Spraying mortar
A spray mortar with optimized cement, quick-setting agent, and fine aggregate composition addresses dust and blockage issues, ensuring effective mixing and superior strength development for tunnel applications.
Patent Information
- Application Number
- JP2024055895
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-15
AI Technical Summary
Existing spray mortar methods using liquid quick-setting agents face issues with dust generation, poor mixing of powder components, hose blockage due to increased viscosity, and insufficient strength development, especially when pumping over long distances.
A spray mortar composition comprising cement, a quick-setting agent, a thickener, and fine aggregate, with specific particle size distributions and content ratios, ensuring thorough mixing and reduced dust generation while maintaining excellent strength development.
The solution provides a spray mortar with improved pumpability, minimal dust, and enhanced strength development, suitable for applications in tunnels and narrow spaces.
Smart Images

Figure 2024146901000001 
Figure 2024146901000002 
Figure 2024146901000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a spray mortar. [Background technology]
[0002] In tunnels, mining pits, underground spaces, etc., cement slurry or cement-based mortar is sprayed on the target surface to prevent collapse of the excavated surface, prevent water leakage from the ground surface, and further to finish these surfaces. In the general spraying method of cement-based mortar, cement, water, and fine aggregate are weighed and mixed at a plant installed near the excavation site to prepare base mortar, which is then transported to the excavation site by an agitator truck, pumped through a transport pipe to the spraying machine, and a separately delivered accelerator is added and mixed just before spraying. Accelerator is roughly divided into powder accelerator such as calcium aluminate and sodium aluminate, and liquid accelerator such as aluminum sulfate and sodium silicate. Powder accelerator has strong quick-setting properties and high initial strength development, but it is difficult to mix with cement mortar when added, so it is prone to dust generation. On the other hand, while liquid quick-setting agents can suppress dust generation, sodium silicate has a high alkaline content and can cause deterioration of cement-based structures, while aluminum sulfate, which is in line with the trend toward alkali-free structures, has low quick-setting properties and tends not to develop high initial strength.
[0003] It is known that, as a measure to improve the spraying properties when aluminum sulfate is used as a liquid quick-setting admixture, adding gypsum to a mortar slurry for adding aluminum sulfate quick-setting admixture in advance has the effect of improving strength (see, for example, Patent Document 1). It is also known that sprayed concrete in which calcium aluminate is added as a quick-setting aid together with gypsum to concrete before water is poured, and then water and liquid aluminum sulfate are added to this, can improve quick-setting properties and strength development (see, for example, Patent Document 2). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 10-212149 [Patent Document 2] Japanese Patent Application Publication No. 11-130500 Summary of the Invention [Problem to be solved by the invention]
[0005] In recent years, the use of liquid quick-setting agents has been increasing in order to further reduce dust and improve safety for workers. As a spraying method using liquid quick-setting agents, a dry spraying method is sometimes adopted in which powder components are mixed in advance to prepare a premixed mortar, and liquid components such as water and liquid quick-setting agents are added in a spraying device while the premixed mortar is being pumped with air pressure, due to the fact that the inside of the transport pipe is less likely to become clogged. However, if the miscibility of the premixed mortar and water is low, powders such as cement and quick-setting agents and fine aggregate particles are discharged without being completely mixed with the water, which causes dust generation. In addition, the more powder there is in the premixed mortar, the more dust is generated. By increasing the pumping distance after mixing the premixed mortar and water, the mixability is improved, making the mortar uniform, and it is expected that the durability will be improved and dust will be suppressed, but the viscosity of the mortar increases during pumping, which may lead to hose blockages, etc. In addition, there is a demand for further strength improvement in spraying materials that use liquid quick-setting agents.
[0006] Therefore, an object of the present invention is to provide a sprayed mortar which has good pumpability without clogging because the materials are thoroughly mixed, generates little dust when sprayed, and has excellent strength development. [Means for solving the problem]
[0007] As a result of intensive research into the above-mentioned problems, the inventors have discovered that by using fine aggregate of a specific grain size and adjusting the content of thickener, a sprayed mortar can be obtained that has excellent kneadability and pumpability, produces little dust, and exhibits good strength development.
[0008] That is, the present invention is as follows. [1] A spray mortar comprising a mortar composition, a liquid quick-setting admixture and water, wherein the mortar composition comprises cement, a quick-setting aid, a thickener and fine aggregate, the thickener content is 0.01 to 1 part by mass, calculated as solid content, per 100 parts by mass of cement, and the fine aggregate has a particle size of 0.6 mm or more and less than 2 mm, and the content of the particles is 80 mass% or more of the total amount of fine aggregate. [2] The spray mortar according to [1], wherein the quick-setting aid is gypsum and / or calcium aluminates. [3] A spray mortar according to [1] or [2], wherein the thickener is a surfactant-based and / or methylcellulose-based thickener. [4] The spray mortar according to [1] or [2], wherein the water content is 25 to 55 parts by mass per 100 parts by mass of cement. [5] The spray mortar according to [1], wherein the quick-setting aid is a gypsum, and the particle size of the gypsum is such that the mass ratio of particles having a size of 1.5 μm or less is 32 to 52 mass% relative to the total amount of gypsum, and the mass ratio of particles having a size of 10.5 μm or more and 100 μm or less is 10 to 29 mass%. Effect of the Invention
[0009] According to the present invention, it is possible to provide a sprayed mortar which has good pumpability without clogging because the materials are thoroughly mixed, generates little dust when sprayed, and has excellent strength development. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, one embodiment of the present invention will be described in detail.
[0011] The sprayed mortar of the present embodiment contains a mortar composition, a liquid quick-setting admixture, and water.
[0012] The mortar composition includes cement, a quick-setting aid, a viscosity improver and fine aggregate.
[0013] Various types of cement can be used, for example, various types of Portland cement such as ordinary, early strength, ultra-early strength, low heat and moderate heat, ecocement, ultra-rapid hardening cement, fly ash cement, etc. One type of cement may be used alone, or two or more types may be used in combination. The cement is preferably Portland cement. When using Portland cement, the particle size is not particularly limited, for example, 2500 cm according to the JIS standard (JIS R 5210:2019). 2 / g or more.
[0014] The quick-setting aid may include gypsum and / or calcium aluminates.
[0015] Examples of gypsum include anhydrous gypsum, hemihydrate gypsum, and dihydrate gypsum. As the gypsum, anhydrous gypsum is preferable from the viewpoint of further improving the strength development. One type of gypsum may be used alone, or two or more types may be used in combination.
[0016] The particle size of the gypsum is preferably such that the mass ratio of particles of 1.5 μm or less is 32 to 52 mass% and the mass ratio of particles of 10.5 μm or more and 100 μm or less is 10 to 29 mass% relative to the total amount of the gypsum. If the particle size of the gypsum is within the above range, the pumpability is further excellent and it is easy to achieve both initial and long-term strength development. In addition, the maximum particle size of the gypsum is preferably 100 μm or less. Regarding the particle size of the gypsum, the mass ratio of particles having a size of 1.5 μm or less to the total amount of the gypsum is preferably 35 to 50 mass %, and more preferably 37 to 48 mass %. Regarding the particle size of the gypsum, the mass ratio of particles having a size of 10.5 μm or more and 100 μm or less is preferably 12 to 27 mass %, and more preferably 13 to 25 mass %, relative to the total amount of the gypsum. Regarding the particle size of the gypsum, the mass ratio of particles larger than 1.5 μm and smaller than 10.5 μm to the total amount of gypsum is preferably 19 to 58 mass%, more preferably 30 to 55 mass%, and further preferably 35 to 50 mass%. The total mass ratio of particles of 1.5 μm or less and particles of 10.5 μm or more and 100 μm or less is preferably 40 to 80 mass%, more preferably 50 to 70 mass%, and further preferably 55 to 65 mass%. If the particle size of the gypsum is within the above range, better pumpability can be obtained, and the initial and long-term strength development can be further improved.
[0017] The median diameter (d50) of the gypsum is preferably 1.5 to 2.9 μm, more preferably 1.55 to 2.5 μm, and even more preferably 1.6 to 2.3 μm. If the median diameter of the gypsum is within the above range, better pumpability can be obtained, and the initial and long-term strength development can be further improved.
[0018] The particle size, median diameter, maximum particle size, etc. of gypsum can be estimated from the cumulative distribution of particle size distribution measured using a laser diffraction particle size distribution measuring device, etc. The particle size of gypsum can be adjusted by a method of crushing the raw material gypsum in a mill or the like and classifying it, or by a method of mixing gypsum of multiple particle sizes.
[0019] The content of the gypsum is preferably 3 to 15 parts by mass, more preferably 5 to 12 parts by mass, further preferably 7 to 11 parts by mass, and particularly preferably 8.2 to 10 parts by mass, based on 100 parts by mass of cement in terms of anhydride. If the content of the gypsum is within the above range, the amount of dust can be reduced and better strength development can be obtained.
[0020] Calcium aluminate is composed of CaO and Al 2 O 3 It is an inorganic hydrated active substance whose main chemical components are CaO and Al. 2 O 3 The molar ratio of CaO / Al 2 O 3 ) is preferably 2.0 to 2.7, more preferably 2.1 to 2.65, and further preferably 2.15 to 2.6. 2 O 3If the molar ratio of the calcium aluminate is within the above range, it is easy to obtain a more excellent quick-setting property. 2 O 3 Other components such as impurities may also be contained within a range that does not impair the effects of the present invention, regardless of the form in which they are present.
[0021] Calcium aluminate may be crystalline, amorphous, or a mixture thereof. From the viewpoint of obtaining superior long-term strength development, calcium aluminate preferably has a vitrification rate, which is the degree of amorphization, of 95% by mass or less, more preferably 80% by mass or less, and even more preferably 60% by mass or less. The vitrification rate is preferably 40% by mass or more. The fineness of calcium aluminate is not particularly limited, but since it is easy to obtain an appropriate reaction activity when used as a quick-setting admixture for concrete, it is preferable that the fineness is the same as or greater than that of the cement in the hydraulic composition to be mixed, and for example, a Blaine specific surface area of 3000 to 6500 cm 2 The powder size is 0.1 to 1.0 μm / g.
[0022] The content of calcium aluminate is preferably 3 to 15 parts by mass, more preferably 5 to 12 parts by mass, further preferably 7 to 11 parts by mass, and particularly preferably 8.2 to 10 parts by mass, relative to 100 parts by mass of cement. If the content of calcium aluminate is within the above range, better strength development can be obtained while reducing the amount of dust.
[0023] Calcium aluminate is, for example, a raw material that is a CaO source and Al 2 O 3 The raw material is treated as the target chemical components CaO and Al. 2 O 3 The mixture of raw materials is heated until melted, so that the molar ratio of the raw materials is obtained. In addition, since the structural state of calcium aluminate after cooling varies depending on the cooling process after heating during production, the vitrification rate, which is the degree of amorphization, can be adjusted depending on the cooling conditions such as the cooling rate.
[0024] The type of thickener is not particularly limited, and examples thereof include surfactant-based thickeners, cellulose-based thickeners, acrylic thickeners, and guar gum-based thickeners. As thickeners, surfactant-based thickeners and cellulose-based thickeners are preferred. As surfactant-based thickeners, for example, cationic, anionic, nonionic, and amphoteric surfactants are included, and more specifically, polyether-based surfactants and mixtures of alkylarylsulfonic acid and its salts with alkylammonium and its salts are preferred. As cellulose-based thickeners, for example, methylcellulose-based thickeners such as carboxymethylcellulose, methylcellulose, and hydroxypropylmethylcellulose, hydroxyethylcellulose, and hydroxypropylcellulose are included. The thickeners may be used alone or in combination of two or more.
[0025] The content of the thickener is 0.01 to 1 part by mass in terms of solid content relative to 100 parts by mass of cement. If the content of the thickener is outside the above range, dust may not be sufficiently suppressed, or the viscosity of the mortar may become too high, resulting in poor kneadability and pumpability, and reduced strength development. From the viewpoint of easily achieving both reduced dust and good kneadability and pumpability of the mortar, the content of the thickener is preferably 0.03 to 0.8 parts by mass in terms of solid content relative to 100 parts by mass of cement, more preferably 0.05 to 0.5 parts by mass, and even more preferably 0.07 to 0.3 parts by mass.
[0026] Examples of fine aggregates include river sand, silica sand, crushed sand, kansui stone, limestone sand, slag aggregate, etc. Among these, it is preferable to use aggregates such as silica sand and limestone adjusted to a grain size that does not contain fine powder or coarse aggregate as the fine aggregate. One type of fine aggregate may be used alone, or two or more types may be used in combination.
[0027] The particle size of the fine aggregate is such that the content of particles having a size of 0.6 mm or more and less than 2 mm is 80% by mass or more relative to the total amount of the fine aggregate. If the particle size of the fine aggregate is outside the above range, the kneadability decreases. The content of particles having a size of 0.6 mm or more and less than 2 mm is preferably 85% by mass or more relative to the total amount of the fine aggregate, more preferably 90% by mass or more, and even more preferably 95% by mass or more, and may be 100% by mass. Regarding the particle size of the fine aggregate, the content of particles of 0.85 mm or more and less than 2 mm is preferably 50 mass % or more, more preferably 60 mass % or more, further preferably 70 mass % or more, and particularly preferably 80 mass % or more, relative to the total amount of the fine aggregate. The upper limit of the content of particles of 0.6 mm or more and less than 2 mm may be 100 mass % or less, relative to the total amount of the fine aggregate. If the particle size of the fine aggregate is within the above range, the particle size of the fine aggregate becomes uniform, so that the fine aggregate can be easily mixed with a small amount of water, and the strength development is further improved. In this specification, "particles of 0.6 mm or more and less than 2 mm" refers to those that pass through a sieve with a nominal opening of 2 mm and are retained on a 0.6 mm sieve, and "particles of 0.85 mm or more and less than 2 mm" refers to those that pass through a sieve with a nominal opening of 2 mm and are retained on a 0.85 mm sieve.
[0028] The content of the fine aggregate is preferably 70 to 450 parts by mass, more preferably 80 to 350 parts by mass, and even more preferably 90 to 260 parts by mass, relative to 100 parts by mass of cement. When the content of the fine aggregate is within the above range, it is easy to achieve both good pumpability and strength development.
[0029] The mortar composition according to the present embodiment may contain components other than those described above, as long as the effects of the present invention are not impaired. Examples of components that may be contained include a water reducing agent, short fibers, and a pozzolanic reactive substance.
[0030] The mortar composition according to the present embodiment is produced by mixing the above-mentioned components. The mixing method is not particularly limited, and for example, a general-purpose mixer such as a Henschel mixer, a tilting mixer, a pan mixer, a two-shaft mixer, a grout mixer, a mortar mixer, or an omni mixer can be used.
[0031] The liquid quick-setting admixture is not particularly limited as long as it is a liquid quick-setting admixture that can impart quick-setting properties. Examples of the liquid quick-setting admixture include an aluminum sulfate aqueous solution and a sodium silicate aqueous solution. As the liquid quick-setting admixture, an alkali-free liquid quick-setting admixture is preferred from the viewpoint of containing as little alkali metal as possible that can cause deterioration of cement-based constructions, and among these, an aluminum sulfate aqueous solution is preferred. The concentration of the liquid quick-setting admixture is not particularly limited, but it is preferred that the aqueous solution be 20 to 60 mass % in order to have better action on cement.
[0032] The content of the liquid quick-setting admixture is preferably 1 to 10 parts by mass, more preferably 2 to 8 parts by mass, and even more preferably 2.5 to 6 parts by mass, in terms of solid content, relative to 100 parts by mass of cement. If the content of the liquid quick-setting admixture is within the above range, adhesion and strength development are likely to be improved.
[0033] The amount of water in the spray mortar of this embodiment can be adjusted appropriately depending on factors such as the purpose and location of use. The water content is preferably 30 to 60 parts by mass, more preferably 35 to 55 parts by mass, and even more preferably 37 to 52 parts by mass, relative to 100 parts by mass of cement. If the water content is within the above range, the strength expression is even more excellent. In this specification, the water content is calculated by converting the amount of water contained in the liquid quick-setting admixture.
[0034] The prepared mortar composition is mixed with a liquid quick-setting admixture and water to form a sprayed mortar. The addition of the liquid quick-setting admixture and water to the mortar composition may be a wet spraying type in which the mortar composition is mixed with water in advance to prepare a mortar, and the liquid quick-setting admixture is added just before spraying after the mortar composition is pumped, or a dry spraying type in which the mortar composition is pumped and water and the liquid quick-setting admixture are added just before spraying. The addition of the liquid quick-setting admixture and water to the mortar composition is preferably a dry spraying type from the viewpoint that the mortar composition can be pumped over a long distance without coagulation and residues in the piping are less likely to be generated. The liquid quick-setting admixture and water may be added simultaneously, or the water may be added after the liquid quick-setting admixture is added. The device for addition is not particularly limited. As an apparatus, for example, a liquid quick-setting admixture supply pipe and a water supply pipe can be connected to a pressure pipe through which the mortar composition is pumped through the pressure pipe via a junction part such as a Y-shaped pipe or a double pipe, or a mortar spraying apparatus equipped with a mechanism for adding the liquid quick-setting admixture and water can be used.
[0035] The sprayed mortar of this embodiment has a compressive strength of 9 N / mm2 at 3 hours of hardening, measured in a 20°C environment in accordance with the Japan Society of Civil Engineers standard JSCE-G561:2010 "Test method for initial strength of sprayed concrete by pull-out method." 2 It is preferable that the resistance is 10N / mm or more. 2 More preferably, it is 12N / mm 2 If the compressive strength at an age of 3 hours, measured in a 20°C environment, is within the above range, sufficient strength can be obtained early, and construction time can be further shortened.
[0036] The spray mortar of the present embodiment has excellent mixing and pumpability of the mortar composition, produces little dust when sprayed, and exhibits sufficient strength. Therefore, the spray mortar of the present embodiment can be suitably used not only for spraying onto tunnel walls and slopes, but also for spraying into narrow spaces where dust is likely to accumulate. EXAMPLES
[0037] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto. The examples were carried out in an environment of 20°C unless otherwise specified. All blend amounts are calculated on an anhydrous basis and on a solid basis.
[0038] [Preparation of calcium aluminate] Commercially available industrial chemical CaCO 3 and Al 2 O 3 Using CaO and Al 2 O 3 The molar ratio of CaO / Al 2 O 3、 The ingredients were weighed and mixed so as to obtain calcium aluminate with the following calcium aluminate composition (C / A ratio) values, and a raw material mixture was prepared using a Henschel mixer. This raw material mixture was heated in an electric furnace at approximately 1600°C ± 50°C for 60 minutes. With the exception of some, the heated objects were immediately removed from the furnace after the heating time had elapsed. Nitrogen gas for cooling was sprayed onto the surface of the removed heated objects at a maximum flow rate of approximately 30 mL / sec to rapidly cool them, obtaining cooled objects. The vitrification rate of the cooled objects was adjusted by spraying the nitrogen gas at a flow rate slower than the maximum value. Each cooled object was pulverized in an all-steel ball mill and passed through a classification device to obtain a Blaine specific surface area of approximately 5400 cm. 2 The vitrification rate of calcium aluminate was calculated by using a powder X-ray diffractometer to quantify the mass of each mineral contained in calcium aluminate clinker with mass M1 using an internal standard method, calculating the total mass of the mineral phases that could be quantified; M2, and assuming the remainder to be a pure glass phase, using the following formula: Vitrification rate (mass%)={1-(M2 / M1)}×100
[0039] <Experimental Example 1> [material] Premix mortar Cement: Ordinary Portland cement Gypsum: Anhydrite Calcium aluminates: CA1: CaO / Al 2 O 3 =2.3, vitrification rate 50% CA2: CaO / Al 2O 3 =2.4, vitrification rate 90% Fine aggregate: S1: Silica sand, adjusted to 95% by mass of particles between 0.6 mm and 2 mm, and 85% by mass of particles between 0.85 mm and 2 mm S2: Silica sand, adjusted to 90% by mass of particles between 0.6 mm and 2 mm, and 60% by mass of particles between 0.85 mm and 2 mm S3: River sand, adjusted to 35% by mass of particles between 0.6 mm and 2 mm, and 30% by mass of particles between 0.85 mm and 2 mm Thickener: V1: Surfactant-based thickener (polyether-based) V2: Methylcellulose-based thickener Liquid quick-setting agent Alkali-free liquid quick-setting agent (aluminum sulfate 50% by weight aqueous solution)
[0040] [Preparation of premix mortar composition] The cement, calcium aluminate, anhydrous gypsum, fine aggregate and thickener were mixed in the proportions shown in Table 1. These materials were put into a Henschel mixer and mixed for 2 minutes to prepare a premix mortar composition.
[0041] [Table 1]
[0042] [Preparation of spray mortar] The prepared premix mortar composition was pumped through a resin hose pipe with a length of about 50 m and an inner diameter of 4.0 cm using compressed air from a pump. Separately delivered water was added from a water addition port provided on the side near the end of the hose pipe to prepare a premix mortar by allowing the premix mortar composition and water to join together inside the pipe. The premixed mortar mixed with water was sprayed in a shower from a circular quick-setting agent addition section with many addition ports provided around the mortar passage in the device by a spraying device connected to the pipe port on the discharge side of the combined mixture. The sprayed mortar that passed through the quick-setting agent addition section was sprayed through a nozzle for spraying. The liquid quick-setting admixture was added at 3.5 parts by mass (solids equivalent) per 100 parts by mass of cement. The water was added at 38.5 parts by mass per 100 parts by mass of cement. The amount of water was calculated based on the amount of water contained in the liquid quick-setting admixture.
[0043] [Evaluation method] The tests were carried out according to the methods described below, and the test results are shown in Table 2. Pumpability After spraying for 3 minutes, the supply of premixed mortar was stopped for 30 minutes. The supply of premixed mortar was then resumed. If there were any problems with pumping the premixed mortar through the transport pipe or any other problems with spraying, such as a decrease in the amount of mortar sprayed, the pumpability was judged to be "poor." If these phenomena were not observed and the premixed mortar could be pumped smoothly and there was no fluctuation in the amount of mortar sprayed, the pumpability was judged to be "good." · Mixability A mortar mixer was prepared separately from the spraying device described above, and premixed mortar was placed in the mixer beforehand, after which water was added. After adding water, the mortar slurry was mixed for 10 seconds, and the state of the mortar slurry was checked without being scraped off. If the materials were thoroughly mixed, the mixing was judged to be "good," and if they were not completely mixed, the mixing was judged to be "poor." Relative dust generation rate The amount of dust generated during spraying was measured using a commercially available dust concentration meter. The amount of dust generated is shown in Table 2 as a relative percentage (%) of the amount of dust generated when conventional sprayed mortar was sprayed (this is taken as 100%). The conventional sprayed mortar is a premixed mortar containing 100 parts by mass of ordinary Portland cement, 9 parts by mass of calcium aluminate (CA1), 9 parts by mass of anhydrous gypsum, and 200 parts by mass of fine aggregate (S3), and containing no thickener, to which 38.5 parts by mass of water and 3.5 parts by mass of liquid quick-setting agent (converted into solids content) were added. The method and conditions for measuring the amount of dust were as follows. One of the 4.5m x 8m walls in a closed space measuring 4.5m wide, 4.5m deep and 8m high was chosen as the target wall to be sprayed, and the spraying device was set up so that the tip of the spray hole (nozzle) of the device was located on the opposite side to the target wall. A commercially available dust concentration meter was installed 8m away from the target wall and 7m behind the tip of the spray hole. Sprayed mortar was discharged at a rate of 1m from the nozzle of the spraying device. 3 The dust concentration was measured when the dust was sprayed vertically onto the target wall surface at 2000m3 / hr for 5 minutes. Strength development The sprayed mortar was sprayed into a molding form with inner dimensions of 30 x 40 x 20 cm, filling the form. After placing it in a thermostatic chamber at 20°C (±1°C) and leaving it for a specified time, a cylindrical specimen with a diameter of 5 cm and a height of 10 cm was taken from the hardened concrete in the form using a core drill, and a 28-day-old specimen was obtained. The uniaxial compressive strength of this 28-day-old specimen was measured using an Amsler type compressive strength tester. In addition, using the pull-out test form and embedding tool specified in the Japan Society of Civil Engineers standard JSCE-G561:2010, sprayed mortar prepared in the same manner was subjected to a pull-out test in accordance with JSCE-G561:2010. The compressive strength of the sprayed mortar at 3 hours and 1 day was measured by this test. In the table, the entry ">26.9" indicates that the measurement limit of the equipment used was exceeded.
[0044] [Table 2]
[0045] The sprayed mortars of the Examples did not generate dust or clog during pumping, and were excellent in kneadability and short- to long-term strength development. On the other hand, the sprayed mortars of the Comparative Examples were insufficiently mixed, generated dust or clogged during operation, and did not exhibit excellent strength development.
[0046] <Experimental Example 2> [material] Premix mortar Cement: Ordinary Portland cement Gypsum: Anhydrous gypsum, particle size adjusted product, maximum particle size 100μm or less G1: d50 = 2.2, the mass ratio of particles of 1.5 μm or less is 38 mass%, and the mass ratio of particles of 10.5 μm to 100 μm is 23 mass%. G2: d50 = 1.8, the mass ratio of particles of 1.5 μm or less is 42 mass%, and the mass ratio of particles of 10.5 μm to 100 μm is 19 mass%. G3: d50 = 1.7, the mass ratio of particles of 1.5 μm or less is 47 mass%, and the mass ratio of particles of 10.5 μm to 100 μm is 14 mass%. Calcium aluminates: CA1: CaO / Al 2 O 3 =2.3, vitrification rate 50% Fine aggregate: S1: Silica sand, adjusted to 95% by mass of particles between 0.6 mm and 2 mm, and 85% by mass of particles between 0.85 mm and 2 mm V1: Thickener: Surfactant-based thickener (polyether-based) Liquid quick-setting agent Alkali-free liquid quick-setting agent (aluminum sulfate 50% by weight aqueous solution)
[0047] [Preparation of premixed mortar composition and preparation of sprayed mortar] The cement, calcium aluminate, anhydrous gypsum, fine aggregate and thickener were mixed in the proportions shown in Table 3. These materials were put into a Henschel mixer and mixed for 2 minutes to prepare a premix mortar composition. The spray mortar was prepared under the same conditions as in Experimental Example 1.
[0048] [Evaluation method] The test was carried out according to the method described in Experimental Example 1, and the test results are shown in Table 4.
[0049] [Table 3]
[0050] [Table 4]
[0051] The sprayed mortar of the embodiment did not generate dust or clog when pumped, and had excellent mixability and short- to long-term strength development.
Claims
1. A spray mortar comprising a mortar composition, a liquid quick-setting admixture and water, The mortar composition includes cement, a quick-setting aid, a thickener, and a fine aggregate, The content of the thickener is 0.01 to 1 part by mass in terms of solid content per 100 parts by mass of the cement, The particle size of the fine aggregate is such that the content of particles having a size of 0.6 mm or more and less than 2 mm is 80 mass % or more relative to the total amount of the fine aggregate.
2. 2. The sprayed mortar according to claim 1, wherein the quick-setting aid is gypsum and / or calcium aluminates.
3. The spray mortar according to claim 1 or 2, wherein the thickener is a surfactant-based and / or methylcellulose-based thickener.
4. The spray mortar according to claim 1 or 2, wherein the water content is 30 to 60 parts by mass per 100 parts by mass of the cement.
5. The quick-setting aid is a gypsum, The particle size of the gypsum is such that the mass ratio of particles having a size of 1.5 μm or less is 32 to 52 mass% and the mass ratio of particles having a size of 10.5 μm or more and 100 μm or less is 10 to 29 mass% relative to the total amount of the gypsum. The spray mortar according to claim 1.
Citation Information
Patent Citations
Spraying material and spraying technique using the same
JP1998212149A
Curing accelerating assistant material for spraying material
JP1999130500A