Granulated powder and glass green sheet

The use of a granulated powder composition with glass powder, a water-soluble binder, and an organic acid with a carboxy group addresses cracking issues in glass green sheets, enhancing moldability and flexibility for fuel cell sealing.

JP2024145410APending Publication Date: 2024-10-15NORITAKE MACHINE TECHNO CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023057739
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Glass green sheets are prone to cracking during the molding process due to high forming loads, which affects their moldability.

Method used

A granulated powder composition for glass green sheets comprising glass powder, a water-soluble binder, and an organic acid with a carboxy group, with specific particle size and concentration ratios, enhances moldability by reducing forming loads and improving uniform mixing.

Benefits of technology

The granulated powder composition significantly reduces cracking and improves the moldability and flexibility of glass green sheets, enabling effective sealing in fuel cell applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024145410000003
    Figure 2024145410000003
  • Figure 2024145410000001
    Figure 2024145410000001
  • Figure 2024145410000002
    Figure 2024145410000002
Patent Text Reader

Abstract

To provide a technology for improving moldability of a glass green sheet.SOLUTION: A granulated powder used for a glass green sheet for sealing disclosed here includes glass powder, a water-soluble binder, and an organic acid including a carboxyl group. A volume-based D50 particle diameter of the glass powder according to laser diffraction / scattering method is 10-50 μm. A carbon number included in the organic acid is 8 or less. A ratio of the organic acid is 5 wt.% or less if the whole of the granulated powder is taken as 100 wt.%.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a granulated powder and a glass green sheet. [Background technology]

[0002] In fuel cells, glass is used for sealing purposes to prevent mixing of air and fuel gas. For example, glass green sheets are known as such glasses. For example, JP 2020-167093 A discloses a technology relating to a sealing green sheet that can prevent molding defects and breakage during sheet molding and form a gas sealing portion that can suitably prevent gas leakage. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2020-167093 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, when a glass green sheet is formed, cracks may occur at its edges. Therefore, a technology for realizing a glass green sheet with excellent formability is desired.

[0005] Therefore, a main object of the present disclosure is to provide a technique for improving the formability of a glass green sheet. [Means for solving the problem]

[0006] The present disclosure provides a granulated powder for use in a sealing glass green sheet. One embodiment of the granulated powder disclosed herein includes a glass powder, a water-soluble binder, and an organic acid containing a carboxyl group (also referred to as an "organic acid additive" in this specification), the glass powder has a volume-based D50 particle size based on a laser diffraction / scattering method of 10 μm to 50 μm, the organic acid contains 8 or less carbon atoms, and the proportion of the organic acid is 5 wt% or less when the entire granulated powder is taken as 100 wt%.

[0007] The inventors have found through their research that the granulated powder containing the organic acid in the above ratio reduces the molding load when the granulated powder is molded into a sheet. The reduced molding load makes it difficult for cracks to occur in the molded glass green sheet. In other words, the granulated powder can improve the moldability of the glass green sheet.

[0008] In one embodiment of the granulated powder disclosed herein, the organic acid is water-soluble, which allows the organic acid additive to be mixed more uniformly in a slurry containing other materials and an aqueous solvent, thereby improving the formability of the glass green sheet.

[0009] In one embodiment of the granulated powder disclosed herein, the number of carboxyl groups in the organic acid is equal to or greater than 2. The greater the number of carboxyl groups in the organic acid, the more improved the water solubility is, and therefore the higher moldability is achieved.

[0010] In one embodiment of the granulated powder disclosed herein, the organic acid contains citric acid, which provides higher moldability.

[0011] In one embodiment of the granulated powder disclosed herein, the ratio of the glass powder to the total weight of the granulated powder is 50 wt % or more and 80 wt % or less, which can further improve the forming stability of the glass green sheet.

[0012] The present disclosure also provides a sealing glass green sheet made from the granulated powder disclosed herein. One embodiment of the glass green sheet disclosed herein includes a glass powder, a water-soluble binder, and an organic acid containing a carboxyl group, the glass powder having a volume-based D50 particle size based on a laser diffraction / scattering method of 10 μm to 50 μm, the organic acid having 8 or less carbon atoms, and the proportion of the organic acid being 5 wt% or less when the entire glass green sheet is taken as 100 wt%. A glass green sheet having such a configuration has excellent moldability. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a schematic diagram of the roll forming method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] A preferred embodiment of the present technology will be described below. Note that matters other than those specifically mentioned in this specification (for example, components of granulated powder, components of glass green sheet, etc.) that are necessary for implementing the present technology can be understood as design matters of a person skilled in the art based on the conventional technology in the field. The present technology can be implemented based on the contents disclosed in this specification and the technical common sense in the field. Note that in this specification, when a numerical range is described as "A to B (where A and B are arbitrary numerical values)", it means "A or more and B or less", and also includes the meanings of "more than A and less than B", "more than A and B or less", and "A or more and less than B". In addition, the dimensional relationships (length, width, thickness, etc.) in the drawings described in this specification do not necessarily reflect the actual dimensional relationships.

[0015] Granulated powder The granulated powder disclosed herein includes at least a glass powder, a water-soluble binder, and an organic acid containing a carboxyl group. The granulated powder is obtained by processing glass powder as a raw material into a granular shape. The granulated powder disclosed herein can be used, for example, in the manufacture of a sealing glass green sheet.

[0016] The properties of the particles constituting the granulated powder, such as the shape and size, are not particularly limited. The shape of the granulated powder is, for example, approximately spherical. However, it may be scaly (flake-like), plate-like, or irregularly shaped. In this specification, the term "approximately spherical" refers to a shape that can be regarded as roughly a sphere as a whole, and the average aspect ratio (major axis / minor axis) based on an image observed with an electron microscope is approximately 1 to 2, for example, 1 to 1.5.

[0017] The D50 particle size of the granulated powder may be, for example, 20 μm or more, 40 μm or more, 60 μm or more, 80 μm or more, 100 μm or more, or 120 μm or more from the viewpoint of improving the handleability, etc. Also, from the viewpoint of improving the sheet moldability, the D50 particle size of the granulated powder may be, for example, 250 μm or less, 200 μm or less, or 150 μm or less. In this specification, the "D50 particle size of the glass powder" refers to the particle size corresponding to the cumulative 50% from the fine particle side in the volume-based particle size distribution measured by a laser diffraction / light scattering method.

[0018] Each component contained in the granulated powder will be described below.

[0019] 1. Glass powder The glass powder may be the main component of the granulated powder disclosed herein. For example, when a glass green sheet containing the granulated powder disclosed herein is fired, the glass powder is fused and solidified by firing to form a sealing portion. Such glass powder can be any conventionally known glass powder without any particular limitation within the scope in which the effect of the present technology is exerted. For example, the glass powder may be crystallized glass containing crystals in addition to general amorphous glass. The components of the glass powder are also not particularly limited. For example, borosilicate glass, alkali glass, alkali-free glass, lead-based glass, lead-lithium glass, zinc-based glass, bismuth-based glass, borate-based glass, lead-free glass, tellurium-based glass, and the like can be mentioned. Among these, it is preferable to use borosilicate glass. Borosilicate glass contains at least SiO2 and B2O3. Examples of borosilicate glass include SiO2-B2O3-based glass, SiO2-RO-B2O3-based glass (R represents, for example, Mg, Ca, Zn, Ba, and Sr. The same applies below), and SiO2-R'2O-B2O3-based glass (R' represents, for example, Li, K, and Na. The same applies below). The borosilicate glass may contain components such as Al2O3, ZrO2, BeO, Ag2O, TiO2, V2O5, FeO, Fe2O3, Fe3O4, CuO, Cu2O, Nb2O5, P2O5, La2O3, CeO2, Bi2O3, and Pb2O3. The glass powder may contain one or more components in addition to the above-mentioned glass components. One of the above-mentioned glass components may be used alone, or two or more may be mixed.

[0020] The D50 particle size of the glass powder may be, for example, 10 μm or more, 15 μm or more, or 20 μm or more. If the D50 particle size of the glass powder is too small, the fluidity of the granulated powder becomes too high, making it difficult to form a sheet. The D50 particle size of the glass powder may be, for example, 50 μm or less, 40 μm or less, or 30 μm or less. If the D50 particle size of the glass powder is too large, the granulated powder tends to be bulky during sheet forming, and formability may decrease.

[0021] In this specification, the "D50 particle size of the glass powder" refers to the particle size corresponding to the cumulative 50% from the fine particle side in the volume-based particle size distribution measured by the laser diffraction / light scattering method. The particle size of the glass powder may be measured, for example, after a process for removing organic matter contained in the granulated powder. For example, the organic matter may be removed by a heat treatment at a temperature equal to or higher than the boiling point of the organic matter contained in the granulated powder and lower than the glass transition point of the glass powder. Furthermore, if aggregation of the glass powder is observed after removing the organic matter, it is preferable to disintegrate the glass powder.

[0022] The glass transition temperature of the glass powder is preferably higher than the heating temperature in the degreasing treatment of the glass green sheet and lower than the heating temperature in the firing treatment. This can prevent the glass powder from melting in the degreasing treatment, which would hinder the removal of organic matter, and can properly fuse and solidify the glass powder in the firing treatment. The suitable glass transition temperature of the glass powder can be appropriately changed depending on the heating temperatures in the degreasing treatment and the firing treatment, but is preferably 530°C or higher, and particularly preferably 550°C or higher and 680°C or lower.

[0023] In addition, it is more preferable to appropriately select the glass powder from the viewpoint of approximating the thermal expansion coefficient between the glass powder and the sealed member (e.g., a gas pipe of a fuel cell). For example, the difference in the thermal expansion coefficient between the glass powder and the sealed member is about 2×10 -6 K -1 For example, 1×10 -6 K -1 Specifically, the thermal expansion coefficient of the sealed member is preferably 8×10 -6 K -1 ~12×10 -6 K -1 When the thermal expansion coefficient of the glass powder is about 8×10 -6 K -1 ~12×10 -6 K -1 , typically 9.5 × 10 -6 K -1 ~11.5×10 -6 K -1 , e.g. 10×10 -6 K -1 ~11×10-6 K -1 This can prevent the gas sealing portion from being damaged due to the difference in the amount of expansion from the sealed member. Note that the "thermal expansion coefficient" in this specification refers to the average linear thermal expansion coefficient from 30°C to 500°C.

[0024] The proportion of the glass powder in the granulated powder may be, for example, 50 wt% or more, 55 wt% or more, or 60 wt% or more, when the entire granulated powder is taken as 100 wt%. This allows a sealing portion with high sealing properties to be formed by firing. The proportion of the glass powder in the granulated powder may be, for example, 80 wt% or less, 75 wt% or less, 70 wt% or less, or 65 wt% or less. If the proportion of the glass powder is too high, the molding stability of the glass green sheet may decrease.

[0025] 2. Water-soluble binder The binder is a component that binds each component of the granulated powder to stabilize the shape of the granulated powder. In the manufacturing process of the granulated powder disclosed herein, an aqueous solvent is preferably used, and therefore a water-soluble binder that dissolves in the aqueous solvent is used. Examples of such water-soluble binders include water-soluble resins having hydrophilic groups. By using a water-soluble resin binder, the use of organic solvents in the manufacturing process can be reduced, thereby reducing the environmental load.

[0026] In this specification, the term "water-soluble binder" may include a binder that is completely dissolved in an aqueous solvent at 25°C, a binder that is partially dissolved in an aqueous solvent and the remainder is dispersed in the aqueous solvent, or a binder that is dispersed in an aqueous solvent. Examples of aqueous solvents include water such as ion-exchanged water (deionized water), pure water, ultrapure water, and distilled water. The aqueous solvent may contain a non-aqueous solvent (such as a lower alcohol or a lower ketone) that can be mixed uniformly with water as necessary, within a range that does not impair the effects of the technology disclosed herein. In this case, for example, 95 vol% or more or 99 vol% or more of the aqueous solvent may be water.

[0027] The type of the water-soluble binder is not particularly limited, but is preferably a resin material with a weight loss rate of 70% or more after heat treatment in an air atmosphere at 400°C. The weight loss rate of the water-soluble binder after heat treatment at 400°C is preferably 80% or more, more preferably 85% or more, even more preferably 90% or more, and particularly preferably 95% or more. The upper limit of the weight loss rate after such heat treatment is not particularly limited, and may be 100% or less, or may be 99% or less. In this way, by selecting a resin material that is sufficiently removed by a relatively low-temperature heat treatment as the water-soluble binder, the water-soluble binder can be more reliably removed, for example, in a degreasing process during the manufacture of a low-temperature operating SOFC. As a result, firing defects due to the remaining water-soluble binder (carbon component) are suitably prevented, and a dense sealing portion with a high relative density can be formed.

[0028] Suitable examples of resin materials used in the water-soluble binder include acrylic resins and polyether resins having carboxyl groups at least on the side chains and terminals. These resin materials can be uniformly dissolved or dispersed in an aqueous solvent to provide stability to the shape of the granulated powder. They can also provide suitable shape integrity to a glass green sheet containing such granulated powder, and can be suitably removed by a low-temperature degreasing treatment.

[0029] The glass transition temperature of the water-soluble binder is preferably lower than the heating temperature in the degreasing treatment. This allows the water-soluble binder to be easily removed in the degreasing treatment, and prevents poor firing due to residual water-soluble binder. The glass transition temperature of the water-soluble binder can be appropriately changed depending on the heating temperatures in the degreasing treatment and the firing treatment, but is preferably, for example, 10°C to 80°C.

[0030] When the entire granulated powder is taken as 100 wt%, the proportion of the water-soluble binder may be, for example, 10 wt% or more, 20 wt% or more, 25 wt% or more, or 30 wt% or more. This stabilizes the shape of the granulated powder. The proportion of the water-soluble binder may be, for example, 50 wt% or less, 40 wt% or less, or 35 wt% or less. If the amount of the water-soluble binder is too large, the proportion of the glass powder in the granulated powder may decrease, and the sealing property after firing may decrease.

[0031] 3.Organic acid (organic acid additive) The granulated powder contains an organic acid containing a carboxyl group (also referred to as an "organic acid additive" in this specification to distinguish it from organic acids that may be contained as other components). The inventors have found that, in a granulated powder having a glass powder with a predetermined D50 particle size (for example, 10 μm to 50 μm), the molding load during sheet molding is reduced by the granulated powder containing an appropriate amount of an organic acid additive. By reducing the molding load, cracks are less likely to occur in the molded glass green sheet, and moldability can be improved. Although the mechanism of such an effect is not clear, the inventors have found that the granulated powder tends to become less likely to flow when an organic acid additive is mixed into the granulated powder having a glass powder with a D50 particle size in the above-mentioned predetermined range. Therefore, it is presumed that the load during sheet molding is reduced by making the granulated powder less likely to flow. Note that such a presumed mechanism does not limit the present technology in any way.

[0032] The organic acid additive is preferably water-soluble. In the manufacturing process of the granulated powder disclosed herein, an aqueous solvent is preferably used. Therefore, since the organic acid additive is water-soluble, the organic acid additive is mixed more uniformly in the slurry mixed with other materials. As a result, the flowability of the granulated powder is more uniformly controlled, the glass green sheet to be molded is less likely to crack, and moldability is further improved. In this specification, the term "water-soluble organic acid additive" may include an additive that is completely dissolved in an aqueous solvent at 25°C, an additive that is partially dissolved in an aqueous solvent with the remainder dispersed in the aqueous solvent, or an additive that is dispersed in the aqueous solvent.

[0033] The number of carbon atoms contained in the organic acid additive may be, for example, 8 or less, preferably 7 or less, and more preferably 6 or less. The number of carbon atoms is smaller, so that the organic acid additive tends to be more soluble in water, and thus the moldability may be improved. The lower limit of the number of carbon atoms of the organic acid additive is not particularly limited, but may be, for example, 1 or more, or 2 or more.

[0034] The number of carboxyl groups contained in the organic acid additive is not particularly limited, and may be, for example, 1 to 3, but is preferably 2 or more (for example, 2 to 3). The greater the number of carboxyl groups, the more improved the water solubility and the higher moldability that can be achieved.

[0035] The molecular weight of the organic acid additive is not particularly limited, but is, for example, 300 g / mol or less, preferably 250 g / mol or less, and more preferably 200 g / mol or less. Although it cannot be generally stated due to differences in functional groups, etc., organic acids tend to be more soluble in water as their molecular weight decreases, so organic acids within this range can be suitably used.

[0036] Specific examples of organic acid additives include organic acids with one carbon atom, such as formic acid, organic acids with two carbon atoms, such as acetic acid and oxalic acid, organic acids with three carbon atoms, such as pyruvic acid and malonic acid, organic acids with four carbon atoms, such as succinic acid, malic acid, tartaric acid, fumaric acid, and maleic acid, organic acids with five carbon atoms, such as glutaric acid, organic acids with six carbon atoms, such as citric acid and adipic acid, organic acids with seven carbon atoms, such as pimelic acid, and organic acids with eight carbon atoms, such as suberic acid. Among these, it is preferable to use citric acid. Citric acid has three carboxy groups and is highly water-soluble, so that it can suitably improve the formability of the glass green sheet. The organic acid additives may be used alone or in combination.

[0037] When the entire granulated powder is taken as 100 wt%, the ratio of the organic acid additive can be, for example, 0.01 wt% or more, 0.1 wt% or more, or 0.2 wt% or more. This makes the granulated powder less likely to flow, improving moldability. The ratio of the organic acid additive can be, for example, 5 wt% or less, 4 wt% or less, 3 wt% or less, 2.5 wt% or less, 2 wt% or less, 1.5 wt% or less, 1 wt% or less, or 0.8 wt% or less. Surprisingly, when the ratio of the organic acid additive is too high, the granulated powder tends to flow easily, and the flexibility of the molded glass green sheet can be reduced.

[0038] 4. Other Ingredients In addition to the above-mentioned glass powder, water-soluble binder, and organic acid additive, the granulated powder may contain other components as necessary. For example, various additives such as plasticizers, release agents, antifoaming agents, dispersants, antioxidants, thickeners, etc. may be included. In a preferred embodiment, the granulated powder contains a plasticizer.

[0039] The plasticizer is a component that imparts strength, flexibility, etc. to the granulated powder and the glass green sheet containing the granulated powder. For example, the plasticizer preferably contains at least one of a trihydric or higher alcohol and a polyether. Even when dispersed in an aqueous solvent, these plasticizers can impart suitable strength and flexibility to the granulated powder and the glass green sheet containing the granulated powder, and therefore can suitably prevent molding defects and breakage during sheet molding. Suitable examples of trihydric or higher alcohols include polyglycerins such as diglycerin, triglycerin, and tetraglycerin, glycerin, trimethylolmethane, trimethylolpropane, pentaerythritol, arbitol, sorbitol, xylose, arabinose, glucose, galactose, sorbose, fructose, palatinose, maltotriose, and maleitose. Suitable examples of polyethers include polyglycerin ether, polyoxyethylene polyglyceryl ether, and polyoxypropylene polyglyceryl ether. Among these, glycerin, polyglycerin ether, and polyoxyethylene polyglyceryl ether are particularly preferred from the viewpoint of storage stability of the glass green sheet after molding, since they can impart suitable strength and flexibility as well as suitable moisture retention.

[0040] When the plasticizer is a polymer, its average molecular weight may be, for example, 1500 or less, 1400 or less, or 1300 or less. If the average molecular weight of the plasticizer is too large, the plasticizer with a long molecular chain will bond excessively with the glass powder, and the granulated powder will tend to become rubbery, making it difficult to form the sheet. From the viewpoint of improving the storage stability (moisture retention) of the glass green sheet after forming, the average molecular weight of the plasticizer is preferably 350 or more, more preferably 750 or more, and even more preferably 1000 or more. In this specification, the "average molecular weight" refers to the weight average molecular weight.

[0041] In the case where the granulated powder contains a plasticizer, the ratio of the plasticizer may be, for example, 0.1 wt% or more, 0.5 wt% or more, or 1 wt% or more when the entire granulated powder is taken as 100 wt%. This provides flexibility to the molded sheet, making it less likely to crack during molding. As a result, cracks are less likely to occur during sheet molding. The ratio of the plasticizer may be, for example, 4 wt% or less, 3 wt% or less, 2 wt% or less, or 1.5 wt% or less. This is because if there is too much plasticizer, the granulated powder is more likely to adhere to the sheet molding device.

[0042] The total proportion of the other components may be, for example, 10 wt% or less, 5 wt% or less, or 3 wt% or less, when the entire granulated powder is taken as 100 wt%.

[0043] In addition, the granulated powder may further contain an aqueous solvent due to the manufacturing method. When the granulated powder contains an aqueous solvent, the proportion of the aqueous solvent may be, for example, 0.1 wt% or more, 0.2 wt% or more, when the entire granulated powder is taken as 100 wt%. In addition, the proportion of such an aqueous solvent may be, for example, 1.0 wt% or less.

[0044] In addition, the granulated powder may have a property of being difficult to flow. For example, the fluidity index (a in formula (1)) calculated by the Kawakita formula shown in the following formula (1) may be, for example, 0.2 or more, 0.22 or more, 0.24 or more, or 0.3 or more. In addition, such a fluidity index may be, for example, 0.4 or less, 0.35 or less, 0.34 or less, or 0.33 or less. Note that the higher the value of the fluidity index, the more difficult it is to flow. With a high fluidity index, the molding load when molding the granulated powder into a sheet is reduced, and cracks are less likely to occur in the sheet (i.e., moldability is improved). Note that the fluidity index can be analyzed, for example, by measuring the number of tappings and the volume corresponding to the number of tappings using a tap density. In formula (1), N represents the number of tappings, C represents the degree of bulkiness (the degree of reduction in the apparent volume of the powder), and b represents a constant.

[0045]

number

[0046] "Green Glass Sheet" The glass green sheet disclosed herein contains the granulated powder disclosed herein as a main component. For example, the glass green sheet is produced by forming the granulated powder disclosed herein into a sheet. When the entire glass green sheet is taken as 100 wt%, the ratio of the granulated powder disclosed herein in the glass green sheet can be, for example, 80 wt% or more, 90 wt% or more, 95 wt% or more, 98 wt% or more, or 100 wt%. This realizes a glass green sheet with high formability.

[0047] The glass green sheet contains the above-mentioned granulated powder as its main component, and therefore contains the above-mentioned glass powder, the above-mentioned water-soluble binder, and the above-mentioned organic acid additive. In addition to these, it may also contain other components as described above. Each component may be the same as described above, so details of each component are omitted. However, in terms of the ratio of each component described above, the description "when the entire granulated powder is taken as 100 wt%" should be read as "when the entire glass green sheet is taken as 100 wt%."

[0048] The average thickness of the glass green sheet is not particularly limited, but is preferably 50 μm to 2000 μm, more preferably 100 μm to 1000 μm. When the average thickness of the glass green sheet is a predetermined value or more, the mechanical strength of the gas sealing portion can be improved. When the average thickness of the glass green sheet is a predetermined value or less, the volume change during firing can be suppressed, and breakage during firing can be suppressed.

[0049] The glass green sheet disclosed herein may have excellent flexibility. For example, the breaking strain of the glass green sheet may be, for example, 0.035 or more, 0.06 or more, or 0.1 or more. The flexibility of the glass green sheet makes it easier to adhere the glass green sheet to a sealed member. The breaking strain here refers to the value of ε calculated by the following formula (2) when the gauge length at the time of breaking is L and the gauge length before the tensile test is Lo in a tensile test at a speed of 0.5 mm / min. ε = (L-Lo) / Lo … Equation (2)

[0050] <Method of manufacturing glass green sheet> Hereinafter, an example of a method for producing a glass green sheet using the granulated powder disclosed herein will be described. The following description is not intended to limit the glass green sheet disclosed herein.

[0051] First, the glass powder, which is the component of the granulated powder described above, the water-soluble binder, other optional components, and the aqueous solvent are prepared, and these materials are mixed to prepare a slurry. For mixing these materials, various conventionally known mixing devices such as a pot mill, a ball mill, a mixer, a disperser, and a kneader can be used without particular limitation.

[0052] Next, the organic acid additive described above is mixed into the prepared slurry. The slurry is then granulated by spray granulation (spray drying) to produce granulated powder. For example, the prepared slurry is sprayed in a dry atmosphere and dried to obtain granulated powder. By using this spray granulation method, particles are formed according to the size of the sprayed droplets, so that the size and mass of the particles in the granulated powder can be easily adjusted. The method for producing the granulated powder is not particularly limited, and may be, for example, a rolling granulation method, a fluidized bed granulation method, an agitation granulation method, a compression granulation method, an extrusion granulation method, a crushing granulation method, or the like.

[0053] Next, the granulated powder obtained above is pressure-molded to produce a glass green sheet. As a molding method, various conventionally known pressure molding methods such as a roll molding method and a press molding method can be suitably adopted. Among these, the roll molding method can be preferably adopted. FIG. 1 is a schematic diagram of the roll molding method. As shown in FIG. 1, in the roll molding method, for example, granulated powder 1a is charged into a storage tank 1 of a roll molding device 5. The granulated powder 1a is discharged to the outside through a feeder 1b at the bottom of the storage tank 1. Then, the discharged granulated powder 1a is supplied between a pair of rolling rolls 2. Then, the pair of rolling rolls 2 rotate (see the arrows in FIG. 1), thereby compressing the supplied granulated powder 1a. As a result, the granulated powder 1a is molded into a sheet shape to obtain a green sheet 10G. Note that the pressure that the rolling roll 2 receives from the granulated powder 1a when compressing the granulated powder 1a by the rolling roll 2 is referred to as a molding load in this specification. The temperature and pressure conditions here are not particularly limited and may be appropriately changed since they may vary depending on the type of raw material, etc. Also, the gap between the rolling rolls 2 may be appropriately changed so as to realize a desired thickness of the green sheet 10G.

[0054] <Applications of glass green sheet> The glass green sheet disclosed herein is suitable for electrical and physical sealing and bonding between homogeneous or dissimilar members. Examples of objects to be sealed and bonded include inorganic members such as metal members and ceramic members. That is, the glass green sheet disclosed herein can be used for sealing and bonding between metal members, between ceramic members, between ceramic members and metal members, etc. Specific examples of the metal members include gas pipes for supplying gas to single cells of the SOFC, and interconnectors disposed between single cells of the SOFC to electrically connect the single cells. Materials for the metal members include stainless steel, aluminum, chromium, iron, nickel, copper, silver, manganese, and alloys thereof. The thermal expansion coefficient of these metal members is 10×10 -6 K -1 ~15×10 -6 K-1 It may be to some extent. On the other hand, specific examples of ceramic members include fuel electrodes and air electrodes of SOFCs, and interconnectors. Materials for the ceramic members include alumina, forsterite, titania, yttria, zirconia, stabilized zirconia, and the like. The ceramic members may be a single type of ceramic, or may be a composite material (e.g., mullite, steatite, alumina zirconia, and the like) in which two or more types of ceramics are combined. The thermal expansion coefficient of these ceramic members is 6×10 -6 K -1 ~8×10 -6 K -1 It may be to some extent.

[0055] The glass green sheet disclosed herein is attached to the above-mentioned portions to be joined, and then is subjected to a degreasing treatment and a firing treatment in that order to form a sealing portion. In the degreasing process for forming the sealing portion, the sealing green sheet is heated in an air atmosphere in a temperature range higher than the burnout temperature of the water-soluble binder and lower than the glass transition temperature of the glass powder. This removes organic substances such as the water-soluble binder. The temperature in the degreasing process is preferably 300°C or higher, more preferably 350°C or higher. On the other hand, the upper limit of the heating temperature in the degreasing process is preferably 550°C or lower, more preferably 500°C or lower, even more preferably 480°C or lower, and particularly preferably 450°C or lower. From the viewpoint of appropriately exerting the effect of improving the density of the sealing green sheet disclosed herein, it is preferable to set the heating temperature in the degreasing process to 400°C.

[0056] On the other hand, in the firing process, the sealing green sheet is heated in a reducing atmosphere at a temperature higher than the glass transition temperature of the glass powder. As a result, the glass powder in the sealing green sheet is fused and solidified to the sealed member to form a gas sealing portion. The heating temperature in this firing process is preferably 700°C or higher, more preferably 750°C or higher, and even more preferably 800°C or higher. The upper limit of the heating temperature is preferably 900°C or lower, and more preferably 875°C or lower. An example of the heating temperature in such a firing process is 850°C.

[0057] As described above, specific aspects of the technology disclosed herein include those described in the following sections. Section 1: A granulated powder used for a sealing glass green sheet, Glass powder; A water-soluble binder; Organic acids containing carboxy groups Including, the glass powder has a volume-based D50 particle size based on a laser diffraction / scattering method of 10 μm or more and 50 μm or less; The organic acid contains 8 or less carbon atoms, When the entire granulated powder is 100 wt%, the ratio of the organic acid is 5 wt% or less. Granulated powder. Item 2: The granulated powder according to Item 1, wherein the organic acid is water-soluble. Item 3: The granulated powder according to Item 1 or 2, wherein the organic acid has two or more carboxy groups. Item 4: The granulated powder according to any one of Items 1 to 3, wherein the organic acid is citric acid. Item 5: The granulated powder according to any one of Items 1 to 4, wherein a ratio of the glass powder is 50 wt % or more and 80 wt % or less when the entire granulated powder is taken as 100 wt %. Item 6: A sealing glass green sheet, Glass powder; A water-soluble binder; Organic acids containing carboxy groups Including, the glass powder has a volume-based D50 particle size based on a laser diffraction / scattering method of 10 μm or more and 50 μm or less; The organic acid contains 8 or less carbon atoms, When the entire glass green sheet is taken as 100 wt %, the ratio of the organic acid is 5 wt % or less. Glass green sheet.

[0058] [Test example] Several test examples relating to the present technology will be described below, but the present technology is not limited to those shown in these test examples.

[0059] 1. Preparation of each sample (1) Sample 1 Borosilicate glass (D50 particle size: 25 μm) was used as glass powder, Rikabond 4366-02 (manufactured by Japan Coating Resin Co., Ltd.) was used as a water-soluble acrylic binder, polyglycerin ether (weight average molecular weight: 750) was used as a plasticizer, Cellosol 920 (manufactured by Chukyo Yushi Co., Ltd.) was used as a release agent, and BYK-011 (manufactured by BYK Japan Co., Ltd.) was used as an antifoaming agent. These were mixed with water in a pot mill to prepare a slurry. Citric acid was added to the obtained slurry as an organic acid additive, and granulated powder (sample 1) was produced from the above slurry using a spray drying method. The D50 particle size of the granulated powder was 150 μm. The proportions of glass powder, binder, and citric acid when the entire granulated powder is taken as 100 wt% are as shown in Table 1. The plasticizer, release agent, and antifoaming agent were set to 1.3 wt%, 2.4 wt%, and 0.3 wt%, respectively.

[0060] (2) Samples 2 to 14 The type of glass powder and the type of organic acid additive for each sample were changed as shown in Table 1. The proportions of the glass powder, binder, and organic acid additive were also changed as shown in Table 1. The plasticizer, release agent, and antifoaming agent were the same as those used in Sample 1. In Samples 2 to 14, the proportion of the plasticizer was 1.2 wt% to 1.3 wt%, the proportion of the release agent was 2.2 wt% to 2.4 wt%, and the proportion of the antifoaming agent was 0.3 wt%.

[0061] 2.Evaluation Test (1) Liquidity assessment The granulated powder of each sample was put into a cylinder and the fluidity was evaluated by a tap density tester. The number of taps into the cylinder and the corresponding volume loss data were taken and applied to the above-mentioned formula (1) (Kawakita's formula). The fluidity index was calculated from the slope of the approximation equation of the straight line obtained.

[0062] (2) Formability evaluation The granulated powder of each sample was press-molded to produce an encapsulating green sheet (thickness: 0.7 mm, width: 180 mm, length: 210 mm). The press-molding of the granulated powder was performed using a roll molding device. The green sheet immediately after molding was then visually observed to evaluate the moldability of each sample. Specifically, the molded sheet was evaluated as "x" when cracks occurred, and as "○" when no cracks occurred. The evaluation results are shown in Table 1.

[0063] (3) Flexibility assessment The molded green sheet was punched into a dumbbell shape with a Thomson blade to prepare a test piece. The test piece was fixed in a universal testing machine and subjected to a tensile test at a speed of 0.5 mm / min. The gauge length L of the test piece at break and the gauge length Lo before the test were measured, and the breaking strain ε calculated by the above formula (2) was used to evaluate the flexibility of the green sheet. Specifically, a breaking strain ε of less than 0.035 was evaluated as "x", a breaking strain ε of 0.035 or more and less than 0.10 was evaluated as "○", and a breaking strain ε of 0.10 or more was evaluated as "◎". The evaluation results are shown in Table 1.

[0064] (4) Overall evaluation When at least one of the moldability and flexibility evaluations was "x", the overall evaluation was "x", when the moldability and flexibility evaluations were "○", the overall evaluation was "○", and when the moldability evaluation was "○" and the flexibility evaluation was "◎", the overall evaluation was "◎". The evaluation results are shown in Table 1.

[0065] [Table 1]

[0066] As shown in Table 1, glass green sheets with excellent moldability and flexibility were produced when the granulated powders of Samples 1 to 9 were used. This shows that, for example, by using granulated powder containing glass powder with a D50 particle size of 10 μm to 50 μm and containing an organic acid additive having a carboxyl group with 8 or less carbon atoms at a ratio of 5 wt % or less, a glass green sheet with excellent moldability and flexibility can be realized.

[0067] Although specific examples of the present technology have been described above in detail, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and alterations of the specific examples exemplified above. [Explanation of symbols]

[0068] 1 Storage tank 1a Granulated powder 1b Feeder 2 rolls 5. Roll forming equipment 10G Green Sheet

Claims

1. A granulated powder used for a sealing glass green sheet, Glass powder; A water-soluble binder; Organic acids containing carboxy groups Including, The glass powder has a volume-based D50 particle size based on a laser diffraction / scattering method of 10 μm or more and 50 μm or less, the organic acid contains 8 or less carbon atoms, When the entire granulated powder is 100 wt%, the ratio of the organic acid is 5 wt% or less. Granulated powder.

2. The granulated powder according to claim 1 , wherein the organic acid is water-soluble.

3. The granulated powder according to claim 1 , wherein the organic acid has two or more carboxy groups.

4. The granulated powder according to claim 1 , wherein the organic acid comprises citric acid.

5. 2. The granulated powder according to claim 1, wherein a ratio of the glass powder is 50 wt % or more and 80 wt % or less when the entire granulated powder is taken as 100 wt %.

6. A sealing glass green sheet, Glass powder; A water-soluble binder; Organic acids containing carboxy groups Including, The glass powder has a volume-based D50 particle size based on a laser diffraction / scattering method of 10 μm or more and 50 μm or less, the organic acid contains 8 or less carbon atoms, When the entire glass green sheet is taken as 100 wt %, the ratio of the organic acid is 5 wt % or less. Glass green sheet.

Citation Information

Patent Citations

  • Green sheet for sealing