondary high-temperature co-sintering is to first heat from room temperature to 1000-1200℃ at a rate of 3-5℃ / min, and keep it at this temperature for 45-95min, then heat to 1100-1300℃ at a rate of 1-2℃ / min, and keep it at this temperature for 60-120min, then heat to 1300-1500℃ at a rate of 1-2℃ / min, and keep it at this temperature for 500-700min, finally cool to 900-1100℃ at a rate of 1-3℃ / min, and then cool naturally to room temperature;

[0068] In step S4, the temperature rise and fall pattern of the high temperature sintering of the barrier layer 20 is to firstly heat from room temperature to 500-700°C at a rate of 1-3°C / min, and keep at this temperature for 55-100min, then heat to 1100-1300°C at a rate of 2-4°C / min, and keep at this temperature for 180-300min, and then naturally cool to room temperature;

[0069] The heating and cooling system of the high temperature sintering of the anode 10 is to first heat from room temperature to 600-700°C at a rate of 1-3°C / min, and keep it at this temperature for 60-120min, then heat to 1000-1200°C at a rate of 2-4°C / min, keep it at this temperature for 180-300min, and finally cool naturally to room temperature;

[0070] The present invention relates to a large-area solid oxide electrolytic cell supported by a cathode with a mesh-like stepped pore structure. The preparation method of the electrolytic cell is tape-casting-co-firing-screen printing-re-sintering. The large-area electrolytic cell with high yield and high performance can be obtained, which makes up for the shortcoming that the traditional specifications are generally above 100×100mm, and provides a technical solution for the preparation of large-area electrolytic cells.

Claims

1. A large-area solid oxide electrolytic cell supported by a cathode with a mesh-like stepped pore structure, characterized in that: include: An anode (10), a barrier layer (20), an electrolyte layer (30), an active cathode (40), and a cathode support layer stacked in sequence; The cathode support layer is provided with a spherical hole (62) and a connecting hole (61), and is divided into a cathode support inner layer (51), a cathode support middle layer (52), and a cathode support outer layer (53); The pore diameter of the spherical hole (62) is larger than the pore diameter of the connecting hole (61), and gradually increases in the cathode support inner layer (51), the cathode support middle layer (52), and the cathode support outer layer (53).

2. The large-area solid oxide electrolytic cell with a cathode supported by a mesh-like stepped pore structure according to claim 1, characterized in that: The distance between adjacent spherical holes (62) is connected by the communicating holes (61), and a mesh-like gas transmission channel is formed between the spherical holes (62) and the communicating holes (61).

3. The large-area solid oxide electrolytic cell with a cathode supported by a mesh-like stepped pore structure according to claim 1 or 2, characterized in that: The cathode support inner layer (51) has a thickness of 100-300 μm, the cathode support middle layer (52) has a thickness of 100-300 μm, and the cathode support outer layer (53) has a thickness of 100-300 μm.

4. The large-area solid oxide electrolytic cell with a cathode supported by a mesh-like stepped pore structure according to claim 3, characterized in that: The cathode support inner layer (51) has a porosity of 10%-20%, and the spherical pores (62) therein have a pore size of 1-10 μm; The cathode support middle layer (52) has a porosity of 20%-30%, and the spherical pores (62) therein have a pore size of 1-10 μm; The cathode support outer layer (53) has a porosity of 30%-40%, and the spherical pores (62) therein have a pore diameter of 20-30 μm.