Nanometer multilayer composite film structure for valve

By plating the nano-multi-layer composite film structure on the alloy substrate surface of the ball valve, the problem of insufficient high temperature and corrosion resistance in high frequency and chemical ball valves is solved, and a longer service life and higher Wear resistance.

CN222064671UActive Publication Date: 2024-11-26SUZHOU HUIZHUAN NANO NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202323199238.5
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2023-11-27
Publication Date
2024-11-26
Estimated Expiration
2033-11-27

AI Technical Summary

Technical Problem

Traditional thermal spray materials are ineffective in high-frequency ball valves and chemical ball valves due to insufficient high temperature and corrosion resistance, resulting in valve seal failure and short service life.

Method used

Using a nano-multi-layer composite thin film structure, including a metal transition layer and a periodic cyclic composite layer. The periodic cyclic composite layer is composed of Al-Cr-Ti-Si-N, Ti-Si-N and amorphous carbon film a-C layers, and is coated On the surface of the alloy matrix, the binding force and density are enhanced, and dislocations and material failure are suppressed.

Benefits of technology

It significantly improves high temperature and corrosion resistance, so that the ball valve is used in an environment of 600℃ for more than one year, and is not prone to corrosion in sulfuric or nitric acid, extending the service life of the ball valve to about one year.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN222064671U_ABST
    Figure CN222064671U_ABST
Patent Text Reader

Abstract

The utility model discloses a nanometer multilayer composite film structure for a valve, which is plated on the surface of an alloy matrix of the valve, the nanometer multilayer composite film structure comprises a metal transition layer and a periodic cycle composite layer, the periodic cycle composite layer is arranged on the metal transition layer, and the periodic cycle composite layer is arranged on the metal transition layer. The periodic cycle composite layer comprises a plurality of stacked periodic units, each periodic unit comprises an Al-Cr-Ti-Si-N layer, a Ti-Si-N layer and an amorphous carbon film a-C layer which are arranged from bottom to top, the number of the periodic units is not less than 100, and the thickness of the periodic cycle composite layer is 100-300 microns. The wear resistance, the high temperature resistance and the corrosion resistance of the valve can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The utility model relates to a composite film structure, in particular to a nano multi-layer composite film structure used for valves. Background Art

[0002] Thermal spraying technology is widely used in the ball valve industry. Common thermal spraying materials include tungsten carbide, nickel-based alloys, chromium carbide, etc. These materials have certain hardness and wear resistance, but they are still limited in their application to special ball valves (such as high-frequency ball valves, chemical industry ball valves, etc.). In the application of high-frequency ball valves, the opening and closing times of the ball and the valve seat are very frequent, for example: once every 10 seconds, 8640 times a day. Traditional thermal spraying materials can only withstand a maximum of four to five weeks of use under relatively low working conditions. After that, the sealing of the valve will have problems and cannot operate normally. In the ball valves used in the chemical industry, the ball valves and valve seats will come into contact with many chemically corrosive materials or high-temperature materials. The coating materials formed by traditional thermal spraying on the surface of the substrate will soon fail when encountering high temperature or corrosion, resulting in the lack of sealing and protection of the ball valve. Utility Model Content

[0003] In view of the above-mentioned defects of the prior art, the utility model provides a nano multi-layer composite film structure for valves, which solves the problem of short valve life caused by insufficient high temperature resistance and corrosion resistance of the coating structure on the valve component.

[0004] The technical solution of the utility model is as follows: a nano multilayer composite film structure for a valve, plated on the surface of an alloy substrate of the valve, the nano multilayer composite film structure comprising a metal transition layer and a periodic cyclic composite layer, the periodic cyclic composite layer being arranged on the metal transition layer, the periodic cyclic composite layer comprising a plurality of superimposed periodic units, the periodic units comprising an Al-Cr-Ti-Si-N layer, a Ti-Si-N layer and an amorphous carbon film aC layer arranged from bottom to top, the number of the periodic units being not less than 100, and the thickness of the periodic cyclic composite layer being 100 to 300 microns.

[0005] Furthermore, the metal transition layer is a metal chromium, titanium or zirconium coating.

[0006] Furthermore, the thickness of the metal transition layer is 1000 to 2000 nanometers.

[0007] Furthermore, the thickness of the Al-Cr-Ti-Si-N layer is 5 to 300 nanometers, the hardness of the Al-Cr-Ti-Si-N layer is 3500 to 4000 HV, and the preferred thickness is 5 to 50 nanometers.

[0008] Furthermore, the thickness of the Ti—Si—N layer is 5 to 300 nanometers, the hardness of the Ti—Si—N layer is 3200 to 3800 HV, and the preferred thickness is 5 to 50 nanometers.

[0009] Furthermore, the thickness of the amorphous carbon film aC layer is 5 to 300 nanometers, the hardness of the amorphous carbon film aC layer is 1800 to 2500 HV, and the preferred thickness is 5 to 20 nanometers.

[0010] Furthermore, the alloy matrix of the valve is stainless steel, titanium alloy or zirconium alloy.

[0011] The utility model uses a metal transition layer to combine the alloy matrix and the periodic cycle composite layer to enhance the bonding force between the alloy matrix and the periodic cycle composite layer. A nano multilayer structure is formed, and a thinner single-layer coating can reduce the internal stress of each single-layer film material and reduce coating defects. The periodic cycle structure effectively inhibits the generation of dislocations. The combination of the Al-Cr-Ti-Si-N layer and the Ti-Si-N layer with similar organizational structures provides support for the amorphous carbon film aC layer on the one hand, and on the other hand, the interlayer bonding force between the two is good and the density is high, and foreign substances are not easy to penetrate from the interlayer to destroy the multilayer structure.

[0012] Compared with the carbide thermal spraying in the prior art, the technical solution provided by the utility model has the following advantages:

[0013] It has better high temperature resistance and can be used in a temperature environment of 600°C. Its corrosion resistance is also improved. In the use environment of sulfuric acid or nitric acid (concentration within 30%), the ball valve with the composite film structure of the utility model will not be seriously corroded after one year of use. In addition, the improvement of wear resistance can increase the life of the ball valve from a few days to a few weeks to about one year. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 It is a schematic diagram of the structure of a nano multilayer composite film structure used for valves. DETAILED DESCRIPTION

[0015] The present invention is further described below in conjunction with embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. After reading this description, various equivalent modifications to the description by those skilled in the art fall within the scope defined by the claims attached to this application.

[0016] Please combine Figure 1 As shown, the nano multilayer composite film structure for valves involved in this embodiment is prepared by the following means:

[0017] First, clean the base of the ball valve, which includes the ball and the valve seat. Use an ultrasonic cleaner and an organic solution (acetone, alcohol) to clean the base to be coated. After cleaning, dry it at 80-90°C.

[0018] The cleaned and dried ball valve substrate 1 is placed in a coating vacuum chamber to prepare a metal transition layer 2, an Al-Cr-Ti-Si-N layer 301a, a Ti-Si-N layer 301b and an amorphous carbon film aC layer 301c. The metal transition layer 2 chromium, titanium, and zirconium targets (purity 99.999%) are atomically deposited on the workpiece surface by an unbalanced magnetron sputtering process, and the process parameters are as follows: an argon flow rate of 150 to 300 sccm, a magnetron sputtering target power set to 5 to 8 kW, a bias voltage of 150 to 350 V, a furnace temperature of 400 to 450°C, and a coil current of 1 to 3 A. The subsequent layers of the periodic unit are also achieved by unbalanced magnetron sputtering technology. The process parameters for preparing each layer of the periodic unit 3 are as follows:

[0019] Al-Cr-Ti-Si-N layer 301a: The target materials used are Al / Cr (atomic ratio 70 / 30) and Ti / Si (85 / 15) with a purity of 99.999%, an argon flow rate of 150-250sccm, a magnetron sputtering target power set to 8-10kW, a bias voltage of 100-150V, a furnace temperature of 450-500°C, a coil current of 5-6A, and a nitrogen flow rate of 100-150sccm.

[0020] Ti-Si-N layer 301b: The target material used is Ti / Si (85 / 15) with a purity of 99.999%, an argon flow rate of 150-250sccm, a magnetron sputtering target power setting of 8-9kW, a bias voltage of 120-180V, a furnace temperature of 450-500°C, a coil current of 4-5A, and a nitrogen flow rate of 80-120sccm.

[0021] aC layer 301c: Use graphite (purity 99.999%), argon gas flow rate 100-150sccm, magnetron sputtering target power set to 4-5kW, bias voltage 200-250V, furnace temperature 450-500℃, coil current 1-2A.

[0022] The steps of preparing Al-Cr-Ti-Si-N layer 301a, Ti-Si-N layer 301b and amorphous carbon film aC layer 301c are repeated multiple times according to the designed number of periodic units 301 in the periodic cyclic composite layer 3 to complete the preparation of the nano multilayer composite thin film structure.

[0023] The parameters of the nano multilayer composite film structure for valves in Example 1 are:

[0024] The coating is based on a stainless steel substrate, with a chromium metal layer thickness of 1000 nanometers; the Al-Cr-Ti-Si-N layer thickness in the periodic unit is 5 nanometers, with a hardness of 4000 HV; the Ti-Si-N layer thickness in the periodic unit is 5 nanometers, with a hardness of 3800 HV; the amorphous carbon film aC layer thickness in the periodic unit is 5 nanometers, with a hardness of 2500 HV; the periodic cyclic composite layer contains 6700 periodic units with a total thickness of 100.5 microns.

[0025] The parameters of the nano multilayer composite film structure for valves in Example 2 are:

[0026] The coating is based on a stainless steel substrate, with a chromium metal layer thickness of 1200 nanometers; the Al-Cr-Ti-Si-N layer thickness in the periodic unit is 20 nanometers, and the hardness is 3500 HV; the Ti-Si-N layer thickness in the periodic unit is 30 nanometers, and the hardness is 3200 HV; the amorphous carbon film aC layer thickness in the periodic unit is 30 nanometers, and the hardness is 1800 HV; the periodic cyclic composite layer contains 2000 periodic units, with a total thickness of 160 microns.

[0027] The parameters of the nano multilayer composite film structure for valves in Example 3 are:

[0028] The coating is based on a stainless steel substrate, with a chromium metal layer thickness of 1500 nanometers; the Al-Cr-Ti-Si-N layer thickness in the periodic unit is 50 nanometers, with a hardness of 3500 HV; the Ti-Si-N layer thickness in the periodic unit is 50 nanometers, with a hardness of 3200 HV; the amorphous carbon film aC layer thickness in the periodic unit is 50 nanometers, with a hardness of 1800 HV; the periodic cyclic composite layer contains 2000 periodic units with a total thickness of 300 microns.

[0029] The parameters of the nano multilayer composite film structure for valves in Example 4 are:

[0030] The coating is based on a titanium alloy substrate, and the thickness of the titanium metal layer is 2000 nanometers; the thickness of the Al-Cr-Ti-Si-N layer in the periodic unit is 100 nanometers, and the hardness is 3500HV; the thickness of the Ti-Si-N layer in the periodic unit is 100 nanometers, and the hardness is 3200HV; the thickness of the amorphous carbon film aC layer in the periodic unit is 100 nanometers, and the hardness is 1800HV; the number of periodic units contained in the periodic cyclic composite layer is 400, and the total thickness is 120 microns.

[0031] The parameters of the nano multilayer composite film structure for valves in Example 5 are:

[0032] The coating is based on a zirconium alloy substrate, and the thickness of the zirconium metal layer is 2000 nanometers; the thickness of the Al-Cr-Ti-Si-N layer in the periodic unit is 300 nanometers, and the hardness is 4000HV; the thickness of the Ti-Si-N layer in the periodic unit is 300 nanometers, and the hardness is 3800HV; the thickness of the amorphous carbon film aC layer in the periodic unit is 300 nanometers, and the hardness is 2500HV; the number of periodic units contained in the periodic cyclic composite layer is 120, and the total thickness is 108 microns.

[0033] The above embodiments were tested for high temperature resistance, wear resistance and corrosion resistance. The high temperature resistance test was conducted by placing the test piece in a high temperature oven with the temperature set from 300 to 700°C for two hours. The wear resistance test was conducted by using a ball mill with a rotation speed of 1500 rpm. Different test pieces were ground for 8 hours and then the depth of the ball pit was measured. The corrosion resistance test was conducted by placing the product in a salt spray chamber and testing it according to the industry standard of the neutral salt spray test.

[0034] The results are as follows:

[0035] Maximum temperature Maximum ball pit diameter Longest corrosion resistance time Example 1 560℃ 667 microns 78 hours Example 2 520℃ 389 microns 112 hours Example 3 600℃ 102 microns 206 hours Example 4 510℃ 450 microns 101 hours Example 5 520℃ 606 microns 86 hours

Claims

1. A nano multilayer composite film structure for a valve, characterized in that: The nano multilayer composite film structure is plated on the surface of the alloy substrate of the valve, and includes a metal transition layer and a periodic composite layer. The periodic composite layer is arranged on the metal transition layer. The periodic composite layer includes a plurality of superimposed periodic units, and the periodic units include an Al-Cr-Ti-Si-N layer, a Ti-Si-N layer and an amorphous carbon film aC layer arranged from bottom to top. The number of the periodic units is not less than 100, and the thickness of the periodic composite layer is 100 to 300 microns.

2. The nano multi-layer composite film structure for valves according to claim 1, characterized in that: The metal transition layer is a metal chromium, titanium or zirconium coating.

3. The nano multi-layer composite film structure for valves according to claim 2, characterized in that: The thickness of the metal transition layer is 1000-2000 nanometers.

4. The nano multi-layer composite film structure for valves according to claim 1, characterized in that: The thickness of the Al-Cr-Ti-Si-N layer is 5 to 300 nanometers, and the hardness of the Al-Cr-Ti-Si-N layer is 3500 to 4000 HV.

5. The nano multi-layer composite film structure for valves according to claim 4, characterized in that: The thickness of the Al-Cr-Ti-Si-N layer is 5 to 50 nanometers.

6. The nano multi-layer composite film structure for valves according to claim 1, characterized in that: The thickness of the Ti-Si-N layer is 5 to 300 nanometers, and the hardness of the Ti-Si-N layer is 3200 to 3800 HV.

7. The nano multi-layer composite film structure for valves according to claim 6, characterized in that: The thickness of the Ti-Si-N layer is 5 to 50 nanometers.

8. The nano multi-layer composite film structure for valves according to claim 1, characterized in that: The thickness of the amorphous carbon film aC layer is 5 to 300 nanometers, and the hardness of the amorphous carbon film aC layer is 1800 to 2500 HV.

9. The nano multi-layer composite film structure for valves according to claim 8, characterized in that: The thickness of the amorphous carbon film aC layer is 5 to 20 nanometers.