SPECIFIC LITHIUM-BASED NEGATIVE ELECTRODE AND LITHIUM ELECTROCHEMICAL GENERATOR INCLUDING SUCH A NEGATIVE ELECTRODE
A lithium-barium alloy-based negative electrode addresses handling and production challenges in lithium electrochemical generators, enabling thin, cost-effective electrodes with improved mechanical properties and power density.
Patent Information
- Application Number
- FR2022002999
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-04-01
- Publication Date
- 2024-09-27
- Estimated Expiration
- 2042-04-01
AI Technical Summary
Lithium electrochemical generators face challenges such as the formation of lithium peroxide and dendrites during discharge, safety issues due to low melting temperature, handling difficulties, and the inability to produce thin negative electrodes with standard rolling mills, which are expensive and commercially unavailable.
A lithium-based negative electrode alloy comprising up to 20 atomic% barium, allowing for easy lamination and achieving low thicknesses, improved mechanical properties, and reduced manufacturing costs, which can be self-supporting or supported by a current collector.
The lithium-barium alloy enables the production of thin, mechanically robust negative electrodes that function similarly to pure lithium electrodes, enhancing power density and reducing manufacturing costs without compromising cell performance.
Smart Images

Figure 00000018_0000 
Figure 00000018_0001 
Figure 00000019_0000
Abstract
Description
Title of the invention: SPECIFIC LITHIUM-BASED NEGATIVE ELECTRODE AND LITHIUM ELECTROCHEMICAL GENERATOR COMPRISING SUCH A NEGATIVE ELECTRODE Technical field
[0001] The present invention relates to a specific negative electrode usable in an energy storage device and, more specifically, a lithium electrochemical generator, this generator being able to be a primary electrochemical generator (or battery), when it is not rechargeable or a secondary electrochemical generator (or accumulator) when it is rechargeable.
[0002] The present invention also relates to an electrochemical generator comprising such a negative electrode, this electrochemical generator having effective electrochemical properties while being able to have a thinner negative electrode thickness than for an electrode comprising only metallic lithium, thus conferring a very particular interest for power applications.
[0003] The field of the invention can be defined as that of energy storage devices, in particular that of lithium electrochemical generators. STATE OF THE PRIOR ART
[0004] Energy storage devices are conventionally electrochemical generators operating on the principle of electrochemical cells capable of delivering an electric current thanks to the presence in each of them of a pair of electrodes (respectively, a positive electrode and a negative electrode) separated by an electrolyte, the electrodes comprising specific materials capable of reacting according to an oxidation-reduction reaction, whereby there is production of electrons at the origin of the electric current and production of ions which will circulate from one electrode to the other by means of an electrolyte.
[0005] The most commonly used electrochemical generators of this type are currently the following:
[0006] *Ni-MH electrochemical generators using metal hydride and nickel oxyhydroxide as electrode materials;
[0007] *Ni-Cd electrochemical generators using cadmium and nickel oxyhydroxide as electrode materials;
[0008] *lead-acid electrochemical generators using lead and lead oxide PbO2 as electrode materials; and
[0009] *lithium electrochemical generators, such as those using metallic lithium as the active material of the negative electrode.
[0010] Because metallic lithium is a particularly light solid element and has the lowest electrochemical potential, thus allowing access to an interesting mass energy density, lithium electrochemical generators are particularly favorable candidates to dethrone the other types of accumulators mentioned above.
[0011] More specifically, metallic lithium, which can constitute the active material of the negative electrode, is a material that can be used in most systems as its mass and volume energy are high. Indeed, lithium has a density of 0.534 g / cm3 and a mass energy of 3861 mAh / g as well as a volume energy density of 2061 mAh / cm3. These values remain very high compared to those obtained with other negative electrode materials, in particular thanks to the reaction Li —> Li+ + e , this reaction involving the exchange of a single electron per lithium atom, which is very light and thus generates a significant amount of energy for a low volume / mass ratio.
[0012] One of the disadvantages of using lithium is due, on the one hand, to the possible formation of lithium peroxide during discharge processes and, on the other hand, to the possible formation of lithium dendrites during repeated charging processes, which can short-circuit the accumulator and damage it.
[0013] Furthermore, lithium can pose safety problems, due to its melting temperature of 180°C and can present handling difficulties for the manufacture of negative electrodes.
[0014] Indeed, lithium is a very reactive metal, particularly when it is subjected to an environment containing water, nitrogen and / or oxygen, and has the ability to adhere to all types of metals or alloys, such as stainless steel, steel, or even certain fluorinated polymers. Thus, it can be difficult to handle and shape, for example, by rolling or extrusion, unless special precautions are taken, particularly by working in a neutral, moisture-free atmosphere and / or by working with tools coated with a layer of non-reactive polymer, such as low-density polyethylene.
[0015] Finally, for use in electrochemical generators, such as batteries and accumulators, it may be advantageous to use very thin lithium foils to form the negative electrode, for example, with a thickness ranging from 10 μm to 50 μm, in particular to increase the energy and power densities and to limit the fact that too much capacity is put on the negative electrode compared to the capacity available on the positive electrode. However, such a thickness is impossible to achieve with standard rolling mills, lithium being too malleable. and tearing at greater thicknesses and when such foils are commercially available they are very expensive, even when already pre-rolled onto current collectors (e.g. copper foil).
[0016] Also, in view of the drawbacks mentioned above and in particular those relating to the difficulty of handling lithium to produce negative electrodes of small thicknesses, the authors of the present invention have set themselves the objective of proposing a new type of negative electrode based on lithium usable in lithium electrochemical generators as well as a new type of lithium electrochemical generator comprising this type of negative electrode. Statement of the invention
[0017] Thus, the invention relates to a negative electrode for a lithium electrochemical generator characterized in that it comprises, as active material, an alloy comprising lithium and barium, in which the barium is present in the alloy at a level of at most 20 atomic%.
[0018] Before going into more detail in the description of this invention, we specify the following definitions.
[0019] By atomic %, we mean, conventionally, in the above and the following, the ratio corresponding to the ratio of (total number of barium atoms / total number of atoms of the alloy) * 100.
[0020] By negative electrode, we mean, conventionally, in the above and the following, the electrode which acts as an anode, when the electrochemical generator delivers current (that is to say when it is in the process of discharging) and which acts as a cathode, when the electrochemical generator is in the process of charging (in the latter case, the electrochemical generator can be qualified as an accumulator, because it can be subjected to a process of charging and discharging).
[0021] By active material of the negative electrode, is meant, conventionally, in the above and the following, the material which is directly involved in the oxidation reaction taking place at the negative electrode, this active material being, in the context of this invention, an alloy comprising lithium and barium.
[0022] The negative electrode comprising such an active material can be easily prepared by lamination and have compatible low thicknesses to obtain an improvement in power density.
[0023] Furthermore, the potential of barium is very close to that of lithium at 0.13 V vs. Li. Thus, lithium and barium alloys should have a working potential very comparable to lithium, which should allow generators containing these alloys to operate similarly to generators containing pure lithium.
[0024] The alloy comprising lithium and barium is an alloy, in which the barium is present in the alloy at a level of at most 20 atomic%, more specifically 2 to 20 atomic% and, even more specifically, 2 to 10 atomic%.
[0025] The negative electrode may consist solely of the active material, which is the alloy comprising lithium and barium as mentioned above.
[0026] From a structural point of view, the negative electrode may advantageously be in the form of a sheet or plate having a thickness ranging from 5 to 50 μm.
[0027] Advantageously, the alloy comprising lithium and barium constituting the active material of the negative electrode may be an alloy comprising exclusively lithium and barium, which means that the alloy in question comprises barium at a level of at most 20 atomic % and lithium at a level of at least 80 atomic %.
[0028] From a structural point of view, when the lithium and barium alloy consists exclusively of lithium and barium and the barium content is 20 atomic %, the lithium and barium alloy is in the form of an intermetallic compound of formula BaLi4. For a barium content of less than 20 atomic %, the alloy will be in the form of a solid solution consisting of a lithium matrix, in which a defined compound BaLi4 is formed.
[0029] The authors of the present invention have been able to demonstrate that an alloy comprising lithium and barium is easily laminated and has good mechanical properties, particularly in terms of tensile strength, particularly for thicknesses as defined above. What is more, an electrode comprising such an alloy can be produced at lower manufacturing costs compared to an electrode having the same thickness of metallic lithium electrode.
[0030] Advantageously, the negative electrode may be self-supporting, that is to say that it does not need to be affixed to a support and, more specifically, that it does not need to be affixed to a current collector. Alternatively, it may be associated with a support, for example, of the current collector type, which may be a strip or a grid made of at least one electrically conductive metal element, such as copper, nickel, tantalum, titanium, tungsten, stainless steel, which strip or grid may have a thickness of up to 500 μm.
[0031] The alloy constituting the active material of the negative electrode may comprise, in addition to lithium and barium, a third element chosen from magnesium, zinc, indium, calcium, gallium and aluminum, this third element being able to be present in a content ranging from 2 to 20 atomic% and, preferably, from 2 to 10 atomic%. This type of alloy may be described as a ternary alloy. More specifically, the alloy constituting the active material of the negative electrode may be an alloy of lithium, barium and aluminum, an alloy of lithium, barium and indium or an alloy of lithium, barium and zinc.
[0032] Negative electrodes are particularly suitable for use in the construction of lithium electrochemical generators (whether batteries or accumulators).
[0033] Thus, the invention also relates to an electrochemical generator comprising at least one electrochemical cell comprising a positive electrode comprising, as active material, a lithium insertion material; a negative electrode and a lithium ion-conducting electrolyte arranged between said negative electrode and said positive electrode, characterized in that the negative electrode is as defined above.
[0034] By positive electrode, we mean, conventionally, in the above and the following, the electrode which acts as cathode, when the electrochemical generator delivers current (that is to say when it is in the process of discharging) and which acts as an anode when the electrochemical generator is in the process of charging (in the latter case, the electrochemical generator can be qualified as an accumulator, because it can be subjected to a process of charging and discharging).
[0035] The positive electrode of the electrochemical generator of the invention comprises, as active material, a lithium insertion material and, more specifically, a material chosen from lithiated oxides comprising at least one transition metal element, lithiated phosphates comprising at least one transition metal element, manganese dioxide and mixtures thereof.
[0036] As a lithium oxide comprising at least one transition metal element, there may be mentioned an oxide of the following formula:
[0037] LiM02
[0038] wherein M is an element selected from Ni, Co, Mn, Al, Mg and mixtures thereof, and preferably, further, with M being an element selected from Ni, Co, Mn, Al and mixtures thereof.
[0039] From a structural point of view, the oxide of the above formula has a lamellar structure.
[0040] Examples of such oxides include the lithium oxides LiCoO2, LiNiO2 and the mixed oxides Li(Ni,Co,Mn)O2 (and more specifically, LiNixMnyCozO2, in which x+y+z=l, such as Li(Nii / 3Mni / 3Coi / 3)O2 also known as NMC) or Li(Nio>6Mn0j2Cooj2)02 (also known as NMC666), Li(Ni,Co,Al)O2 (and more specifically, LiNixCoyAlzO2, in which x+y+z=l, such as Li(NioJsCooji5Alo>o5)02 also known as NCA) or Li(Ni,Co,Mn,Al)O2.
[0041] As a lithium oxide comprising at least one transition metal element, mention may also be made of lithium oxides of spinel structure, such as LiMn2O4.
[0042] As examples of lithium phosphate compounds comprising at least one element transition metal, we can cite compounds of formula LiM'PO4, where M1 is chosen from Fe, Mn, Co and mixtures thereof, such as LiFePO4.
[0043] The active material of the positive electrode may be present at a rate of 80 to 95% by mass of the total mass of the positive electrode.
[0044] Furthermore, the positive electrode may comprise at least one electronically conductive additive and / or at least one binder, such as a polymeric binder, which may ensure the cohesion of the positive electrode.
[0045] The electronically conductive additive may be selected from carbon blacks, acetylene blacks, graphite (in particular, graphite powder), carbon fibers (in particular, vapor-formed carbon fibers known by the abbreviation VGCF), carbon nanotubes, titanium (in particular, in powder form), nickel (in particular, in powder or foam form), aluminum (in particular, in powder form), stainless steel (in particular, in powder form) and mixtures thereof.
[0046] The binder(s) may be, in particular, chosen from polymeric binders, such as:
[0047] *fluorinated (co)polymers which may be proton conductors, such as:
[0048] -fluorinated polymers, such as polytetrafluoroethylene (known by the abbreviation PTFE), polyvinylidene fluoride (known by the abbreviation PVDF);
[0049] -fluorinated copolymers, such as poly(vinylidene fluoride-co-hexafluoropropene) (known by the abbreviation PVDF-HFP);
[0050] -proton-conducting fluorinated polymers, such as Nafion®;
[0051] *elastomeric polymers, such as a styrene-butadiene copolymer (known by the abbreviation SBR), an ethylene-propylene-diene monomer copolymer (known by the abbreviation EPDM);
[0052] *polymers of the polyvinyl alcohol family;
[0053] *cellulosic polymers, such as sodium carboxymethylcellulose; and
[0054] *mixtures thereof.
[0055] Preferably, the binder used is a binder based on a fluorinated polymer, such as polytetrafluoroethylene, polyvinylidene fluoride and mixtures thereof, this type of binder allowing a good percolating network to be obtained.
[0056] Furthermore, the positive electrode may also be associated with a support intended, as its name indicates, to support the aforementioned ingredients, this support being able, in addition, to contribute to ensuring good mechanical strength of the electrode and good electronic conduction (in which case it may be described as a current collector support).
[0057] This type of supported electrode can thus be described.
[0058] This support can be in the form of foam, a grid or even a plate and may be made of a material comprising a metal or a metal alloy or even a carbon material.
[0059] It may be, in particular, a titanium support, an aluminum support, a nickel support, a tantalum support or a stainless steel support, these supports being able to be in the form of sheets or grids.
[0060] The electrolyte intended to be used in the constitution of the electrochemical generators of the invention may be a liquid electrolyte comprising at least one organic solvent and at least one lithium salt.
[0061] More specifically, it may include:
[0062] -as solvent(s), one or more organic solvents chosen from carbonate solvents, ether solvents, amide solvents, sulfoxide solvents, lactone solvents, lactam solvents, nitrile solvents, ester solvents, sulfite solvents and mixtures thereof;
[0063] -at least one lithium salt; and
[0064] - possibly an additive other than a lithium salt.
[0065] As examples, the lithium salt may be selected from the group consisting of LiPF6, LiC104, LiBF4, LiAsF6, LiSbF6, LiAlCl4, LiGaCl4, LiCF3SO3, LiC(SO2CF3)3, lithium α(trifluoromethylsulfonyl)imide (known by the abbreviation LiTFSI) LiN[SO2CF3]2, LiSCN, lithium nitrate LiNO3, lithium α(oxalato)borate (known by the abbreviation LIBOB), lithium difluoro(oxalato)borate (known by the abbreviation LiDFOB), lithium α(fluorosulfonyl)imide (known by the abbreviation LiFSI), LiPF3(CF2CF3)3 (known by the abbreviation LiFAP), lithium trifluoromethanesulfonate LiCF3SO3 (known as LiTf), lithium fluorosulfonate LiSO3F, LiC6F5SO3, LiO3SCF2CF3, LiO2CCF3,LiB(C6H5)4 and mixtures thereof.
[0066] The lithium salt may be included in the electrolyte at a level of 0.1 M to 2 M, preferably 0.5 to 1.5 M.
[0067] As organic solvents belonging to the family of carbonate solvents, mention may be made of ethylene carbonate (known by the abbreviation EC), propylene carbonate (known by the abbreviation PC), dimethyl carbonate (known by the abbreviation DMC), diethyl carbonate (known by the abbreviation DEC), fluoroethylene carbonate (known by the abbreviation FEC) and mixtures thereof.
[0068] As organic solvents belonging to the family of ether solvents, mention may be made of tetrahydrofuran (known by the abbreviation THF), 1,2-dimethoxyethane (known by the abbreviation DME), diglyme, triglyme, tetraglyme or tetraethylene glycol dimethyl ether (known by the abbreviation TEGDME), methoxybenzene.
[0069] As organic solvent belonging to the family of amide solvents, mention may be made of dimethylformamide and dimethylacetamide.
[0070] As an organic solvent belonging to the family of sulfoxide solvents, we can cite dimethyl sulfoxide (known by the abbreviation DMSO).
[0071] As organic solvent belonging to the family of lactone solvents, mention may be made of γ-butyrolactone, γ-valerolactone, δ-valerolactone, ε-caprolactone, γ-caprolactone.
[0072] As an organic solvent belonging to the family of lactam solvents, mention may be made of N-methyl-2-pyrrolidone (known by the abbreviation NMP).
[0073] As an organic solvent belonging to the family of nitrile solvents, mention may be made of acetonitrile.
[0074] As an organic solvent belonging to the family of ester solvents, methyl acetate may be mentioned.
[0075] As an organic solvent belonging to the family of sulfite solvents, dimethyl sulfite may be mentioned.
[0076] The solvent may be used as a single solvent or as a mixture of separate solvents (thus forming a binary solvent or a ternary solvent).
[0077] For example, the solvent may consist of a mixture of several carbonate solvents, and more specifically a mixture of two carbonate solvents, a mixture meeting this specificity being the fluoroethylene carbonate / dimethyl carbonate mixture.
[0078] The aforementioned liquid electrolyte can be brought, in the electrochemical cell(s) of the electrochemical generators of the invention, to impregnate a separator, which is arranged between the positive electrode and the negative electrode of the electrochemical cell.
[0079] This separator may be made of a porous material capable of accommodating the liquid electrolyte in its porosity.
[0080] This separator may consist of a membrane made of a material selected from glass fibers (and more specifically, a nonwoven of glass fibers), a polymeric material, such as a polyethylene terephthalate (such as polyethylene terephthalate, known by the abbreviation PET), a polyolefin (for example, polyethylene, polypropylene), polyvinyl alcohol, polyamide, polytetrafluoroethylene (known by the abbreviation PTFE), polyvinyl chloride (known by the abbreviation PVC), polyvinylidene fluoride (known by the abbreviation PVDF). The separator may have a thickness ranging from 5 to 300 μm.
[0081] The electrolyte may also be an ionic liquid, for example, 1-methyl-1-propylpiperidinium bis(trifluoromethylsulfonyl)imide, 1-n-butyl-1-methylpyrrolidinium bis(trifluoromethylsulfonyl)imide and mixtures thereof.
[0082] The electrolyte may also consist of a solid electrolyte, for example, a lithium ion conductive ceramic membrane, conventionally called LISICON (corresponding to the English terminology Lithium Super Ion Conductor), this ceramic membrane can be of the perovskite type, such as (La,Li)TiO3 (known by the abbreviation LLTO), of the garnet type, such as Li5La3Ta20i2, Li6La3Zr20nj5, of the phosphate type, such as Lii+xAlxGe2 X(PO4)3 with 0 <x<0,8 (connu sous l’abréviation LAGP), Lii+xTi2 xAlx(PO4)3 avec 0,25<x<0,3 et Lii+x+yTi2xAlxSiy(PO4)3y avec 0,2<x<0,25 et 0<y<0,05(connu sous l’abréviation LTAP).
[0083] The electrolyte may also be a polymer electrolyte such as a polyethylene oxide membrane.
[0084] The electrochemical generators of the invention may be included in a rigid enclosure, for example, made of stainless steel, nickel-plated steel, aluminum or even titanium, or in a flexible enclosure.
[0085] The electrochemical generators of the invention can be adapted to different types of formats, such as the button cell type format, cylindrical formats, in particular, AAA, AA, C, D and DD formats; wound or spiral formats; prismatic format, pouch type format (known under the Anglo-Saxon name “pouch cell”).
[0086] An electrochemical generator specific to the invention is an electrochemical generator comprising at least one electrochemical cell comprising:
[0087] -a negative electrode consisting of a lithium and barium alloy sheet comprising a barium content of 2 atomic% or 10 atomic%;
[0088] -a positive electrode comprising a mixture comprising, as active material, LiNi0j6Mnoj2Co0j202;
[0089] -a porous separator disposed between said negative electrode and said positive electrode, said separator being impregnated with an electrolyte comprising a lithium salt LiPF6 in a mixture of carbonate solvents (for example, a binary mixture comprising fluoroethylene carbonate and dimethyl carbonate).
[0090] This electrochemical generator is a secondary electrochemical generator and can therefore be described as an accumulator.
[0091] The electrochemical generators of the invention can be produced by conventional techniques within the reach of those skilled in the art, for example, by stacking the different constituent elements of the electrochemical generator (namely, negative electrode, positive electrode and separator), this stack being able to be maintained in a housing. The alloy constituting the negative electrode can be produced by melting lithium and barium, for example, on a hot plate, at a temperature ranging from 145 to 400°C, under a neutral atmosphere (for example, an argon or nitrogen atmosphere) followed, after mixing, by quenching the molten mixture to quickly form the alloy. The alloy thus obtained can be put into the form of a plate or sheet by rolling in order to enter into the constitution of the negative electrode.
[0092] The invention will now be described in the following examples, given for informational purposes and without limitation. BRIEF DESCRIPTION OF THE FIGURES
[0093] [Fig. 1] is a graph illustrating the evolution of the average potential U (in V) as a function of the number of cycles N, curve a) being relative to the charge potential and curve b) being relative to the discharge potential, for the cell exemplified in example 2.
[0094] [Fig.2] is a graph representing the evolution of the potential U (in V) as a function of time T (in h), curve a) being relative to the first cell and curve b) being relative to the second cell of example 3.
[0095] [Fig.3] is a graph illustrating the evolution of the capacity C (in mAh / g) in function of the number of cycles N, curve a) being relative to the first cell and curve b) being relative to the second cell of example 3.
[0096] [Fig.4] is a graph illustrating the evolution of the potential U (in V) as a function of the duration T (in h) for the third cell of example 3.
[0097] [Fig.5] is a graph illustrating the evolution of the stress C (in MPa) as a function of the deformation D (in %) of example 4.
[0098] [Fig.6] is a graph illustrating the evolution of the potential E (in V) as a function of the time T (in h), curve a) being relative to the LiZn alloy, curve b) being relative to the LiZnBa alloy, curve c) being relative to the LiAl alloy, curve d) being relative to the LiAlBa alloy, curve e) being relative to the LiZn alloy and curve f) being relative to the LiZnBa alloy for example 4. DETAILED PRESENTATION OF IMPLEMENTATION METHODS EXAMPLE 1
[0099] The example below illustrates the synthesis of several materials consisting of an alloy of lithium and barium and the determination of their mechanical properties.
[0100] More specifically, a lithium and barium alloy comprising 2 atomic % of barium and a lithium and barium alloy comprising 10 atomic % of barium are prepared.
[0101] To do this, metallic lithium and metallic barium are melted on a hot plate under an argon atmosphere in the required proportions and, after mixing, the molten medium obtained is quenched to quickly form a solid material. At the end of these manipulations, balls of material are obtained, which cool very quickly once deposited on metal plates.
[0102] The balls of material obtained are easily laminated compared to pure lithium. and more easily compared to lithium and calcium alloys. In particular, they are easily rolled with hand rolling mills up to thicknesses of 20-25 μm and appear in the form of shiny films. EXAMPLE 2
[0103] The following example illustrates a solid electrolyte electrochemical cell according to the invention with the use of a lithium and barium alloy with a barium content of 2 atomic%.
[0104] This electrochemical cell is a cell in a so-called symmetrical electrode configuration, in order to test the operation of an electrode made of an alloy of lithium and barium with a barium content of 2 atomic%, the cell being in the form of a flexible bag with electrodes with a surface area of 10 cm2 and the solid electrolyte being in the form of a polyethylene oxide (PEO) membrane, mainly of the Osaka Soda brand.
[0105] This cell is subjected to an average charged / discharged current of 0.3 mA / cm2 for an exchanged capacity of 1 mAh / cm2, the test being carried out at 60°C to allow the operation of the ion exchange membrane.
[0106] The results are reported in [Fig. 1] illustrating the evolution of the average potential U (in V) as a function of the number of cycles N, curve a) being relative to the charge potential and curve b) being relative to the discharge potential. As long as the average potential is stable and greater than 0.1 V, this denotes good functioning of the cell, unlike where the potential drops drastically and denotes a malfunction. In our case, the test demonstrates a durability of 15 cycles before malfunction, which is sufficient to demonstrate the good functioning of the alloy used for the constitution of the electrodes. EXAMPLE 3
[0107] The following example illustrates a liquid electrolyte electrochemical cell according to the invention (hereinafter referred to as the first cell or BaLi in Table 1 below) with the use of a lithium and barium alloy with a barium content of 2 atomic%, this cell comprising:
[0108] - a negative electrode consisting of a disc 14 mm in diameter and composed of an alloy of lithium and barium with a barium content of 2 atomic%, said electrode having a thickness of 100 pm and a surface area of 1.54 cm2;
[0109] -a positive electrode consisting of a disc 16 mm in diameter, said electrode being composed of a layer comprising LiNio>6Mnoj2Cooj202 (90.5% by mass), polyvinylidene fluoride (5% by mass) and Super P® carbon black (4.5% by mass), this layer being deposited on an aluminum foil having a thickness of 20 μm and the weight of LiNio,6Mno,2Coo,202 being approximately 25 mg / cm2, or a battery capacity of approximately 4 mAh / cm2;
[0110] - between the negative electrode and the positive electrode, a separator of the Celgard 2400® type in the form of a disc 16.5 mm in diameter and with a surface area of 2 cm2, said separator being impregnated with an electrolyte consisting of a mixture of carbonate solvents (fluoroethylene carbonate / dimethyl carbonate) in respective volume proportions of 20 / 80 and a lithium salt LiPF6 IM.
[0111] Another cell not in accordance with the invention (hereinafter referred to as the second cell or Li in Table 1 below) was produced in parallel, this second cell meeting the same specifications as the first cell, except that the lithium and barium alloy was replaced by pure lithium.
[0112] First, these two cells are electrochemically formed at 60°C during a formation cycle at C / 10 and D / 10. This allows the correct operation of the electrodes to be validated. Table 1 below represents the result of this formation.
[0113] [Tables 1] Cell Charging capacity (mAh) Discharging capacity (mAh) Charging energy (mWh) Discharging energy (mWh) Reversibility (%) Irreversibility (%) BaLi 7.2 6.9 28.0 26.2 95.4 4.6 Li 7.0 6.6 26.9 25.1 94.5 5.5
[0114] [Fig.2] illustrates the result of this training cycle via a graph representing the evolution of the potential U (in V) as a function of time T (in h), curve a) being relative to the first cell and curve b) being relative to the second cell.
[0115] In the figure, the two curves are superimposed, which shows that the use of an alloy does not disrupt the cell voltage during the test. Furthermore, the superposition also shows that the positive electrode is used in the same way. The use of the alloy therefore does not hinder the overall operation of the cell at all.
[0116] Furthermore, from the table, it can be seen that the two cells are very homogeneous, as can be seen in the figure. Thus, this confirms the possibility of using a lithium and barium alloy in battery technologies without altering the operation of the cells.
[0117] The two cells are then placed in simple cycling at room temperature to check the operation at this temperature of the alloy. The result of this cycling is shown in [Fig.3], which is a graph illustrating the evolution of the capacity C (in mAh / g) as a function of the number of cycles N, curve a) being relative to the first cell and curve b) being relative to the second cell.
[0118] In this figure, we can once again see the homogeneity of the results between the first cell and the second cell. This demonstrates that at room temperature, there is also no difference in operation between these two electrodes. Furthermore, in this specific example, the cell containing the alloy exhibits a later operating fault than the cell operating with pure lithium.
[0119] A final test was carried out with a cell similar to the first cell, except that the negative electrode is now an electrode composed of an alloy of lithium and barium with a barium content of 10 atomic% (called the third cell), said third cell being subjected to formation and cycling at room temperature (23°C) during a formation cycle at C / 10 and D / 10. Similar data are obtained in formation compared to the first cell.
[0120] [Fig.4] represents the evolution of the potential U (in V) as a function of the duration T (in h).
[0121] It appears that this cell also operates very correctly at a potential identical to a cell containing metallic lithium. This demonstrates the correct operation of a cell comprising, as negative electrode, an electrode made of a lithium and barium alloy with 10 atomic% barium. EXAMPLE 4
[0122] The present example illustrates the synthesis of several materials consisting of a ternary alloy of lithium, barium and another metallic element, these materials having been obtained by the synthesis technique in a molten bath. For this, the desired quantity of lithium metal and the elements to be associated is introduced and heated to 400°C. The bath is then stirred to absorb the elements to be associated with the lithium metal.
[0123] The materials prepared are as follows:
[0124] -a first series of aluminum-based materials with a lithium-aluminum alloy material comprising 2 atomic% aluminum and a lithium-aluminum-barium alloy material comprising 2 atomic% aluminum and 2 atomic% barium;
[0125] -a second series of indium-based materials with a lithium-indium alloy material comprising 2 atomic% indium and a lithium-indium-barium alloy material comprising 2 atomic% indium and 2 atomic% barium;
[0126] -a third series of zinc-based materials with a lithium-zinc alloy material comprising 2 atomic% zinc and a lithium-zinc-barium alloy material comprising 2 atomic% zinc and 2 atomic% barium.
[0127] These different materials could be rolled down to 30-50 micrometers. However, alloys without barium prove to be more difficult to handle, because they stick to the rolling mill in the event of excessive stresses, making it difficult to obtain lower thicknesses. Thus, the addition of barium is advantageous for obtaining parts with a low thickness.
[0128] These different materials were then subjected to tensile tests in the form of 100 μm thick test pieces, the different test pieces having been preconditioned according to the same operating procedure and then stretched at 2 mm / minute. The results obtained were then processed to obtain a representation of the stress undergone as a function of the deformation, this representation being illustrated by [Fig.5], which is a graph illustrating the evolution of the stress C (in MPa) as a function of the deformation D (in %), curve a) being relative to a metallic lithium specimen, curve b) being relative to the lithium and zinc alloy specimen, curve c) being relative to the lithium, zinc and barium alloy specimen, curve d) being relative to the lithium and aluminium alloy specimen, curve e) being relative to the lithium, aluminium and barium alloy specimen, curve f) being relative to the lithium and indium alloy specimen and curve g) being relative to the lithium, indium and barium alloy specimen.
[0129] It appears that the transition from binary LiX alloys at 2 atomic% to ternary LiXBa alloys at 2 atomic% in X (X being zinc, aluminum or indium) and in Ba made it possible, in all cases, to gain on the deformation / stress couple in the context of our tensile manipulation. This demonstrates the usefulness of adding barium in all these compositions to improve the rolling step.
[0130] Finally, in order to validate the possible use of these alloys in electrochemistry, these different alloys were tested in symmetrical button cells (namely, with two negative electrodes made of said alloys) comprising a polyethylene oxide membrane and an electrolyte based on a LiTFSI salt, the different button cells having been subjected to three charge-discharge cycles under a regime of 0.1mA / cm2 and a capacity of 1 mAh / cm2.
[0131] The results are reported in [Fig.6], which illustrates the evolution of the potential E (in V) as a function of time T (in h), curve a) being relative to the LiZn alloy, curve b) being relative to the LiZnBa alloy, curve c) being relative to the LiAl alloy, curve d) being relative to the LiAlBa alloy, curve e) being relative to the Liln alloy and curve f) being relative to the LilnBa alloy.
[0132] In all cases, binary alloys have a slightly lower exchange plateau voltage than ternary alloys. Thus, ternary alloys probably have a slightly greater interface resistance than binary alloys. Nevertheless, the cell voltage performance is sufficiently analogues so that this does not compromise the use of ternary alloys in batteries.
Claims
Claims
1. Negative electrode for a lithium electrochemical generator characterized in that it comprises, as active material, an alloy comprising, in addition to lithium and barium, a third element chosen from magnesium, zinc, indium, calcium, gallium and aluminum, the barium being present in the alloy at a level of at most 20 atomic%.
2. A negative electrode according to claim 1, wherein, for the alloy comprising lithium and barium, the barium is present in the alloy at a level of 2 to 20 atomic %.
3. A negative electrode according to claim 1 or 2, wherein, for the alloy comprising lithium and barium, the barium is present in the alloy at a level of 2 to 10 atomic %.
4. A negative electrode according to any preceding claim, which consists solely of the active material, which is the alloy comprising lithium and barium.
5. A negative electrode according to any preceding claim, wherein the third element is present in a content of from 2 to 20 atomic% and preferably from 2 to 10 atomic%.
6. A negative electrode according to any preceding claim, which is in the form of a sheet or plate having a thickness of 5 to 50 µm.
7. A negative electrode according to any preceding claim, which is self-supporting.
8. Electrochemical generator comprising at least one electrochemical cell comprising a positive electrode comprising, as active material, a lithium insertion material; a negative electrode and a lithium ion conductive electrolyte disposed between said negative electrode and said positive electrode, characterized in that the negative electrode is as defined according to any one of claims 1 to 7.
9. Electrochemical generator according to claim 8, in which the lithium insertion material is chosen from lithiated oxides comprising at least one transition metal element, lithiated phosphates comprising at least one transition metal element, manganese dioxide and mixtures thereof.
10. An electrochemical generator according to claim 9, wherein the lithium oxide comprising at least one transition metal element is an oxide of the following formula: LiMO2 in which M is an element chosen from Ni, Co, Mn, Al, Mg and mixtures thereof.
11. Electrochemical generator according to any one of claims 8 to 10, wherein the positive electrode comprises at least one electronically conductive additive and / or at least one binder.
12. An electrochemical generator according to claim 11, wherein the binder is a polymeric binder.
13. Electrochemical generator according to any one of claims 8 to 12, in which the lithium ion conductive electrolyte is a liquid electrolyte comprising at least one organic solvent and at least one lithium salt.