Silicon carbide deposition equipment
By setting up an array of air intake units and air intake pipe joints in the reaction chamber of the silicon carbide deposition equipment, the problems of deposition uniformity and thickness consistency are solved, and the overall performance and product quality of the equipment are improved.
Patent Information
- Application Number
- CN202323436908.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-15
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2033-12-15
AI Technical Summary
The existing silicon carbide deposition equipment is insufficient in the intake pipe setting, resulting in inconsistent deposition uniformity and product deposition thicknesses at different locations in the chamber, affecting the pass rate of a single furnace.
Design a silicon carbide deposition equipment, using a cylindrical reaction chamber to set up multiple graphite boats, an air intake conduit is set up outside, an exhaust joint is set up on the top, an array of air intake units are set up around the circumference of the inner surface of the reaction chamber, and each group of air intake is in. The unit has several air intake pipe joints arranged at equal intervals. The air intake pipe joints include a main pipe and a sub-tube that penetrates the inner wall of the reaction chamber. The main pipe is located in the middle of the sub-tube, and the air outlet hole is provided on the outer surface. The orthogonal projection of the air intake pipe joint in the vertical direction. The angle is 10-45 degrees.
Through the improved intake pipe joint structure, the overall uniformity of the intake in the reaction chamber is improved, the uniformity of product deposition and the consistency of deposition thicknesses at different locations in the chamber are improved, and the pass rate of a single furnace is significantly improved.
Smart Images

Figure CN222043341U_ABST
Abstract
Description
Technical Field
[0001] The utility model relates to the technical field of silicon carbide preparation, in particular to silicon carbide deposition equipment. Background Art
[0002] For semiconductor equipment, its structural ceramic parts need low expansion coefficient, high thermal conductivity, and high precision in surface structure roughness. Conventional materials have many limitations and cannot meet the application requirements. Chemical vapor deposition silicon carbide parts can solve this problem well. For example, in the etching process, with the continuous improvement of the performance requirements of power electronic devices, the physical limitations of silicon materials are becoming increasingly apparent, which seriously restricts the improvement of the performance of silicon devices. In conventional processes and etching equipment, silicon materials are mostly used for gas uniformity disks and various focusing ring components. For advanced processes, in stronger corrosive environments, the service life of silicon is greatly reduced, which increases the frequency of component replacement, thereby reducing the available time of equipment, resulting in reduced production capacity and increased production costs. The service life of silicon carbide components can generally be increased by 1.5-2 times compared to silicon components, and can even reach more than 2 times in some processes.
[0003] Silicon carbide thin film deposition and block deposition, uniformity has a great impact on quality control, yield improvement and cost. Good uniformity of thin film deposition and one-time forming can avoid the pollution risk and processing cost introduced by secondary processing. Good block uniformity can also reduce the final machining removal amount. Silicon carbide has a high hardness and is difficult to machine, so it can effectively reduce the machining cost. At the same time, the machining process is prone to product breakage. Reducing machining also reduces the product scrap rate, which has a significant effect on cost control.
[0004] The Chinese patent with prior art publication number CN104046959B discloses a chemical vapor deposition device for epitaxial growth of silicon carbide, which does not have a special arrangement for the air inlet pipe and cannot meet actual review requirements. Utility Model Content
[0005] In order to improve the uniformity of product deposition and the consistency of product deposition thickness at different positions in a chamber under existing equipment conditions, thereby increasing the single furnace qualification rate, the present application provides a deposition device for improving CVD deposition uniformity.
[0006] In order to achieve the above purpose, the technical solution adopted by the utility model is:
[0007] A silicon carbide deposition device comprises a cylindrical reaction chamber, a plurality of graphite boats are arranged inside the reaction chamber, an air intake duct is arranged outside the reaction chamber, an exhaust joint connected to the inside is arranged on the top of the reaction chamber, and a plurality of air intake units are arranged symmetrically on the inner surface of the reaction chamber, and each group of air intake units is composed of a plurality of air intake pipe joints arranged at equal intervals;
[0008] The air inlet pipe joint comprises a main pipe penetrating the inner wall of the reaction chamber, one end of the main pipe located in the reaction chamber is fixedly connected to a sub-pipe perpendicular thereto, and the main pipe is located in the middle of the sub-pipe, one end of the sub-pipe is blocked, and an air outlet is provided on its outer surface at a distance from the main pipe;
[0009] One end of the main pipe located outside the reaction chamber is connected with an air inlet pipe.
[0010] Furthermore, there are at least two groups of air intake units, at least three rows of air intake pipe joints, and projections of the air intake pipe joints in the vertical direction do not cross each other.
[0011] Furthermore, the orthographic projection angle of the air intake pipe joint in the vertical direction is 10-45 degrees.
[0012] Furthermore, the diameter of the air outlet is 2-10 mm, and the inner diameter of the auxiliary pipe is 10-30 mm.
[0013] Working principle and beneficial effects: By setting an air intake pipe joint in the reaction chamber, the overall uniformity of the internal air intake is improved, and the uniformity of product deposition and the consistency of product deposition thickness at different positions in the chamber are improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 It is a schematic diagram of the three-dimensional structure of the utility model;
[0015] Figure 2 It is a schematic diagram of the cross-sectional structure of the air intake pipe joint of the utility model;
[0016] Figure 3 It is a schematic diagram of the three-dimensional structure of the air intake pipe joint of the utility model.
[0017] In the figure: 1, reaction chamber; 2, exhaust joint; 3, air inlet pipe joint; 31, main pipe; 32, auxiliary pipe; 33, air outlet. DETAILED DESCRIPTION
[0018] The present invention can be better understood according to the following embodiments.
[0019] The structures, proportions, sizes, etc. illustrated in the drawings of the specification are only used to match the contents disclosed in the specification for people familiar with this technology to understand and read, and are not used to limit the limiting conditions for the implementation of the utility model, so they have no substantial technical significance. Any modification of the structure, change of the proportion relationship or adjustment of the size, without affecting the effect and purpose that can be achieved by the utility model, should still fall within the scope of the technical content disclosed by the utility model. At the same time, the terms such as "upper", "lower", "front", "back", "middle" and so on quoted in this specification are only for the convenience of description, and are not used to limit the scope of the implementation of the utility model. The change or adjustment of their relative relationship should also be regarded as the scope of the implementation of the utility model without substantial change of the technical content.
[0020] like Figure 1-3 As shown, a silicon carbide deposition device comprises a cylindrical reaction chamber 1, a plurality of graphite boats are arranged inside the reaction chamber 1, an air intake duct is arranged outside the reaction chamber 1, and an exhaust joint 2 connected to the inside is arranged on the top of the reaction chamber 1, characterized in that: a plurality of air intake units are arranged symmetrically at the circumference of the inner surface of the reaction chamber 1, and each group of air intake units is composed of a plurality of air intake pipe joints 3 arranged at equal intervals;
[0021] The air inlet pipe joint 3 includes a main pipe 31 penetrating the inner wall of the reaction chamber 1, and one end of the main pipe 31 located in the reaction chamber 1 is fixedly connected to a sub-pipe 32 perpendicular thereto, and the main pipe 31 is located in the middle of the sub-pipe 32, one end of the sub-pipe 32 is blocked, and an air outlet hole 33 is provided on its outer surface at a position opposite to the main pipe 31;
[0022] One end of the main pipe 31 located outside the reaction chamber 1 is connected to an air inlet pipe.
[0023] Among them, there are at least two groups of air intake units, at least three rows of air intake pipe joints 3, and the projections of the air intake pipe joints 3 in the vertical direction do not cross each other, that is, the upper and lower adjacent rows of conversion pipes do not overlap or interfere with each other. The air intake pipe joints can be placed vertically or rotated at a certain angle. The rotation angle can be adjusted according to the shape, placement form, density, etc. of the deposited parts. The orthographic projection angle of the air intake pipe joints 3 in the vertical direction is 10-45 degrees.
[0024] The diameter of the air outlet 33 is 2-10 mm, the inner diameter of the auxiliary pipe 32 is 10-30 mm, and the number and distribution of the small holes can be adjusted according to the actual deposition conditions, the type, shape, placement and density of the deposition parts.
[0025] The deposit thickness differences were tested using a micrometer.
[0026] In order to better understand the following examples, three comparative examples are given.
[0027] Comparative Example 1: A method for improving the uniformity of silicon carbide deposition, comprising the following steps:
[0028] (a) Place 10 deposition substrates (from top to bottom) into the reaction chamber of the SiC chemical vapor deposition equipment, connect the air inlet pipe to the air inlet pipe joint 3, evacuate the reaction chamber to below 1 Pa, maintain for 10 min, then fill the reaction chamber with inert gas to 1 kPa, and then evacuate to below 1 Pa, and repeat this process 5 times.
[0029] (b) The reaction chamber is heated to 1200°C, and argon, hydrogen and MTS gas are introduced into the reaction chamber, with a total gas flow rate of 16 L / min, a diameter of the gas outlet 33 of 1 mm, an inner diameter of the auxiliary pipe 32 of 9 mm, two groups of gas inlet units, each group of gas inlet units having four rows of gas inlet pipe joints 3, and an orthographic projection angle of the gas inlet pipe joints 3 in the vertical direction of 9 degrees. The pressure in the reaction chamber is maintained at 2000 Pa, and silicon carbide deposition is performed;
[0030] (c) determining whether the SiC deposited layer has reached the required thickness; if not, repeating step (b); if so, executing step (d);
[0031] (d) When the set deposition thickness is reached, the raw material gas supply is stopped, argon gas is continued to be introduced into the reaction chamber, and the temperature is kept at 15-30 minutes before cooling down;
[0032] (e) When the temperature drops below 200° C., inert gas purging and vacuuming are performed, and the process is repeated 3-5 times while maintaining the indoor pressure at normal pressure. The chamber is then naturally cooled to room temperature to obtain a deposited silicon carbide material.
[0033] Comparative Example 2: A method for improving the uniformity of silicon carbide deposition, comprising the following steps: The difference from Comparative Example 1 is that the total gas flow rate is 16 L / min, the diameter of the air outlet 33 is 11 mm, the inner diameter of the auxiliary pipe 32 is 35 mm, there are two groups of air intake units, each group of air intake units has four rows of air intake pipe joints 3, and the orthographic projection angle of the air intake pipe joints 3 in the vertical direction is 9 degrees.
[0034] Comparative Example 3: A method for improving the uniformity of silicon carbide deposition, comprising the following steps: The difference from Comparative Example 1 is that the total air intake volume is 16 L / min, there is no auxiliary pipe 32, there are two groups of air intake units, each group of air intake units has four rows of air intake pipe joints 3, and the orthographic projection angle of the air intake pipe joints 3 in the vertical direction is 9 degrees.
[0035] Comparative Example 4: A method for improving the uniformity of silicon carbide deposition, comprising the following steps: The difference from Comparative Example 1 is that the total air intake volume is 16 L / min, there is no auxiliary pipe 32, there are two groups of air intake units, and each group of air intake units has four rows of air intake pipe connectors 3.
[0036] The following is an example
[0037] Example 1: A method for improving the uniformity of silicon carbide deposition, comprising the following steps: The difference from Example 1, Example 2, Example 3 and Example 4 is that: the gas flow rate is 16 L / min, the diameter of the air outlet 33 is 2 mm, the inner diameter of the auxiliary pipe 32 is 10 mm, there are two groups of air intake units, each group of air intake units has four rows of air intake pipe joints 3, and the orthographic projection angle of the air intake pipe joints 3 in the vertical direction is 20 degrees.
[0038] Example 2: A method for improving the uniformity of silicon carbide deposition, comprising the following steps: The difference from Example 1, Example 2, Example 3 and Example 4 is that: the gas flow rate is 16 L / min, the diameter of the air outlet 33 is 2 mm, the inner diameter of the auxiliary pipe 32 is 10 mm, there are two groups of air intake units, each group of air intake units has four rows of air intake pipe joints 3, and the orthographic projection angle of the air intake pipe joints 3 in the vertical direction is 9 degrees.
[0039] Example 3: A method for improving the uniformity of silicon carbide deposition, comprising the following steps: The difference from Example 1, Example 2, Example 3 and Example 4 is that: the gas flow rate is 16 L / min, the diameter of the air outlet 33 is 8 mm, the inner diameter of the auxiliary pipe 32 is 20 mm, there are two groups of air intake units, each group of air intake units has four rows of air intake pipe joints 3, and the orthographic projection angle of the air intake pipe joints 3 in the vertical direction is 9 degrees.
[0040] Example 4: A method for improving the uniformity of silicon carbide deposition, comprising the following steps: The difference from Example 1, Example 2, Example 3 and Example 4 is that: the gas flow rate is 16 L / min, the diameter of the air outlet 33 is 10 mm, the inner diameter of the auxiliary pipe 32 is 30 mm, there are two groups of air intake units, each group of air intake units has four rows of air intake pipe joints 3, and the orthographic projection angle of the air intake pipe joints 3 in the vertical direction is 9 degrees.
[0041] The deposition uniformity of the embodiment and the comparative example was tested, and the data are shown in Table 1.
[0042] The deposit thickness differences were tested using a micrometer.
[0043] Table 1 Deposition uniformity test data
[0044] Test Data Substrate 1 Substrate 2 Substrate 3 Substrate 4 Substrate 5 Substrate 6 Substrate 7 Substrate 8 Substrate 9 Substrate 10 Example 1 95.5% 97.2% 96.7% 95.8% 98.1% 96.2% 95.1% 97.0% 97.8% 96.9% Example 2 94.3% 96.6% 95.8% 94.9% 96.0% 94.4% 93.9% 95.2% 96.1% 94.9% Example 3 92.8% 93.7% 94.4% 93.0% 93.7% 92.9% 92.8% 92.2% 94.3% 93.3% Example 4 90.9% 91.2% 92.1% 90.8% 91.5% 91.9% 91.7% 90.8% 91.1% 90.2% Comparative Example 1 52.8% 57.8% 82.7% 72.7% 60.5% 78.9% 55.8% 62.1% 72.8% 58.1% Comparative Example 2 43.0% 49.3% 75.8% 70.2% 55.8% 72.7% 50.1% 58.9% 69.9% 55.6% Comparative Example 3 39.1% 43.9% 69.7% 62.7% 50.2% 66.1% 44.9% 56.8% 65.8% 50.8% Comparative Example 4 30.8% 51.8% 67.7% 61.8% 49.0% 65.8% 43.0% 52.9% 62.9% 49.3%
[0045] In some embodiments, the best effect is achieved when the vertical projection angle of the air intake pipe joint is 20 degrees.
[0046] It can be seen from the above data that under the same conditions, when the air intake pipe joint is not used, the uniformity is very poor and the uniformity difference between substrates is also large. When the air intake pipe joint is used, the overall uniformity is significantly improved, and the difference between substrate parts is significantly reduced. When the orthographic projection angle of the air intake pipe joint 3 in the vertical direction is 20 degrees, the effect is best.
Claims
1. A silicon carbide deposition device, comprising a cylindrical reaction chamber (1), wherein a plurality of graphite boats are arranged inside the reaction chamber (1), an air inlet duct is arranged outside the reaction chamber (1), and an exhaust joint (2) communicating with the inside of the reaction chamber (1) is arranged on the top of the reaction chamber (1), characterized in that: A plurality of air intake units are arranged symmetrically on the inner surface of the reaction chamber (1), and each group of air intake units is composed of a plurality of air intake pipe joints (3) arranged at equal intervals. The air inlet pipe joint (3) comprises a main pipe (31) penetrating the inner wall of the reaction chamber (1); one end of the main pipe (31) located in the reaction chamber (1) is fixedly connected to a secondary pipe (32) perpendicular thereto; the main pipe (31) is located in the middle of the secondary pipe (32); one end of the secondary pipe (32) is blocked; and an air outlet hole (33) is provided on its outer surface at a position opposite to the main pipe (31); One end of the main pipe (31) located outside the reaction chamber (1) is connected to an air inlet pipe.
2. A silicon carbide deposition device according to claim 1, characterized in that: There are at least two groups of air intake units, there are at least three rows of air intake pipe joints (3), and the projections of the air intake pipe joints (3) in the vertical direction do not intersect each other.
3. The silicon carbide deposition device according to claim 2, characterized in that: The orthographic projection angle of the air intake pipe joint (3) in the vertical direction is 10-45 degrees.
4. The silicon carbide deposition device according to claim 2, characterized in that: The diameter of the air outlet (33) is 2-10 mm, and the inner diameter of the auxiliary pipe (32) is 10-30 mm.