Adhesive composition for wood, adhesive kit for wood, method for manufacturing woody material, and woody material
A wood adhesive composition combining resol type phenolic resin, an amine compound, and an organic acid ester addresses the issue of increased formaldehyde emission in wood materials, achieving reduced emissions even with accelerated manufacturing processes.
Patent Information
- Application Number
- JP2023045345
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-22
- Publication Date
- 2024-10-04
AI Technical Summary
Adhesives containing resol type phenolic resin and organic acid esters, while offering improved curing properties, result in increased formaldehyde emission when used for manufacturing wood materials under reduced time or temperature conditions.
A wood adhesive composition combining resol type phenolic resin, an amine compound with a hydrogen atom bonded to a nitrogen atom, and an organic acid ester, along with optional resorcinol, to reduce formaldehyde emission.
The composition enables the production of wood materials with reduced formaldehyde emission even when manufactured under hot or cold pressure in a short time or at low temperatures.
Smart Images

Figure 2024134905000002 
Figure 2024134905000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a wood adhesive composition, a wood adhesive kit, a method for producing a wood material, and a wood material. [Background technology]
[0002] 2. Description of the Related Art Adhesives containing resol-type phenolic resins (alkali phenolic resins) have been conventionally known as adhesives for bonding pieces of wood together to produce wood materials. In order to enhance the curing property of the resol type phenolic resin, a curing accelerator may be blended into the adhesive containing the resol type phenolic resin. Known examples of the curing accelerator include organic acid esters (Patent Document 1).
[0003] On the other hand, in the process of producing cellulose products using a thermosetting composition containing a resol-type phenolic resin, it has been proposed to incorporate an amine into the thermosetting composition in order to prevent free aldehydes in the resol-type phenolic resin from volatilizing and generating harmful odors (Patent Document 2). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 7076049 [Patent Document 2] JP 2022-153295 A Summary of the Invention [Problem to be solved by the invention]
[0005] An adhesive containing a resol-type phenolic resin and an organic acid ester as described in Patent Document 1 has excellent curing properties, and is said to be able to obtain sufficient adhesive strength by hot pressing or cold pressing in a shorter time or at a lower temperature than conventional methods. However, when such an adhesive is used to produce a wood material by hot pressing or cold pressing in a shorter time or at a lower temperature than conventional methods, the amount of formaldehyde emitted from the resulting wood material (formaldehyde emission amount) increases. Patent Document 2 does not consider reducing the amount of formaldehyde emitted.
[0006] The present invention aims to provide a wood adhesive composition, a wood adhesive kit, and a method for producing a wood material, which can produce a wood material with low formaldehyde emissions even when the wood material is produced by hot-pressing or cold-pressing for a short time or at a low temperature, as well as a wood material with low formaldehyde emissions even when the wood material is produced by hot-pressing or cold-pressing for a short time or at a low temperature. [Means for solving the problem]
[0007] As a result of extensive investigations, the present inventors have found that the above problems can be solved by combining a resol-type phenolic resin, an organic acid ester, and a specific amine compound, and have thus completed the present invention.
[0008] The present invention has the following aspects. [1] A wood adhesive composition comprising a resol-type phenolic resin, an amine compound having a hydrogen atom bonded to a nitrogen atom, and an organic acid ester. [2] The adhesive composition for wood according to [1], wherein the amine compound has at least one type selected from the group consisting of a primary amino group and a secondary amino group. [3] The wood adhesive composition according to [1] or [2], wherein the content of the amine compound is 0.1 to 10.0 parts by mass per 100 parts by mass of the solid content of the resol type phenolic resin. [4] The adhesive composition for wood according to any one of [1] to [3], wherein the resol type phenolic resin has a pH of 7 to 14. [5] The wood adhesive composition according to any one of [1] to [4], wherein the content of the organic acid ester is 1.0 to 40.0 parts by mass per 100 parts by mass of the resol type phenolic resin and the amine compound combined. [6] The adhesive composition for wood according to any one of [1] to [5], further comprising resorcinol. [7] The wood adhesive composition according to [6], wherein the content of the resorcinol is 0.5 to 20.0 parts by mass per 100 parts by mass of the resol type phenolic resin and the amine compound combined. [8] A first container containing a first agent including a resol type phenolic resin and an amine compound having a hydrogen atom bonded to a nitrogen atom; a second container containing a second agent including an organic acid ester; A wood adhesive kit comprising: [9] The wood adhesive kit according to [8], wherein the amine compound has at least one selected from the group consisting of a primary amino group and a secondary amino group.
[10] The wood adhesive kit according to [8] or [9], wherein the content of the amine compound is 0.1 to 10.0 parts by mass per 100 parts by mass of the solid content of the resol type phenolic resin.
[11] The wood adhesive kit according to any one of [8] to
[10] , wherein the first agent has a pH of 7 to 14.
[12] The wood adhesive kit according to any one of [8] to
[11] , wherein the content of the organic acid ester is 1.0 to 40.0 parts by mass per 100 parts by mass of the resol type phenolic resin and the amine compound combined.
[13] The wood adhesive kit according to any one of [8] to
[12] , wherein the second agent further contains resorcinol.
[14] The wood adhesive kit according to
[13] , wherein the content of the resorcinol is 0.5 to 20.0 parts by mass per 100 parts by mass of the resol type phenolic resin and the amine compound combined.
[15] A process for preparing a wood adhesive composition by mixing raw materials including a resol-type phenolic resin, an amine compound having a hydrogen atom bonded to a nitrogen atom, and an organic acid ester; A step of stacking a plurality of pieces of wood with the wood adhesive composition interposed therebetween to obtain a laminate; curing the wood adhesive composition in the laminate; A method for producing a wood material having the above structure.
[16] The method for producing a wood material according to
[15] , wherein the amine compound has at least one type selected from the group consisting of a primary amino group and a secondary amino group.
[17] The method for producing a wood material according to
[15] or
[16] , wherein the content of the amine compound is 0.1 to 10.0 parts by mass per 100 parts by mass of the solid content of the resol type phenolic resin.
[18] The method for producing a woody material according to any one of
[15] to
[17] , wherein the resol type phenolic resin has a pH of 7 to 14.
[19] A method for producing a wood material according to any one of
[15] to
[18] , wherein the content of the organic acid ester is 1.0 to 40.0 parts by mass per 100 parts by mass of the resol type phenolic resin and the amine compound combined.
[20] The method for producing a woody material according to any one of
[15] to
[19] , wherein the raw material further contains resorcinol.
[21] The method for producing a wood material according to
[20] , wherein the content of the resorcinol is 0.5 to 20.0 parts by mass per 100 parts by mass of the resol type phenolic resin and the amine compound combined.
[22] A wood material in which a plurality of pieces of wood are bonded together via a cured product of the wood adhesive composition according to any one of [1] to [7].
[23] The wood material according to
[22] , which is plywood. Effect of the Invention
[0009] The present invention provides a wood adhesive composition, a wood adhesive kit, and a method for producing a wood material that can produce a wood material with low formaldehyde emissions even when the wood material is produced by hot-pressing or cold-pressing in a short time or at a low temperature, as well as a wood material with low formaldehyde emissions even when the wood material is produced by hot-pressing or cold-pressing in a short time or at a low temperature. [Brief description of the drawings]
[0010] [Figure 1] 1 is a graph showing the results of Test Example 1 (horizontal axis: amount of MEA added, vertical axis: amount of formaldehyde emitted). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] In the present invention, pH is the value at 25° C. unless otherwise specified. The viscosity is a value measured at 25°C using an E-type viscometer. The weight average molecular weight (hereinafter also referred to as "Mw") of a phenolic resin (a resol type phenolic resin or a novolac type phenolic resin) is a polystyrene-equivalent value measured by gel permeation chromatography (hereinafter also referred to as "GPC"). The solid content is the non-volatile content. The non-volatile content is the residue when 1.5 g of a sample is heated at 135°C for 1 hour. The specific method for measuring the solid content (non-volatile content) of a sample is shown below. Weigh out the mass C1 (g) of an aluminum foil dish (inner diameter 50 mm, height 15 mm), weigh out the sample so that it is 1.5±0.1 g, and the specific mass of the sample is the sample mass S (g) before drying. Place this aluminum foil dish in a thermostat previously kept at 135±1°C, dry for 60±2 minutes, then cool in a desiccator, and weigh its mass C2 (g). From the results, calculate the sample mass D (mass of the sample remaining on the aluminum foil dish after drying) (g) after drying using the following formula (1), and calculate the solids concentration using the following formula (2). D = C2 - C1 (1) Solid content concentration (mass%)=D / S×100 (2)
[0012] [Wood Adhesive Composition] A wood adhesive composition according to one embodiment of the present invention (hereinafter also referred to as "the composition") contains a resol-type phenolic resin, an amine compound having a hydrogen atom bonded to a nitrogen atom, and an organic acid ester. The composition may further include resorcinol. The present composition may further contain other components other than the resol type phenolic resin, the amine compound, the organic acid ester and resorcinol, if necessary.
[0013] <Resol-type phenolic resin> The resol type phenolic resin is also called an alkaline phenolic resin, and typically contains an addition condensation product (phenol condensation product) of a phenol with an aldehyde, an alkaline substance, and water. At least a part of the alkaline substance is usually an alkaline catalyst used in the production of the resol type phenolic resin. The alkaline catalyst may be neutralized.
[0014] The pH of the resol type phenolic resin is preferably 7 to 14, more preferably 8 to 14, and even more preferably 10 to 14. If the pH is equal to or higher than the lower limit, the organic acid ester is easily hydrolyzed when mixed with the organic acid ester, and the hardening acceleration effect of the organic acid ester is easily obtained. If the pH is equal to or lower than the upper limit, the hardening acceleration effect of the organic acid generated by the hydrolysis of the organic acid ester is easily obtained.
[0015] The viscosity of the resol type phenolic resin is preferably 10 to 20,000 mPa·s, more preferably 100 to 15,000 mPa·s, and even more preferably 1,000 to 10,000 mPa·s. If the viscosity of the resol type phenolic resin is equal to or higher than the lower limit, the resin is less likely to drip from the bonding surface when applied to wood and when bonding wood, and if the viscosity is equal to or lower than the upper limit, the resin has excellent coatability in bonding wood materials.
[0016] The solid content of the resol type phenolic resin is preferably 30 to 70 mass%, more preferably 40 to 60 mass%, and further preferably 45 to 55 mass%. When the solid content of the resol type phenolic resin is within the above range, the viscosity of the resol type phenolic resin is easily adjusted to the above-mentioned preferred range.
[0017] Phenols are compounds having an aromatic ring and a hydroxyl group bonded to the aromatic ring. Phenols may be compounds known as monomers of phenolic resins, such as phenol, alkylphenols (o, m, p cresols, o, m, p ethylphenols, xylenol isomers, etc.), polyaromatic ring phenols (α, β naphthols, etc.), polyhydric phenols (bisphenol A, bisphenol F, bisphenol S, pyrogallol, resorcinol, catechol, hydroquinone, etc.). These phenols may be used alone or in combination of two or more. From the viewpoint of storage stability of the resol type phenolic resin, phenols other than resorcinol are preferable. Practical phenols other than resorcinol include phenol, o-, m- and p-cresol isomers, and xylenol isomers.
[0018] The aldehydes are at least one compound selected from the group consisting of compounds having a formyl group and their polymers, and examples thereof include formaldehyde, paraformaldehyde, acetaldehyde, propylaldehyde, benzaldehyde, salicylaldehyde, glyoxal, etc. These aldehydes may be used alone or in combination of two or more. Among these, the practical substances are formaldehyde and paraformaldehyde.
[0019] The alkali catalyst is not particularly limited as long as it can promote the addition condensation reaction, and various alkaline substances can be used. Specific examples include inorganic alkaline substances such as hydroxides of alkali metals such as sodium and potassium (sodium hydroxide, potassium hydroxide, etc.), oxides and hydroxides of alkaline earth metals such as calcium, magnesium, barium, etc., sodium carbonate, and ammonia; organic alkaline substances such as tertiary amines such as triethylamine and trimethylamine, and cyclic amines such as DBU (1,8-diazabicyclo[5.4.0]undec-7-ene) and DBN (1,5-diazabicyclo[4.3.0]non-5-ene); and the like. These alkali catalysts may be used alone or in combination of two or more.
[0020] An example of the resol type phenolic resin is a resol type novolac phenolic resin (hereinafter also referred to as "phenolic resin (1)"). Specifically, the phenol resin (1) is a reaction product (secondary reaction, resol-type reaction) between a novolak-type phenol resin and an aldehyde in the presence of an alkali catalyst, and is also called a secondary reaction resol-type phenol resin. Phenolic resin (1) has excellent curing properties in the presence of organic acid esters compared to resol-type phenolic resins obtained by reacting phenols with aldehydes only in the presence of an alkaline catalyst, and can be sufficiently cured even by cold pressing or by hot pressing at a relatively low temperature. Therefore, it is suitable for use in wood applications.
[0021] Novolac-type phenolic resins are the products of a reaction (primary reaction, novolac-type reaction) between phenols and aldehydes in the presence of an acid catalyst. Novolac-type phenolic resins contain phenol condensates in which aromatic rings of two or more phenols are bonded together via methylene groups derived from aldehydes. In the secondary reaction, aldehydes are added to the aromatic rings of the phenol condensates to generate methylol groups, and some of the generated methylol groups react with other phenol condensates to increase the molecular weight. Therefore, the phenolic resin (1) contains phenol condensates that have methylol groups and have a higher molecular weight than the phenol condensates contained in the novolac-type phenolic resins.
[0022] The acid catalyst used in the primary reaction is not particularly limited as long as it allows the primary reaction to proceed, and examples thereof include inorganic acids such as hydrochloric acid, sulfuric acid, phosphoric acid, etc., organic acids such as oxalic acid, acetic acid, citric acid, tartaric acid, benzoic acid, paratoluenesulfonic acid, etc., and organic acid salts such as zinc acetate, zinc borate, etc. These acid catalysts may be used alone or in combination of two or more.
[0023] The amount of the acid catalyst used is preferably 0.05 to 2.0 parts by mass, more preferably 0.1 to 1.0 parts by mass, based on 100 parts by mass of the phenols. When the amount of the acid catalyst used is equal to or more than the lower limit, a sufficient reaction rate can be obtained, and when the amount is equal to or less than the upper limit, the reaction can be easily controlled. In this specification, the preferred upper and lower limits can be appropriately combined. For example, the amount of the acid catalyst used may be 0.05 to 1.0 part by mass or 0.1 to 1.0 part by mass relative to 100 parts by mass of the phenols.
[0024] The molar ratio of aldehydes / phenols in the novolak phenolic resin (hereinafter also referred to as "F / P molar ratio") is preferably 0.6 to 0.9, more preferably 0.7 to 0.8. When the F / P molar ratio in the novolak phenolic resin is equal to or higher than the lower limit, the amount of aldehydes during the resol reaction (secondary reaction) can be reduced, and heat generation during the reaction can be suppressed. When the F / P molar ratio is equal to or lower than the upper limit, gelation during the novolak reaction (primary reaction) can be suppressed.
[0025] The Mw of the novolac phenolic resin is preferably from 1,000 to 8,000, more preferably from 1,500 to 6,000. When the Mw of the novolac phenolic resin is within the above range, the Mw of the phenolic resin (1) tends to fall within the preferred range described below.
[0026] The alkali catalyst used in the secondary reaction may be the same as those mentioned above. The preferred amount of the alkali catalyst used is determined by the molar ratio of alkali catalyst / phenols (hereinafter also referred to as "alkali / P molar ratio"). The alkali / P molar ratio is preferably 0.1 to 1.0, more preferably 0.2 to 0.9, and further preferably 0.5 to 0.8. When the alkali / P molar ratio is equal to or more than the lower limit, the phenol resin (1) can be obtained quickly, and when it is equal to or less than the upper limit, the secondary reaction can be easily controlled.
[0027] The F / P molar ratio in the phenol resin (1) is preferably from 2.0 to 2.8, more preferably from 2.0 to 2.6, and even more preferably from 2.0 to 2.4. Here, the F / P molar ratio in the phenolic resin (1) is the molar ratio of the total amount of aldehydes used in the first and second reactions to the phenols used in the first reaction. Hereinafter, this molar ratio is also referred to as the "final F / P molar ratio." If the final F / P molar ratio is equal to or greater than the lower limit, there will be a sufficient amount of methylol groups in the phenolic resin (1), resulting in superior adhesive strength between wood pieces. If the final F / P molar ratio is equal to or less than the upper limit, the amount of free aldehydes volatilized during the production of wood materials and the amount of formaldehyde emitted from wood materials will be reduced. Free aldehydes are unreacted aldehydes.
[0028] The weight average molecular weight (Mw) of the phenolic resin (1) is preferably 2,000 to 10,000, more preferably 3,000 to 10,000, even more preferably 3,000 to 8,000, particularly preferably 3,500 to 8,000, and most preferably 3,500 to 7,000. When the weight average molecular weight of the phenolic resin (1) is equal to or higher than the lower limit, the adhesive strength between wood pieces tends to be superior, and when it is equal to or lower than the upper limit, the viscosity of the composition tends to be lower, and the coatability tends to be improved.
[0029] At least a part of the alkaline substance contained in the phenol resin (1) is usually an alkaline catalyst used in the secondary reaction. A part of the alkaline substance may be added after the secondary reaction.
[0030] The molar ratio of alkaline substance / phenols in the phenol resin (1) is preferably from 0.1 to 1.0, more preferably from 0.2 to 0.9, and even more preferably from 0.5 to 0.8. Here, the molar ratio of alkaline substance / phenols in the phenolic resin (1) is the molar ratio of the total amount of the alkaline catalyst used in the secondary reaction and the alkaline substance added after the secondary reaction to the total amount of the phenols used in the primary reaction. Hereinafter, this molar ratio is also referred to as the "final alkaline substance / phenols molar ratio." When no alkaline substance is added after the secondary reaction, the total amount of the alkaline catalyst used in the secondary reaction and the alkaline substance added after the secondary reaction is the amount of the alkaline catalyst used in the secondary reaction. When the final alkaline substance / phenols molar ratio is equal to or greater than the lower limit, the amount of free aldehydes in the phenol resin (1) can be reduced without causing a significant increase in molecular weight (without increasing viscosity), whereas when the final alkaline substance / phenols molar ratio is equal to or less than the upper limit, a sufficient reaction rate can be obtained and control is easy.
[0031] The phenol resin (1) can be produced, for example, by the method described in JP 2018-53131 A.
[0032] As the resol type phenolic resin, a reaction product of a phenol with an aldehyde in the presence of an alkali catalyst (hereinafter, also referred to as "phenolic resin (2)") may be used. The phenolic resin (2) is obtained by reacting a phenol with an aldehyde in the presence of an alkali catalyst. The phenol, aldehyde, and alkali catalyst are the same as those described above. The reaction product can be produced by a known method.
[0033] The preferred amount of the alkali catalyst used when reacting a phenol with an aldehyde in the presence of the alkali catalyst is determined by the molar ratio of alkali catalyst / phenol (hereinafter also referred to as "alkali / P molar ratio"). The alkali / P molar ratio is preferably 0.1 to 1.0, more preferably 0.2 to 0.9, and further preferably 0.5 to 0.8. When the alkali / P molar ratio is equal to or more than the lower limit, the phenol resin (2) can be obtained quickly, and when it is equal to or less than the upper limit, the resol reaction can be easily controlled.
[0034] The F / P molar ratio in the phenolic resin (2) is preferably 1.5 to 3.5, more preferably 2.0 to 3.0, and even more preferably 2.0 to 2.4. If the F / P molar ratio is equal to or greater than the lower limit, a sufficient amount of methylol groups is present in the phenolic resin (2), resulting in superior adhesive strength between wood pieces. If the molar ratio is equal to or less than the upper limit, the amount of free aldehydes volatilized during the production of wood materials and the amount of formaldehyde emitted from wood materials are reduced.
[0035] The weight average molecular weight (Mw) of the phenolic resin (2) is preferably 1,000 to 10,000, more preferably 1,500 to 10,000, even more preferably 2,000 to 8,000, particularly preferably 2,000 to 7,500, and most preferably 2,000 to 7,000. When the weight average molecular weight of the phenolic resin (2) is equal to or higher than the lower limit, the adhesive strength between wood pieces tends to be superior, and when it is equal to or lower than the upper limit, the viscosity of the composition tends to be lower and the coatability tends to be improved.
[0036] <Amine compounds> In the present invention, the term "amine compound" means a compound having a nitrogen atom and a hydrocarbon group bonded to the nitrogen atom. In this embodiment, the amine compound has a hydrogen atom bonded to a nitrogen atom. Such an amine compound is excellent in reducing the amount of formaldehyde emitted from wood materials. The reason for this is believed to be that the nitrogen atom bonded to a hydrogen atom reacts with formaldehyde. Examples of the amine compound having a hydrogen atom bonded to a nitrogen atom include amine compounds having at least one type selected from the group consisting of a primary amino group and a secondary amino group.
[0037] The amine compound may be either linear or cyclic. The amine compound may be a monoamine compound having one nitrogen atom, or a polyamine compound having two or more nitrogen atoms. The number of nitrogen atoms in the polyamine compound is not particularly limited, but is, for example, 2 to 6. The hydrocarbon group bonded to the nitrogen atom may be a saturated or unsaturated hydrocarbon group, and may be either linear or cyclic.
[0038] From the viewpoint of easily obtaining the effect of reducing the amount of formaldehyde emitted from wood materials, the molecular weight of the amine compound is preferably 1000 or less, more preferably 500 or less, and even more preferably 100 or less. The lower limit of the molecular weight of the amine compound is not particularly limited, but is, for example, 31.1 (monomethylamine). The value obtained by dividing the molecular weight of the amine compound by the number of nitrogen atoms to which hydrogen atoms are bonded (molecular weight / number of nitrogen atoms to which hydrogen atoms are bonded) is preferably 1000 or less, more preferably 500 or less, and even more preferably 100 or less, in order to easily obtain the effect of reducing the amount of formaldehyde emitted. The lower limit of this value is not particularly limited, but is, for example, 31.1 (monomethylamine).
[0039] Examples of the amine compound include an aliphatic amine compound, an alicyclic amine compound, an aromatic amine compound, and an amine derivative. Examples of the aliphatic amine compound include (mono- or di-)alkanolamines and (mono- or di-)alkylamines. (Mono- or di-)alkanolamines refer to monoalkanolamines or dialkanolamines. The same applies to (mono- or di-)alkylamines. Examples of (mono- or di-)alkanolamines include (mono- or di-)ethanolamines and (mono- or di-)isopropanolamines. Examples of (mono- or di-)alkylamines include (mono- or di-)methylamines, (mono- or di-)ethylamines, ethylenediamines, diethylenetriamines, triethylenetetramines, tetraethylenepentamines, pentaethylenehexamines, hexamethylenediamines, and tetramethylethylenediamines. Examples of the alicyclic amine compound include piperidine, piperazine, pyrrolidine, morpholine, pyrrole, pyrazole, and imidazole. Examples of the aromatic amine compound include aniline, aminophenol, and toluidine. Examples of the amine derivatives include ether amines and amino acids. Examples of the amino acids include glycine, glutamine, and glutamic acid.
[0040] As the amine compound, from the viewpoint of easily obtaining the effect of reducing the amount of formaldehyde emitted from wood materials, a monoamine compound having a primary amino group or a secondary amino group is preferred, an aliphatic monoamine compound having a primary amino group or a secondary amino group is more preferred, a (mono- or di)alkanolamine is further preferred, and monoethanolamine is particularly preferred. The amine compounds may be used alone or in combination of two or more kinds.
[0041] <Organic acid ester> The organic acid ester functions as a curing accelerator. When cold or hot pressure is applied, the organic acid ester is hydrolyzed to generate an organic acid, which lowers the pH of the composition, accelerating the curing reaction.
[0042] Examples of organic acid esters include carbonates such as ethylene carbonate, propylene carbonate, and dimethyl carbonate; lactones such as γ-butyrolactone, α-acetolactone, and β-propiolactone; monocarboxylates such as triacetin, ethylene glycol diacetate, triethylene glycol diacetate, ethyl acetate, methyl butyrate, ethyl butyrate, ethyl formate, methyl salicylate, and ethyl acetoacetate; and dicarboxylate monoesters or dicarboxylate diesters such as dimethyl succinate, diethyl succinate, dimethyl adipate, diethyl adipate, dimethyl glutarate, diethyl glutarate, and diethyl malonate. These organic acid esters may be used alone or in combination of two or more.
[0043] As the organic acid ester, among the above, at least one selected from the group consisting of carbonate ester, lactone and polyol carboxylate is preferred in terms of superior low-temperature curing property and relatively high boiling point, and at least one selected from the group consisting of ethylene carbonate, propylene carbonate, dimethyl carbonate, γ-butyrolactone, α-acetolactone, β-propiolactone, triacetin and ethylene glycol diacetate is more preferred. Among these, at least one selected from the group consisting of propylene carbonate, γ-butyrolactone, triacetin and ethylene glycol diacetate is preferred in terms of obtaining a curing acceleration effect with a smaller amount. If necessary, organic acid esters other than these may be used in combination.
[0044] <Other ingredients> Examples of other ingredients include carbohydrates and various other additives.
[0045] When the present composition contains carbohydrates, particularly reducing sugars, it is possible to reduce the amount of free aldehydes that volatilize during the production of wood materials, to reduce the amount of formaldehyde emitted from the wood materials, and to lighten the color of the cured product. The reducing sugar is not particularly limited and may be, for example, monosaccharide, oligosaccharide, dextrin, etc. Here, "oligosaccharide" refers to a combination of 2 to 10 monosaccharides, and "dextrin" includes the concept of general maltodextrin and refers to a sugar composition with a DE of 20 or less. Examples of monosaccharides include glucose, fructose, mannose, galactose, ribose, and xylose. Examples of oligosaccharides include disaccharides such as maltose, lactose, isomaltose, etc.; trisaccharides such as maltotriose, etc.; and tetrasaccharides or higher oligosaccharides (for example, maltooligosaccharides, isomaltooligosaccharides, fructooligosaccharides, mannooligosaccharides, galactooligosaccharides, etc.). These reducing sugars may be used alone or in combination of two or more.
[0046] As the additive, any of the known components constituting the adhesive composition for wood can be appropriately used. Examples of the additive include a hardening accelerator other than the organic acid ester, a thickener, an extender, a viscosity adjuster, etc. Other hardening accelerators include, for example, alkali metal carbonates such as sodium carbonate, sodium bicarbonate, potassium carbonate, and potassium bicarbonate. Thickeners include, for example, polysaccharides such as wheat flour. Examples of the bulking agent include alkaline earth metal salts such as calcium carbonate. Other bulking agents include organic fillers such as wood flour, walnut flour, lignin, tannin, blood meal, and the like. Examples of the viscosity adjuster include high-boiling water-soluble organic solvents such as glycerin, ethylene glycol, diethylene glycol, triethylene glycol, polyethylene glycol, propylene glycol, dipropylene glycol, polypropylene glycol, butylene glycol, hexylene glycol, and phenoxyethanol.
[0047] <Composition of the composition> In the present composition, the content of the amine compound is preferably 0.1 to 10.0 parts by mass, more preferably 0.1 to 8.0 parts by mass, even more preferably 0.2 to 6.0 parts by mass, particularly preferably 0.3 to 4.0 parts by mass, and particularly preferably 0.5 to 4.0 parts by mass, relative to 100 parts by mass of the solid content of the resol type phenolic resin. When the content of the amine compound is equal to or more than the above lower limit, the formaldehyde emission amount of the wood material can be further reduced. When the content of the amine compound is equal to or less than the above upper limit, the adhesive performance of the present composition is superior, and the wood break rate of the wood material tends to be superior.
[0048] The content of the organic acid ester is preferably 1.0 to 40.0 parts by mass, more preferably 1.0 to 30.0 parts by mass, per 100 parts by mass of the total of the resol type phenolic resin and the amine compound. If the content of the organic acid ester is equal to or more than the lower limit, the curing property of the composition and the adhesive strength between wood pieces tend to be superior. If the content of the organic acid ester is equal to or less than the upper limit, the adhesive strength between wood pieces is superior.
[0049] The content of resorcinol is preferably 0.5 to 20.0 parts by mass, more preferably 1.0 to 15.0 parts by mass, even more preferably 2.0 to 10.0 parts by mass, even more preferably 3.0 to 9.0 parts by mass, and particularly preferably 3.0 to 8.0 parts by mass, based on 100 parts by mass of the total of the resol type phenolic resin and the amine compound. When the content of resorcinol is within the above range, the curing property of the composition and the adhesive strength between woods tend to be more excellent.
[0050] The total proportion of the solid content of the resol type phenolic resin, the amine compound and the organic acid ester relative to 100% by mass of the solid content of the present composition is preferably 70% by mass or more, more preferably 80% by mass or more, and may be 100% by mass. When the present composition contains resorcinol, the total proportion of the solid content of the resol-type phenolic resin, the amine compound, the organic acid ester, and resorcinol relative to 100% by mass of the solid content of the present composition is preferably 70% by mass or more, more preferably 80% by mass or more, and may be 100% by mass.
[0051] The pH of the present composition immediately after production (immediately after mixing all components) is preferably 7 to 14, and more preferably 8 to 14. If the pH is equal to or higher than the lower limit, the penetration into wood is good and the adhesive strength is superior, and if the pH is equal to or lower than the upper limit, the curing time is sufficiently fast and the adhesive strength is superior.
[0052] The viscosity of the composition is preferably 10 to 20,000 mPa s, and more preferably 100 to 15,000 mPa s. When the viscosity of the composition is equal to or higher than the lower limit, sufficient adhesive strength can be maintained when temporarily bonding wood, and when the viscosity is equal to or lower than the upper limit, the coatability of the composition is excellent.
[0053] The solid content of the composition is preferably 20 to 100% by mass, more preferably 30 to 90% by mass, and even more preferably 40 to 70% by mass. When the solid content of the composition is within the above range, the viscosity of the composition can be easily adjusted to the above-mentioned preferred range.
[0054] <Method of preparing the present composition> The composition can be prepared by mixing raw materials including a resol type phenolic resin, an amine compound, and an organic acid ester. The raw materials may further include additional water, an alkaline substance, resorcinol, and other components, as necessary, in addition to the resol type phenolic resin, the amine compound, and the organic acid ester. Although the order of mixing the raw materials is not particularly limited, mixing the resol-type phenolic resin with the organic acid ester facilitates thickening due to gelation of the resol-type phenolic resin, so it is preferable to mix the resol-type phenolic resin with the organic acid ester immediately before the production of the wood material. Similarly, mixing the resol-type phenolic resin with resorcinol facilitates thickening due to gelation of the resol-type phenolic resin, so it is preferable to mix the resol-type phenolic resin with resorcinol immediately before the production of the wood material. When the composition contains resorcinol, the organic acid ester and resorcinol may be mixed with the resol phenolic resin individually, or may be mixed in advance with the resol phenolic resin. In view of the simplification of the manufacturing process of the wood material, it is preferable that the organic acid ester and resorcinol are mixed in advance. It is preferable that the time from mixing the resol type phenolic resin with at least one of the organic acid ester and resorcinol until the composition is applied to wood is 1 hour or less. A suitable method for preparing this composition is to mix the first and second parts of a wood adhesive kit described below.
[0055] The composition is for wood and is used to bond pieces of wood together. Wood will be described in detail later. By bonding two or more pieces of wood together with the composition, a wood material is obtained. The composition can also be said to be for use in the manufacture of wood materials.
[0056] Since the composition contains a resol-type phenolic resin, an amine compound, and an organic acid ester, even when the wood material is produced by hot pressing or cold pressing for a short time or at a low temperature, the wood material has a low formaldehyde emission amount. The reason why amine compounds can reduce the amount of formaldehyde emitted is believed to be that free phenols or aldehydes and amine compounds form condensations through the Mannich reaction, and nitrogen atoms bonded to hydrogen atoms in these Mannich condensations capture the emitted formaldehyde.
[0057] [Wood adhesive kit] A wood adhesive kit according to one embodiment of the present invention (hereinafter also referred to as "this kit") comprises a first container containing a first agent and a second container containing a second agent.
[0058] The first agent contains a resol type phenolic resin and an amine compound. The first agent preferably does not contain an organic acid ester and resorcinol. The first agent may further contain other components. The resol type phenolic resin, the amine compound, and the other components are as described above, and the preferred embodiments are also the same. The pH of the first agent is preferably 7-14, more preferably 8-14, and even more preferably 9-14. The viscosity of the first agent is preferably from 10 to 20,000 mPa·s, more preferably from 100 to 15,000 mPa·s, and even more preferably from 1000 to 10,000 mPa·s. The solid content concentration of the first agent is preferably from 30 to 70 mass %, more preferably from 40 to 60 mass %, and even more preferably from 45 to 55 mass %.
[0059] The second agent contains an organic acid ester. The second agent preferably does not contain a resol-type phenolic resin. The second agent may further contain one or more of resorcinol and other components. The organic acid ester is as described above, and the preferred embodiments are also the same.
[0060] The preferred content (parts by mass) of the amine compound per 100 parts by mass of the resol type phenolic resin in the present kit is the same as the preferred content of the amine compound per 100 parts by mass of the resol type phenolic resin in the present composition.
[0061] The preferred content (parts by mass) of the organic acid ester per 100 parts by mass of the resol-type phenolic resin and the amine compound in this kit is the same as the preferred content of the organic acid ester per 100 parts by mass of the resol-type phenolic resin and the amine compound in this composition.
[0062] The preferred content (parts by mass) of resorcinol per 100 parts by mass of the resol-type phenolic resin and the amine compound in this kit is the same as the preferred content of resorcinol per 100 parts by mass of the resol-type phenolic resin and the amine compound in this composition.
[0063] The preferred ratio (mass %) of the total of the solid content of the resol-type phenolic resin, the amine compound, and the organic acid ester to the total of 100 mass % of the solid content of the first agent and the solid content of the second agent is the same as the preferred ratio of the total of the solid content of the resol-type phenolic resin, the amine compound, and the organic acid ester to 100 mass % of the solid content of this composition. When the second agent contains resorcinol, the preferred ratio (mass %) of the total of the solid content of the resol-type phenolic resin, the amine compound, the organic acid ester, and resorcinol to the total of 100 mass % of the solid content of the first agent and the solid content of the second agent is the same as the preferred ratio of the total of the solid content of the resol-type phenolic resin, the amine compound, the organic acid ester, and resorcinol to 100 mass % of the solid content of the composition.
[0064] In this kit, the first and second agents are mixed to form the composition, which is used to bond pieces of wood together.
[0065] [Wood material] A wood material according to one embodiment of the present invention is formed by bonding two or more pieces of wood together via a cured product of the present composition.
[0066] Examples of wood include solid wood and wood-based materials, and the typical example is solid wood. Examples of solid wood include birch, paulownia, cedar, cypress, pine, Japanese cypress, sawara, pine, etc. The form of the solid wood may be sawn lumber, cut board, veneer, etc. Examples of wood materials include plywood, laminated timber, CLT (cross laminated timber), LVL (laminated veneer lumber), blockboard, veneer, wood board, etc. Examples of wood boards include IB (insulation board), MDF (medium density fiberboard), HB (hardboard), particle board, OSB (oriented strand board), etc.
[0067] Examples of the wood material of this embodiment include the same wood materials as those given as examples of wood. As the wood material of this embodiment, plywood, laminated lumber, CLT or LVL are preferred, and plywood and LVL are more preferred. In view of the importance of reducing formaldehyde emissions, plywood is particularly preferred. In the case of plywood, multiple wooden veneers are bonded via the cured product of the present composition. The wooden veneers are not particularly limited, and any known wooden veneers for plywood can be used. For example, cedar, larch, etc. are preferably used as materials for the wooden veneers. The number of wooden veneers constituting the plywood is not particularly limited, and can be, for example, 2 to 20 sheets. In the case of laminated lumber, a plurality of laminas are bonded via the cured product of the present composition. Generally, laminas cut from sawn boards are used. The number of laminas constituting the laminated lumber is not particularly limited, and may be, for example, 2 to 30.
[0068] [Method of manufacturing wood materials] A method for producing a wood material according to one embodiment of the present invention comprises the steps of: A step of preparing a wood adhesive composition by mixing raw materials including a resol type phenolic resin, an amine compound, and an organic acid ester; A step of stacking a plurality of pieces of wood with the wood adhesive composition interposed therebetween to obtain a laminate; curing the wood adhesive composition in the laminate; has. Hereinafter, the manufacturing method of this embodiment will be described using an example in which plywood or laminated lumber is manufactured as a wood material, but the manufacturing method of this embodiment is not limited to the following example.
[0069] <Manufacturing method of plywood> The method for producing plywood in this example includes a step of mixing a resol-type phenolic resin, an amine compound, and an organic acid ester to prepare the composition (a composition preparation step); a step of stacking a plurality of veneers via the present composition to obtain a laminate (lamination step); a step of curing the composition in the obtained laminate (adhesion step); has. After the curing step, the prepared plywood may be stacked and cured for a certain period of time, if necessary.
[0070] The composition preparation process is the same as the above-mentioned method for preparing the present composition.
[0071] In the lamination process, the composition is applied to at least one surface of the veneers that overlap in the plywood, and then the multiple veneers are laminated together. The method of applying the composition and the method of laminating the veneers may be the same as those used in the production of known plywood. The amount of the composition applied is, for example, 100 to 350 g / m2 as the mass per unit area of the laminated surface of the veneer. 2 Examples include: As described above, the time from mixing the resol-type phenolic resin with at least one of the organic acid ester and resorcinol in the composition preparation step until the composition is applied to a veneer is preferably 1 hour or less.
[0072] In the bonding step, the method of curing the present composition in the laminate includes, for example, applying only cold pressure, only hot pressure, or both cold pressure and hot pressure to the laminate. When applying both cold pressure and hot pressure, typically, hot pressure is applied after cold pressure is applied. The cold pressing conditions and hot pressing conditions may each be such that the composition can be cured. Examples of the cold pressing conditions include a temperature of room temperature (25° C.), a pressure of 0.1 to 2.0 MPa, and a cold pressing time of 10 to 360 minutes. Regarding the heat and pressure conditions, in consideration of energy costs, the temperature is preferably 300° C. or less, more preferably 250° C. or less, and even more preferably 200° C. or less, and in consideration of productivity, the temperature is preferably 50° C. or more, more preferably 80° C. or more, and even more preferably 100° C. or more. The pressure is, for example, 0.1 to 2.0 MPa. The time for applying heat and pressure is, for example, 10 to 100 seconds per 1 mm of thickness after heat and pressure in the direction of applying heat and pressure. When hot pressing is applied after cold pressing in the bonding process, the time from when the composition is applied to the veneer in the lamination process until when cold pressing is applied in the bonding process, that is, the open assembly time, is preferably within 40 minutes, and the time from when cold pressing is applied until when hot pressing is applied, that is, the closed assembly time, is preferably within 3 hours. After cold pressing or hot pressing, a treatment such as applying a load may be carried out, if necessary.
[0073] <Manufacturing method of laminated lumber> The manufacturing method of this example of laminated wood includes a step of preparing the composition by mixing raw materials including a resol-type phenolic resin, an amine compound, and an organic acid ester (a composition preparation step); a step of stacking a plurality of laminas via the composition to obtain a laminate (lamination step); a step of pressing the obtained laminate to cure the composition (adhesion step); has. If necessary, the produced laminated lumber may be stacked and cured at a constant temperature for a certain period of time.
[0074] The composition preparation process is the same as the above-mentioned method for preparing the present composition.
[0075] In the lamination step, for example, the composition is applied to at least one lamination surface of adjacent or overlapping laminas among a plurality of laminas, and a plurality of wooden pieces are laminated together. The method of applying the composition and the method of laminating the wooden pieces may be the same as those used in the production of known laminated lumber. The amount of the composition applied is, for example, 100 to 350 g / m2 as the mass per unit area of the lamination surface of the lamina. 2 Examples include: In the composition preparation step, the time from mixing the resol type phenolic resin with at least one of the organic acid ester and resorcinol to applying the composition to the lamina is preferably 1 hour or less, as described above.
[0076] In the bonding step, the method of curing the present composition in the laminate includes, for example, applying only cold pressure, only hot pressure, or both cold pressure and hot pressure to the laminate. When applying both cold pressure and hot pressure, typically, hot pressure is applied after cold pressure is applied. The cold pressing conditions and hot pressing conditions may each be such that the composition can be cured. Examples of the cold pressing conditions include a temperature of room temperature (25° C.), a pressure of 0.1 to 2.0 MPa, and a cold pressing time of 10 to 360 minutes. As for the heat and pressure conditions, in consideration of the energy cost, the temperature is preferably 300° C. or less, more preferably 250° C. or less, and even more preferably 200° C. or less, and in consideration of the productivity, the temperature is preferably 50° C. or more, more preferably 80° C. or more, and even more preferably 100° C. or more. The pressure is, for example, 0.1 to 2.0 MPa. The time from application of the present composition until application of cold or hot pressure, so-called open assembly time, is preferably within 40 minutes. EXAMPLES
[0077] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the following examples, "parts" and "%" respectively indicate "parts by mass" and "% by mass" unless otherwise specified.
[0078] <Measurement method> (Weight average molecular weight measured by GPC) 2 g of sample (phenolic resin) was diluted with 2 g of pure water and 10 g of THF (tetrahydrofuran), and while checking the pH, the pH was adjusted to 4.0 with 1N hydrochloric acid solution. The THF layer and the water layer were separated, and the THF layer was diluted 5 times to prepare a sample for GPC measurement. The obtained sample for GPC measurement was subjected to GPC measurement under the following measurement conditions, and the weight average molecular weight in terms of polystyrene was confirmed from the results. Columns: 1 TSKgel G3000HXL 7.8 x 300 mm (manufactured by Tosoh Corporation), 2 TSKgel G2000HXL 7.8 x 300 mm (manufactured by Tosoh Corporation). Column temperature: 40°C. Detector: RI (Differential Refractive Index Detector). Solvent: THF (tetrahydrofuran). Flow rate: 0.8mL / min.
[0079] (viscosity) The viscosity was measured at 25°C using an E-type viscometer.
[0080] (solid content concentration) The mass C1 (g) of an aluminum foil dish (inner diameter 50 mm, height 15 mm) was measured, and the sample was precisely weighed to be 1.5±0.1 g thereon, and the specific mass of the sample was taken as the sample mass S (g) before drying. This aluminum foil dish was placed in a thermostatic chamber previously kept at 135±1°C, and dried for 60±2 minutes, then cooled in a desiccator, and its mass C2 (g) was measured. From the results, the sample mass D (mass of the sample remaining on the aluminum foil dish after drying) (g) after drying was calculated using the following formula (1), and the solid content concentration was calculated using the following formula (2). D = C2 - C1 (1) Solid content concentration (mass%)=D / S×100 (2)
[0081] <Production Example 1: Production of resol-type phenolic resin> A reactor equipped with a condenser, thermometer, and stirrer was charged with 376.0 parts of phenol, 192.0 parts of 50% formalin (F / P molar ratio: 0.80), 1.25 parts of 30% sulfuric acid, and 26.2 parts of water, and reacted for 3 hours under reflux conditions. The mixture was then cooled to below 80°C, and 116.7 parts of 48% aqueous sodium hydroxide solution, 360.0 parts of 50% formalin (final F / P molar ratio: 2.30), and 49.09 parts of water were added, and the mixture was reacted at 65°C until the viscosity reached 7,500 mPa·s, and then immediately cooled to below 50°C. When the reaction liquid was below 50°C, 116.7 parts of an aqueous 48% sodium hydroxide solution was added to obtain a resol-type phenolic resin with a solid content of 50%. The pH of this resol-type phenolic resin was 12.1, the weight average molecular weight was 2850, and the viscosity was 1700 mPa·s.
[0082] <Test Example 1> This test was conducted to evaluate the effect of adding amine compounds on formaldehyde emissions.
[0083] (Preparation of the first agent) The resol type phenolic resin obtained in Production Example 1 was used as the first agent in Comparative Example 1 as it was. The amount (parts) of monoethanolamine (MEA) shown in Table 1 was added to 100 parts of the resol type phenolic resin obtained in Production Example 1, and mixed to obtain the first agents of Examples 1-5.
[0084] (Special class steaming repeated test) To 100 parts of the first agent (total of resol-type phenolic resin and MEA) of each example, 14 parts of triacetin, 4 parts of resorcinol, 35 parts of calcium carbonate, and 5 parts of water were added and stirred for 1 minute to obtain wood adhesive compositions of Comparative Example 1 and Examples 1 to 5. Immediately after preparing the above-mentioned wood adhesive composition (within about 1 minute), 220 g / m of the above-mentioned wood adhesive composition was applied to both sides of a 30 cm square piece of cedar wood with a thickness of 2.5 mm. 2 A 30 cm square, 1.0 mm thick piece of cypress wood was then layered perpendicular to the grain direction of the cedar wood, and the resulting material was press molded at 25°C and 0.9 MPa for 60 minutes to obtain a 3-ply, 4.5 mm thick plywood. Twelve test pieces measuring 2.5cm x 8cm were cut from one piece of plywood obtained, and six pieces were cut in each direction to perform a special steaming test according to the Japanese Agricultural Standards (JAS) to determine the shear strength (MPa) and average wood fracture rate (%). The results were used to determine whether the test pieces met the JAS standards. The results are shown in Table 1. Regarding the JAS standard, a product is considered to have passed if its shear strength is 0.7 MPa or more, or if its shear strength is 0.6 MPa or more and its average wood fracture rate is 50% or more, or if its shear strength is 0.5 MPa or more and its average wood fracture rate is 65% or more, or if its shear strength is 0.4 MPa or more and its average wood fracture rate is 80% or more. Both the shear strength and wood breaking rate are indicators of the strength of the wood material and, in turn, the adhesive performance of the adhesive composition, but usually, more importance is attached to the wood breaking rate.
[0085] (Formaldehyde emission amount) A 3-ply, 4.5 mm-thick plywood was prepared in the same manner as above, and four test pieces of 5 cm x 15 cm were cut from the obtained plywood. The obtained test pieces were subjected to a test in accordance with the JAS formaldehyde emission test method, except that the scale was changed to 1 / 5. Specifically, a poly cup containing 60 mL of pure water and two pieces of cut plywood were placed in a 2 L poly container, which is 1 / 5 the size of a glass desiccator (JIS R 3503), and sealed. After leaving it at 20°C for 24 hours, the amount of formaldehyde in the pure water was measured by the acetylacetone method. This value corresponds to the amount of formaldehyde emitted from the test piece. The poly cup was adjusted by reducing the size of a crystallizing dish specified by JAS to 1 / 5. Each condition was carried out under n=2 (2 plywood samples x 2), and the average value was calculated. The results are shown in Table 1 and Figure 1. Table 1 also shows the JAS standard symbols for formaldehyde emission levels (F☆☆☆, F☆☆☆☆, etc.).
[0086] [Table 1]
[0087] As shown in Table 1 and Figure 1, the plywoods of Examples 1 to 5 to which MEA was added emitted less formaldehyde than the plywood of Comparative Example 1 to which MEA was not added. In addition, the shear strength and average wood fracture rate also passed the JAS standard. Comparing Examples 1 to 5, as the amount of MEA added increased, the amount of formaldehyde emitted decreased, while the average wood fracture rate tended to decrease. [Industrial Applicability]
[0088] The present invention provides a wood adhesive composition, a wood adhesive kit, and a method for producing a wood material that can produce a wood material with low formaldehyde emissions even when the wood material is produced by hot-pressing or cold-pressing in a short time or at a low temperature, as well as a wood material with low formaldehyde emissions even when the wood material is produced by hot-pressing or cold-pressing in a short time or at a low temperature.
Claims
1. An adhesive composition for wood comprising a resol-type phenolic resin, an amine compound having a hydrogen atom bonded to a nitrogen atom, and an organic acid ester.
2. 2. The wood adhesive composition according to claim 1, wherein the amine compound has at least one type selected from the group consisting of a primary amino group and a secondary amino group.
3. 3. The wood adhesive composition according to claim 1, wherein the content of the amine compound is 0.1 to 10.0 parts by mass per 100 parts by mass of the solid content of the resol type phenolic resin.
4. 3. The wood adhesive composition according to claim 1, wherein the resol type phenolic resin has a pH of 7 to 14.
5. 3. The wood adhesive composition according to claim 1, wherein the content of the organic acid ester is 1.0 to 40.0 parts by mass per 100 parts by mass of the resol type phenolic resin and the amine compound combined.
6. 3. The wood adhesive composition according to claim 1, further comprising resorcinol.
7. 7. The wood adhesive composition according to claim 6, wherein the content of the resorcinol is 0.5 to 20.0 parts by mass per 100 parts by mass of the resol type phenolic resin and the amine compound combined.
8. a first container containing a first agent including a resol type phenolic resin and an amine compound having a hydrogen atom bonded to a nitrogen atom; a second container containing a second agent including an organic acid ester; A wood adhesive kit comprising:
9. 9. The wood adhesive kit according to claim 8, wherein the amine compound has at least one selected from the group consisting of a primary amino group and a secondary amino group.
10. 10. The wood adhesive kit according to claim 8, wherein the content of the amine compound is 0.1 to 10.0 parts by mass per 100 parts by mass of the solid content of the resol type phenolic resin.
11. The wood adhesive kit according to claim 8 or 9, wherein the pH of the first agent is 7 to 14.
12. 10. The wood adhesive kit according to claim 8, wherein the content of the organic acid ester is 1.0 to 40.0 parts by mass per 100 parts by mass of the resol type phenolic resin and the amine compound combined.
13. 10. The wood adhesive kit according to claim 8 or 9, wherein the second part further comprises resorcinol.
14. The wood adhesive kit according to claim 13, wherein the content of the resorcinol is 0.5 to 20.0 parts by mass per 100 parts by mass of the resol type phenolic resin and the amine compound combined.
15. A step of preparing a wood adhesive composition by mixing raw materials including a resol type phenolic resin, an amine compound having a hydrogen atom bonded to a nitrogen atom, and an organic acid ester; A step of stacking a plurality of pieces of wood with the wood adhesive composition interposed therebetween to obtain a laminate; curing the wood adhesive composition in the laminate; A method for producing a wood material having the above structure.
16. 16. The method for producing a woody material according to claim 15, wherein the amine compound has at least one type selected from the group consisting of a primary amino group and a secondary amino group.
17. 17. The method for producing a wood material according to claim 15, wherein the content of the amine compound is 0.1 to 10.0 parts by mass per 100 parts by mass of the solid content of the resol type phenolic resin.
18. The method for producing a woody material according to claim 15 or 16, wherein the resol type phenolic resin has a pH of 7 to 14.
19. 17. The method for producing a woody material according to claim 15, wherein the content of the organic acid ester is 1.0 to 40.0 parts by mass per 100 parts by mass of the resol type phenolic resin and the amine compound combined.
20. The method for producing a woody material according to claim 15 or 16, wherein the raw material further contains resorcinol.
21. The method for producing a woody material according to claim 20, wherein the content of the resorcinol is 0.5 to 20.0 parts by mass per 100 parts by mass of the resol type phenolic resin and the amine compound combined.
22. 3. A wood material comprising a plurality of pieces of wood bonded together via a cured product of the wood adhesive composition according to claim 1 or 2.
23. 23. The wood material according to claim 22, which is plywood.
Citation Information
Patent Citations
Method for reducing formaldehyde emissions in wood-based materials
JP2009523628A
Adhesive composition for plywood, kit for producing adhesive composition for plywood, plywood, and method for producing plywood
JP2021161200A
Adhesive composition for wood, adhesive kit for wood, woody material and method for producing the same
JP2022113657A
Thermosetting composition for cellulose product and cellulose product
JP2022153295A
Wood adhesive composition, wood adhesive kit, wood material and method for producing the same
JP7076049B1