Processing method of wafer
The wafer processing method addresses the issue of debris generation by using a phenol novolak resin resist film and a soft polishing pad to remove debris, ensuring high-quality chip production by preventing burrs and maintaining resist film integrity during laser-induced groove formation and plasma etching.
Patent Information
- Application Number
- JP2023063367
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-10
- Publication Date
- 2024-10-23
AI Technical Summary
Conventional wafer processing methods using laser beams generate processing debris such as debris and burrs around grooves, which cannot be effectively removed, leading to poor quality of chips in subsequent processes.
A wafer processing method involving resist film formation, laser-induced groove formation, polishing with a polishing pad, and plasma etching, where a phenol novolak resin resist film is used to protect the device regions and a soft polishing pad is employed to remove debris without damaging the devices.
The method effectively removes processing debris without damaging devices, ensuring high-quality chip production by preventing burrs from adhering to the grooves and maintaining the integrity of the resist film during polishing.
Smart Images

Figure 2024150112000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a wafer processing method. [Background technology]
[0002] As methods for dividing a wafer such as a semiconductor wafer into individual chips, there have been proposed a method in which a laser beam is applied along a planned dividing line set on the wafer to form a groove, and then the wafer is broken along the groove to divide it, and a method in which the wafer is divided by etching using plasma (see Patent Documents 1 and 2). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 10-305420 [Patent Document 2] JP 2018-190857 A Summary of the Invention [Problem to be solved by the invention]
[0004] In the conventional technology, when a groove is formed in a wafer by a laser, processing waste such as debris and burrs are generated around the groove, and if the processing waste is not removed, it leads to poor quality of chips in the subsequent process. As a conventional measure against debris, the wafer is coated with a water-soluble resin before the laser beam is irradiated, and the water-soluble resin is washed away after the laser beam irradiation so that the debris is removed together. However, for example, when a laser beam is irradiated on an oxide film to form a groove, the dissolved oxide film becomes burrs and adheres to the periphery of the groove, and there is a problem that the water-soluble resin is not removed together with the wafer even if the water-soluble resin is washed.
[0005] The present invention has been made in consideration of the above, and an object of the present invention is to provide a wafer processing method capable of removing processing debris generated after irradiation with a laser beam without damaging the device. [Means for solving the problem]
[0006] In order to solve the above-mentioned problems and achieve the object, the wafer processing method of the present invention is a wafer processing method comprising: a resist film forming step of forming a resist film on the surface of the wafer; a processing groove forming step of removing the resist film along a planned dividing line to form a processing groove exposing the wafer; a polishing step of inserting a polishing pad into the processing groove while leaving the resist film formed on the surface of the wafer, to remove processing debris adhering to the periphery of the processing groove; and an etching step of plasma etching the wafer along the processing groove using the resist film as a mask.
[0007] In the wafer processing method, the wafer may have a functional layer laminated on the surface of a substrate, on which a plurality of planned division lines and a plurality of device regions partitioned by the planned division lines are formed, and the processing groove forming step may include removing the resist film and the functional layer to expose the substrate.
[0008] In the wafer processing method, the etching step may divide the wafer to produce a plurality of chips.
[0009] In the above-mentioned wafer processing method, after the etching step, the wafer may be divided by applying an external force to produce a plurality of chips.
[0010] In the wafer processing method, the groove forming step may involve irradiating a laser beam.
[0011] In the above-described wafer processing method, the polishing step may include supplying a polishing liquid containing abrasive grains to the polishing pad and the wafer.
[0012] In the wafer processing method, the functional layer may include an oxide film.
[0013] In the wafer processing method, the resist film may contain a phenol novolac resin.
[0014] In the above-described wafer processing method, the polishing pad may include suede or nonwoven fabric. Effect of the Invention
[0015] The present invention has an effect of being able to remove processing debris generated after irradiation with a laser beam without damaging the device. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is a perspective view showing an example of a wafer to be processed by the processing method according to the embodiment. [Diagram 2] FIG. 2 is a perspective view showing a configuration example of a laser processing apparatus for performing the wafer processing method according to the embodiment. [Diagram 3] FIG. 3 is a flowchart showing the flow of the wafer processing method according to the embodiment. [Figure 4] FIG. 4 is a diagram for explaining an example of the resist film forming step shown in FIG. [Diagram 5] FIG. 5 is a diagram for explaining an example of the processed groove forming step shown in FIG. [Figure 6] FIG. 6 is a diagram for explaining an example of a polishing pad used in the polishing step shown in FIG. [Figure 7] FIG. 7 is a diagram for explaining an example of the polishing step shown in FIG. [Figure 8] FIG. 8 is a diagram for explaining an example of the etching step shown in FIG. [Figure 9] FIG. 9 shows the experimental results showing the relationship between the height of the processing debris and the Shore hardness of the polishing pad. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. The present invention is not limited to the contents described in the following embodiment. Furthermore, the components described below include those that a person skilled in the art can easily imagine and those that are substantially the same. Furthermore, the configurations described below can be appropriately combined. Furthermore, various omissions, substitutions, or modifications of the configurations can be made without departing from the gist of the present invention.
[0018] [Embodiment] A method for processing a wafer 10 according to an embodiment of the present invention will be described with reference to the drawings. First, a wafer 10 to be processed and a configuration example of a laser processing device 100 used for processing will be described. Fig. 1 is a perspective view showing an example of a wafer 10 to be processed by the processing method according to the embodiment. Fig. 2 is a perspective view showing an example of a configuration of a laser processing device 100 that performs the method for processing a wafer 10 according to the embodiment.
[0019] The wafer 10 shown in FIG. 1 is a disk-shaped semiconductor device wafer, optical device wafer, or the like, having a substrate 11 made of silicon (Si), sapphire (Al2O3), gallium arsenide (GaAs), silicon carbide (SiC), lithium tantalate (LiTaO3), or the like.
[0020] The wafer 10 has a plurality of planned dividing lines 13 set on the surface 12. The planned dividing lines 13 are a first planned dividing line 13-1 and a second planned dividing line 13-2. The first planned dividing lines 13-1 extend along a first direction 21, and a plurality of the first planned dividing lines 13-1 are set side by side in a second direction 22 intersecting the first direction 21. The second planned dividing lines 13-2 extend along the second direction 22, and a plurality of the second planned dividing lines 13-2 are set side by side in the first direction 21. In the embodiment, the first direction 21 and the second direction 22 are perpendicular to each other.
[0021] The wafer 10 has devices 15 formed in areas partitioned by first dividing lines 13-1 and second dividing lines 13-2 set in a lattice pattern. The devices 15 are, for example, integrated circuits such as ICs (Integrated Circuits) or LSIs (Large Scale Integrations), image sensors such as CCDs (Charge Coupled Devices) or CMOSs (Complementary Metal Oxide Semiconductors), or MEMS (Micro Electro Mechanical Systems).
[0022] The wafer 10 is transported and processed while being supported by, for example, an annular frame 30 and a tape 31 as shown in FIG. 2. The frame 30 is an annular plate member formed of metal or resin and having an opening larger than the outer diameter of the wafer 10. The tape 31 is in the form of a sheet having an outer diameter larger than the opening of the frame 30, and is attached to the rear surface side of the frame 30 so as to cover the opening of the frame 30. The tape 31 may be configured to include, for example, a base layer made of a synthetic resin having elasticity, and a glue layer laminated on the base layer and made of a synthetic resin having elasticity and adhesiveness, or may be configured of a resin having thermoplasticity without having a glue layer.
[0023] The wafer 10 is positioned at a predetermined position in the opening of the frame 30, and fixed to the frame 30 and the tape 31 by adhering the front surface 12 or back surface 16 side to the tape 31. The wafer 10 is divided into individual devices 15 along a plurality of planned division lines 13, and is singulated into device chips 17. Note that, although the device chips 17 are square-shaped in the embodiment, they may also be rectangular-shaped. Also, although the wafer 10 is disc-shaped in the embodiment, it does not have to be disc-shaped in the present invention.
[0024] The laser processing apparatus 100 shown in FIG. 2 processes the wafer 10 by irradiating the wafer 10, which is an object of processing, with a laser beam 122. As shown in the figure, the laser processing apparatus 100 includes a holding table 110, a laser beam irradiation unit 120, a moving unit 140, a display unit 150, and a control unit 160. In the following description, the X-axis direction is one direction on a horizontal plane. The Y-axis direction is a direction perpendicular to the X-axis direction on a horizontal plane. The Z-axis direction is a direction perpendicular to the X-axis direction and the Y-axis direction. In the laser processing apparatus 100 of the embodiment, the processing feed direction is the X-axis direction, the indexing feed direction is the Y-axis direction, and the focal point position adjustment direction is the Z-axis direction.
[0025] The holding table 110 holds the wafer 10 on a holding surface 111. The holding surface 111 is a disk shape made of porous ceramics or the like. In the embodiment, the holding surface 111 is a plane parallel to the horizontal direction. The holding surface 111 is connected to a vacuum suction source, for example, via a vacuum suction path. The holding table 110 suction-holds the wafer 10 placed on the holding surface 111. A plurality of clamps 112 that clamp the frame 30 that supports the wafer 10 are arranged around the holding table 110.
[0026] The holding table 110 is rotated around an axis parallel to the Z-axis direction by a rotation unit 113. The rotation unit 113 is supported by an X-axis direction moving plate 114. The rotation unit 113 and the holding table 110 are moved in the X-axis direction by a processing feed unit 141 of the moving unit 140 via the X-axis direction moving plate 114. The rotation unit 113 and the holding table 110 are moved in the Y-axis direction by an indexing feed unit 142 of the moving unit 140 via the X-axis direction moving plate 114, the processing feed unit 141, and the Y-axis direction moving plate 115.
[0027] The laser beam application unit 120 is a unit that applies a pulsed laser beam 122 having a predetermined wavelength for processing the wafer 10 to the wafer 10 held on the holding table 110. In the embodiment, a part of the laser beam application unit 120 including an application head 121 is supported on a tip of a support beam 103 whose base end is attached to an erect wall 102 erected from the apparatus body 101.
[0028] The laser beam application unit 120 has, for example, an oscillator that emits a laser beam 122, a collector that focuses and irradiates the laser beam 122 emitted from the oscillator to a processing point, and various optical components that guide the laser beam 122 from the oscillator to the collector. The collector is provided inside the application head 121. A focus point 123 of the laser beam 122 that is focused by the collector and irradiated from the application head 121 can be moved relatively to the holding table 110 in the Z-axis direction, which is the focus point position adjustment direction, by, for example, a focus point position adjustment unit (not shown).
[0029] The moving unit 140 is a unit that relatively moves the holding table 110 and the focal point of the laser beam 122 emitted from the laser beam application unit 120. The moving unit 140 includes a processing feed unit 141 and an indexing feed unit 142.
[0030] The processing feed unit 141 is a unit that relatively moves the holding table 110 and the focal point of the laser beam 122 irradiated from the laser beam application unit 120 in the X-axis direction, which is the processing feed direction. In the embodiment, the processing feed unit 141 moves the holding table 110 in the X-axis direction. In the embodiment, the processing feed unit 141 is installed on the device body 101 of the laser processing device 100. The processing feed unit 141 supports the X-axis moving plate 114 so as to be freely movable in the X-axis direction.
[0031] The indexing feed unit 142 is a unit that relatively moves the holding table 110 and the focal point of the laser beam 122 irradiated from the laser beam application unit 120 in the Y-axis direction, which is the indexing feed direction. In the embodiment, the indexing feed unit 142 moves the holding table 110 in the Y-axis direction. In the embodiment, the indexing feed unit 142 is installed on the apparatus body 101 of the laser processing apparatus 100. The indexing feed unit 142 supports the Y-axis moving plate 115 so as to be freely movable in the Y-axis direction.
[0032] The processing feed unit 141 and the indexing feed unit 142 each include, for example, a known ball screw, a known pulse motor, and a known guide rail. The ball screw is provided so as to be rotatable about its axis. The pulse motor rotates the ball screw about its axis. The guide rail of the processing feed unit 141 is provided so as to be fixed to the Y-axis direction moving plate 115, and supports the X-axis direction moving plate 114 so as to be movably in the X-axis direction. The guide rail of the indexing feed unit 142 is provided so as to be fixed to the device body 101, and supports the Y-axis direction moving plate 115 so as to be movably in the Y-axis direction.
[0033] The display unit 150 is a display section configured by a liquid crystal display device or the like. The display unit 150 displays, for example, a setting screen for processing conditions, a state of processing operation, and the like on a display surface. When the display surface of the display unit 150 includes a touch panel, the display unit 150 may include an input section. The input section can receive various operations such as an operator registering processing content information. The input section may be an external input device such as a keyboard. The display unit 150 switches information and images displayed on the display surface by an operation from the input section or the like. The display unit 150 may include an alarm device. The alarm device emits at least one of sound and light to notify the operator of the laser processing apparatus 100 of predetermined alarm information. The alarm device may be an external alarm device such as a speaker or a light-emitting device.
[0034] The control unit 160 controls each of the above-mentioned components of the laser processing apparatus 100, and causes the laser processing apparatus 100 to execute a processing operation on the wafer 10. The control unit 160 is a computer including an arithmetic processing device as a calculation means, a storage device as a storage means, and an input / output interface device as a communication means. The arithmetic processing device includes, for example, a microprocessor such as a CPU (Central Processing Unit). The storage device has a memory such as a ROM (Read Only Memory) or a RAM (Random Access Memory). The arithmetic processing device performs various calculations based on a predetermined program stored in the storage device. The arithmetic processing device outputs various control signals to each of the above-mentioned components via the input / output interface device according to the calculation results, and controls the laser processing apparatus 100.
[0035] The configuration example of the laser processing apparatus 100 according to the present embodiment has been described above. Note that the above configuration described with reference to Fig. 2 is merely an example, and the configuration of the laser processing apparatus 100 according to the present embodiment is not limited to this example. The functional configuration of the laser processing apparatus 100 according to the present embodiment can be flexibly modified according to the specifications and operation.
[0036] (Wafer Processing Method) Next, a method for processing the wafer 10 according to the present embodiment will be described. FIG. 3 is a flow chart showing the flow of the method for processing the wafer 10 according to the embodiment. FIG. 4 is a diagram for explaining an example of the resist film forming step shown in FIG. 3. FIG. 5 is a diagram for explaining an example of the processed groove forming step shown in FIG. 3. FIG. 6 is a diagram for explaining an example of a polishing pad used in the polishing step shown in FIG. 3. FIG. 7 is a diagram for explaining an example of the polishing step shown in FIG. 3. FIG. 8 is a diagram for explaining an example of the etching step shown in FIG. 3.
[0037] 3 is a method for processing a wafer 10 in which a plurality of division lines 13 and a plurality of device regions partitioned by the division lines 13 are formed in a functional layer laminated on the surface of a substrate 11. The processing method 1000 includes a resist film forming step 1100, a groove forming step 1200, a polishing step 1300, and an etching step 1400. In this embodiment, the processing method 1000 executes the steps in the order of the resist film forming step 1100, the groove forming step 1200, the polishing step 1300, and the etching step 1400.
[0038] First, the processing method 1000 executes a resist film forming step 1100. The resist film forming step 1100 is a step of forming a resist film on the surface of the functional layer of the wafer 10. In the resist film forming step 1100, a resin coating device (not shown) applies a resist film to cover the entire surface of the wafer 10 while the back side of the wafer 10 is held by suction on the holding surface of a spinner table.
[0039] In this embodiment, as shown in Fig. 4, the wafer 10 has a functional layer 18 formed by laminating an insulating film and a functional film forming a circuit on the surface of a substrate 11 such as silicon having a thickness of, for example, 140 µm. The functional layer 18 includes an oxide film, and devices 15 are formed in a plurality of regions partitioned by a plurality of planned division lines 13 formed in a lattice pattern. A tape 31 is attached to the back surface of the substrate 11.
[0040] The processing method 1000 forms a resist film 19 on the wafer 10 by laminating the resist film 19 on the surface of the functional layer 18. In this embodiment, the resist film 19 is formed to a thickness of, for example, 1 to 5 μm. The resist film 19 may be configured to include, for example, a phenol novolac resin-based resist, a water-soluble resin such as HOGOMAX (registered trademark) manufactured by Disco Corporation, or the like. For example, when a water-soluble resin is used as a mask during plasma etching, it may be removed during polishing. For this reason, in this embodiment, the resist film 19 includes a phenol novolac resin-based resist. The resist film 19 is preferably made of a material with high adhesion that does not peel off from the wafer 10 during polishing. In addition, when a water-soluble resin is used, polishing may be performed by dry polishing.
[0041] Furthermore, the experimental results showed that cyclized rubber-based resists have low adhesion to the wafer 10 and peel off from the wafer 10 during polishing, making them unsuitable for the resist film 19. On the other hand, it was found that phenol novolac resin-based resists have excellent adhesion to the wafer 10 and do not peel off from the wafer 10 during polishing, making them suitable for a protective film. It was also found that the polishing speed of the phenol novolac resin-based resist is slower than that of an oxide film, making it possible to protect the pattern.
[0042] As shown in FIG. 3, the processing method 1000 executes a processed groove forming step 1200 after the resist film forming step 1100 is completed. The processed groove forming step 1200 is a step of removing the resist film 19 and the functional layer 18 along the division lines 13 of the wafer 10 to form a processed groove that exposes the substrate 11. As shown in FIG. 5, the processed groove forming step 1200 irradiates the wafer 10 with a laser beam having a wavelength absorbed by the wafer 10 from the laser beam applying unit 120 along the division lines 13 while the laser processing device 10 moves the wafer 10 and the laser beam applying unit 120 relatively along the division lines 13. In this embodiment, in the processed groove forming step 1200, the laser processing device 100 sets a focusing point of the laser beam on the surface of the resist film 19 or the surface of the substrate 11, and irradiates the wafer 10 with the laser beam from the irradiation head 121 along each division line 13. In the groove formation step 1200, the laser processing apparatus 100 performs ablation processing on the resist film 19, functional layer 18 and substrate 11 on each planned division line 13, removing portions of these and forming grooves 14 at each planned division line 13 that divide the functional layer 18.
[0043] In the example shown in FIG. 5, the processing groove forming step 1200 shows a state in which the processing groove 14 of the resist film 19 is recessed by the heat of the laser beam, and processing debris 300 is generated in the exposed region 18-1 of the functional layer 18. The processing debris 300 includes debris, burrs, etc. If the processing debris 300 is not removed from the wafer 10, there is a problem that it will lead to poor quality of the device chip 17 in a later process. The debris countermeasure is to cover the wafer 10 with a water-soluble resin before the irradiation of the laser beam, and to wash away the water-soluble resin after the irradiation of the laser beam so that the debris is removed together. However, for example, when the laser beam is irradiated to an oxide film to form the processing groove 14, the dissolved oxide film becomes a burr and adheres to the periphery of the processing groove, and there is a problem that the water-soluble resin is not removed together with the processing debris even if the water-soluble resin is washed. For this reason, the processing method 1000 of the wafer 10 according to this embodiment realizes a method for removing the processing debris 300 generated after the irradiation of the laser beam without damaging the device 15.
[0044] As shown in FIG. 3, the processing method 1000 executes a polishing step 1300 after the processing groove forming step 1200 is completed. The polishing step 1300 is a step in which a polishing pad is inserted into the processing groove 14 to remove processing debris 300 attached to the periphery of the processing groove 14 while leaving the resist film 19 formed on the region of the device 15 of the wafer 10. As shown in FIG. 6, the polishing step 1300 uses a polishing pad 232 containing suede or nonwoven fabric to perform polishing and remove the processing debris 300. The polishing step 1300 uses a soft polishing pad 232 so as not to polish the pattern of the wafer 10, and has the characteristic of polishing many corners of steps. When the polishing pad 232 is pressed against the resist film 19 from above, it enters the processing groove 14 and performs polishing.
[0045] The polishing step 1300 uses a slurry that is easy to polish the oxide film debris and difficult to polish the resist film 19. The slurry is a polishing liquid, and may be a single chemical liquid, or a mixture of multiple chemical liquids diluted with water to a predetermined concentration. In this embodiment, the polishing step 1300 uses a slurry that is easier to polish the oxide film than the resist film 19 when the resist film 19 and the oxide film are used. Specifically, the slurry has an alkalinity of 9 to 11 pH, colloidal silica particles of 40 to 150 nm, and an abrasive concentration of 5 to 20%. For example, when a 0.5 μm resist film 19 is polished, there is a difference in the polishing rate such that a 2 μm oxide film is removed. For this reason, in this embodiment, the time required to remove the processing debris 300 such as burrs is obtained in advance by experiment, and polishing is performed for a predetermined time, so that the resist film 19 is not removed and remains due to the difference in polishing rate.
[0046] As shown in FIG. 7, the polishing apparatus 200 that performs the polishing step 1300 includes a polishing unit 210. The polishing unit 210 is mounted so as to be movable in the vertical direction along a guide rail (not shown). The polishing unit 210 includes a spindle 222 rotatably accommodated in a housing, a wheel mount 226 fixed to the tip of the spindle 222, and a polishing wheel 228 detachably mounted on the wheel mount 226. The spindle 222 is driven to rotate by a servo motor 24 (not shown). The polishing wheel 228 includes a wheel base 230 and a polishing pad 232 bonded to the lower surface of the wheel base 230. A slurry supply path 223 is formed in the spindle 222, and a slurry supply path 233 that connects to the slurry supply path 23 of the spindle 222 is also formed in the polishing wheel 228. A slurry supply passage 223 of the spindle 222 communicates with a slurry supply source 250 that supplies a slurry containing abrasive grains, and supplies the slurry to the polishing point.
[0047] The polishing apparatus 200 includes a holding table 234. The holding table 234, like the holding table 110 described above, is capable of holding the wafer 10 by suction, and is rotated by a rotation unit about an axis parallel to the vertical direction.
[0048] In the polishing step 1300, while supplying slurry from the slurry supply source 250 to the wafer 10 held on the holding table 234, the holding table 234 is rotated at a predetermined rotation speed, and the polishing wheel 228 is rotated at a speed different from the rotation speed of the holding table 234 while the polishing pad 232 is brought into contact with the resist film 19 of the wafer 10 with a predetermined pressure, so that the polishing pad 232 slides against the wafer 10 to polish the resist film 19 of the wafer 10. In this case, the polishing step 1300 adjusts the thickness of the resist film 19 so that a sufficient thickness of the resist film 19 remains to protect the region of the device 15 in plasma etching. As a result, the processing method 1000 can remove the processing debris 300 while preventing damage to the device 15 by polishing the region of the wafer 10 in a state where the region of the device 15 is covered with the resist film 19.
[0049] As shown in Fig. 3, in the processing method 1000, after the polishing step 1300 is completed, an etching step 1400 is performed. The etching step 1400 is a step of plasma etching the substrate 11 along the processed groove 14 using the resist film 19 as a mask. In the etching step 1400, a plasma etching device (not shown) holds the back side of the wafer 10 on the holding surface of a holding table via a tape 31. As shown in scene 1401 of Fig. 8, in the etching step 1400, high frequency power for generating and maintaining plasma is applied to the upper electrode, and high frequency power for attracting ions is applied to the holding table, which is the lower electrode, while an etching gas 500 is supplied to the resist film 19 side of the wafer 10.
[0050] Then, as shown in scene 1402 of FIG. 8, in the etching step 1400, the plasma etching apparatus converts the etching gas 500 in the space between the holding table and the upper electrode into plasma, and this plasmatized etching gas 500 is drawn toward the wafer 10 to etch (so-called plasma etching) the substrate 11 exposed at the bottom of the groove 14 formed in the resist film 19, which is a mask for the wafer 10, thereby progressing the groove 14 toward the back surface of the wafer 10.
[0051] In the etching step 1400, the plasma etching device plasma etches the wafer 10 until the processed grooves 14 open on the back side of the wafer 10 and the wafer 10 is divided into device chips 17, as shown in Fig. 8. Thus, the etching step 1400 divides the wafer 10 to manufacture a plurality of device chips 17. When the etching step 1400 is completed, the processing method 1000 ends the processing procedure shown in Fig. 3.
[0052] As described above, the processing method 1000 for the wafer 10 forms the resist film 19 on the surface of the functional layer 18 of the wafer 10, and forms the processing groove 14 along the planned dividing line 13 of the wafer 10 by removing the resist film 19 and the functional layer 18 to expose the substrate 11. The processing method 1000 causes the polishing pad 232 to enter the processing groove 14 while leaving the resist film 19 formed on the device 15 region of the wafer 10, and removes the processing debris 300 attached to the periphery of the processing groove 14, and performs plasma etching on the substrate 11 along the processing groove 14 using the resist film 19 as a mask. In this way, the processing method 1000 can remove the processing debris 300 generated along the processing groove 14 of the wafer 10 by the polishing pad 232, thereby suppressing quality defects of the device chips 17.
[0053] Moreover, in the processing method 1000, the laser beam is irradiated by the laser processing device 100 in the processed groove forming step 1200. As a result, in the processing method 1000, the resist film 19 of the wafer 10 is receded by the laser beam, and a part of the functional layer 18 becomes a burr around the processed groove 14, but since it can be removed by the polishing pad 232, it is possible to prevent the burr from adhering to the periphery of the processed groove 14. Therefore, in the processing method 1000, the processing chips 300 generated after the irradiation of the laser beam can be removed without damaging the device 15.
[0054] Furthermore, in the processing method 1000, a slurry (polishing liquid) containing abrasive grains is supplied to the polishing pad 232 and the wafer 10 in the polishing step 1300. As a result, the processing method 1000 does not remove the resist film 19 on the wafer 10, and therefore the resist film 19 can remain in a thickness sufficient to protect the device 15 region.
[0055] Moreover, in the processing method 1000, the functional layer 18 of the wafer 10 includes an oxide film. As a result, in the processing method 1000, when a laser beam is irradiated onto the oxide film of the functional layer 18 to form a processed groove, even if the dissolved oxide film becomes a burr and adheres to the periphery of the processed groove, the burr can be removed by the polishing pad 232.
[0056] Moreover, in the processing method 1000, the resist film 19 of the wafer 10 contains a phenol novolac resin. As a result, in the processing method 1000, the phenol novolac resin has better adhesion to the wafer 10 than a cyclized rubber-based resist, so that the resist film 19 is less likely to peel off from the wafer 10, and the pattern of the wafer 10 can be reliably protected.
[0057] In addition, in the processing method 1000, the polishing pad 232 includes suede or nonwoven fabric. As a result, in the processing method 1000, the polishing pad 232 can be brought into close contact with the periphery of the processing groove 14 of the wafer 10 for polishing, so that the processing chips 300 generated along the processing groove 14 can be removed more reliably.
[0058] In the above-described processing method 1000, the polishing step 1300 is described as polishing while supplying a slurry containing abrasive grains to the polishing pad 232 and the wafer 10, but is not limited thereto. For example, the processing method 1000 may be dry polishing in which polishing is performed by a polishing pad containing abrasive grains.
[0059] In the above-described processing method 1000, in the etching step 1400, the wafer 10 may be fully cut by plasma etching and divided into chips, or may be only half-cut and divided into chips in a later process.
[0060] The above-described processing method 1000 has been described as a case in which the etching step 1400 is performed after the polishing step 1300, but is not limited thereto. For example, the processing method 1000 may be a processing procedure in which the polishing step 1300 is performed after the etching step 1400.
[0061] (Experimental Results) For example, if the polishing pad 232 is hard, the pad may not come into contact with the processing debris 300 (e.g., burrs) adhering to the periphery of the processing groove 14 on the front surface 12 of the wafer 10, and polishing may not be possible. An example of an experimental result in which polishing was performed by changing the Shore hardness (hardness) of the polishing pad 232 in the polishing step 1300 of the above-mentioned processing method 1000 will be described below.
[0062] 9 shows the experimental results showing the relationship between the height of the processing chips 300 and the Shore hardness of the polishing pad 232. In FIG. 9, the vertical axis shows the height (μm) of the processing chips 300, and the horizontal axis shows the Shore hardness (HS) of the polishing pad 232. As shown in FIG. 9, when the height of the processing chips 300 before polishing is 2 μm, if a polishing pad 232 with a Shore hardness of 35 is used in the polishing step 1300, the height of the processing chips 300 after polishing becomes almost zero, and it was confirmed that the processing chips 300 are removed. When the height of the processing chips 300 before polishing is 2 μm, if a polishing pad 232 with a Shore hardness of 45 is used in the polishing step 1300, the height of the processing chips 300 after polishing becomes almost zero, and it was confirmed that the processing chips 300 are removed. When the height of the machining chips 300 before polishing is 2 μm, if a polishing pad 232 with a Shore hardness of 52 is used in the polishing step 1300, the height of the machining chips 300 after polishing is 1 μm, and the height of the machining chips 300 is significantly reduced. When the height of the machining chips 300 before polishing is 2 μm, if a polishing pad 232 with a Shore hardness of 60 is used in the polishing step 1300, the height of the machining chips 300 after polishing does not change, and it was confirmed that the machining chips 300 are not removed.
[0063] In this way, in the polishing step 1300 of the above-mentioned processing method 1000, when a polishing pad 232 having a Shore hardness of 55 or less is used, the height of the processing debris 300 is significantly reduced, and further, when a polishing pad 232 having a Shore hardness of 45 or less is used, the height of the processing debris 300 becomes almost zero and the processing debris 300 is removed, as confirmed by the experimental results.
[0064] In addition, in the above-mentioned processing method 1000, when the polishing pad 232 is made of polyurethane, the pad is too hard to enter the processing groove 14, and the processing debris 300 is not removed. Furthermore, in the above-mentioned processing method 1000, the surface 12 side of the wafer 10 is polished with a chemical solution that does not contain abrasive grains and a polishing pad that does not contain abrasive grains, thereby reducing damage to the surface 12 of the wafer 10 and reducing the height of the processing debris 300. The type of chemical includes, for example, an organic alkali chelating agent. However, the wafer 10 with a protective film (resist) is less likely to scratch the surface 12 of the wafer 10 with the processing debris 300 or the polishing pad 232, and therefore there is less risk. [Explanation of symbols]
[0065] 10 wafers 11 Substrate 12 Surface 13 Division line 14 Machining groove 15 Devices 17 Device Chip 18 Functional Layer 18-1 Exposure area 19 Resist film 31 Tape 100 Laser processing equipment 110 Holding table 120 Laser beam irradiation unit 121 Irradiation head 122 Laser beam 123 Focus point 140 Mobile Units 141 Processing feed unit 142 Indexing feed unit 150 display units 160 Control Unit 200 Polishing equipment 210 Polishing Unit 222 Spindle 226 Wheel mount 228 Abrasive Wheel 230 Wheel base 232 Polishing Pad 233 Slurry supply line 250 Slurry Source 300 Processing waste 500 Etching gas 1000 Processing method 1100 Resist film formation step 1200 Groove forming step 1300 Polishing Steps 1400 Etching Steps
Claims
1. A wafer processing method comprising the steps of: a resist film forming step of forming a resist film on a surface of the wafer; a groove forming step of removing the resist film along a planned dividing line to form a groove for exposing the wafer; a polishing step of removing processing debris adhering to the periphery of the processing groove by inserting a polishing pad into the processing groove while leaving the resist film formed on the surface of the wafer; an etching step of plasma etching the wafer along the etched groove using the resist film as a mask.
2. The wafer has a functional layer laminated on a surface of a substrate, and a plurality of division lines and a plurality of device regions partitioned by the division lines are formed in the functional layer.
2. The wafer processing method according to claim 1, wherein the groove forming step removes the resist film and the functional layer to expose the substrate.
3. 3. The wafer processing method according to claim 1, wherein the etching step divides the wafer into a plurality of chips.
4. 3. The wafer processing method according to claim 1, further comprising the step of: dividing the wafer by applying an external force to the wafer after the etching step, thereby producing a plurality of chips.
5. 3. The wafer processing method according to claim 1, wherein the groove forming step comprises irradiating a laser beam.
6. 3. The method for processing a wafer according to claim 1, wherein the polishing step comprises supplying a polishing liquid containing abrasive grains to the polishing pad and the wafer.
7. 3. The wafer processing method according to claim 2, wherein the functional layer includes an oxide film.
8. The resist film is characterized in that it contains a phenol novolac resin.
3. The wafer processing method according to claim 1 or 2.
9. 3. The method for processing a wafer according to claim 1, wherein the polishing pad includes at least one of suede and nonwoven fabric.
Citation Information
Patent Citations
Method for fabricating matrix made up of oxide single crystal and method for manufacturing functional device
JP1998305420A
Wafer processing method
JP2018190857A