Stripping agent and stripping method
A solvent-based release agent using dialkylene glycol monoalkyl ether acetate and diacetate effectively removes polyurethane layers from polyester materials like PET and PEN, ensuring recyclability by not dissolving the polyurethane.
Patent Information
- Application Number
- JP2023027347
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-02-24
- Publication Date
- 2024-11-27
- Estimated Expiration
- 2043-02-24
Smart Images

Figure 0007591075000001 
Figure 0007591075000002 
Figure 0007591075000003
Abstract
Description
[Technical field]
[0001] FIELD OF THE DISCLOSURE The present invention relates to a release agent and a release method, and more particularly to a release agent for releasing a polyurethane layer adhered to a polyester substrate, and a release method using the same. [Background technology]
[0002] Coated substrates in which a resin substrate is coated with another resin layer on its surface are used in various applications including optical applications, and for example, a polyurethane layer is provided on a PET film as a resin substrate. From the viewpoint of effective use of resources, it is desirable to recycle the resin substrate by removing the resin layer from such coated substrates.
[0003] Patent Document 1 describes an adhesive treatment liquid capable of easily removing various types of adhesives from an adhesive tape containing a substrate and an adhesive, and describes that the adhesive treatment liquid contains a liquid having a Hansen solubility parameter value of 31 or less and an alkaline compound. Also, organic solvents such as methanol and ethanol are described as examples of the liquid having a Hansen solubility parameter value of 31 or less. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2022 / 004609 Summary of the Invention [Problem to be solved by the invention]
[0005] The present inventors have studied a release agent for peeling off the polyurethane layer of a coated substrate having a polyurethane layer on a polyester substrate, in order to enable recycling of the polyester substrate. Such a release agent is required to be able to peel off the polyurethane layer, and is also required not to damage the polyester substrate. In addition, from the viewpoint of enabling repeated use of the release agent, it is also required that the polyurethane layer is not easily dissolved by the release agent, i.e., that the release agent is insoluble.
[0006] In view of the above, an object of an embodiment of the present invention is to provide a release agent that does not easily attack a polyester substrate and does not easily dissolve a polyurethane layer, yet has excellent releasability. [Means for solving the problem]
[0007] The present invention includes the embodiments set forth below. [1] A release agent for removing a polyurethane layer adhered to a polyester substrate formed from a polyester having an aromatic dicarboxylic acid and ethylene glycol as its constituent components, the release agent comprising at least one member selected from the group consisting of dialkylene glycol monoalkyl ether acetates, dialkylene glycol diacetates, and trialkylene glycol diacetates.
[0008] [2] The stripping agent according to [1], which contains 40 mass% or more of at least one selected from the group consisting of dialkylene glycol monoalkyl ether acetate, dialkylene glycol diacetate, and trialkylene glycol diacetate. [3] The release agent according to [1] or [2], wherein the polyurethane forming the polyurethane layer has an acid value of 0 to 40 mgKOH / g. [4] The release agent according to any one of [1] to [3], wherein the polyurethane that forms the polyurethane layer is a polyurethane containing polyester polyol as a raw material. [5] The release agent according to any one of [1] to [4], wherein the polyester substrate is a polyethylene terephthalate substrate, a polyethylene naphthalate substrate, or a polyethylene furanoate substrate. [6] The at least one selected from the group consisting of dialkylene glycol monoalkyl ether acetate, dialkylene glycol diacetate, and trialkylene glycol diacetate is at least one selected from the group consisting of a compound represented by the following general formula (1) and a compound represented by the following general formula (2): [ka] In formula (1), R 1 represents an alkyl group having 1 to 6 carbon atoms, and R 2 represents an alkanediyl group having 2 to 4 carbon atoms, and in formula (2), R 3 represents an alkanediyl group having 2 to 4 carbon atoms, and n represents 2 or 3. The stripping agent according to any one of [1] to [5].
[0009] [7] A peeling method using the release agent according to any one of [1] to [6], comprising immersing a coating substrate, which is a polyester substrate formed of a polyester containing an aromatic dicarboxylic acid and ethylene glycol as constituent components and has a polyurethane layer provided thereon, in the release agent, and peeling off the polyurethane layer from the polyester substrate. Effect of the Invention
[0010] The release agent according to the embodiment of the present invention is unlikely to attack the polyester substrate and is unlikely to dissolve the polyurethane layer, yet is capable of releasing the polyurethane layer adhered to the polyester substrate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The release agent according to this embodiment is a release agent for releasing a polyurethane layer adhered to a polyester substrate.
[0012] The subject of treatment with the release agent is a coated substrate having a polyurethane layer provided on a polyester substrate. The coated substrate includes a polyester substrate and a polyurethane layer formed as a resin film on at least one of the front and rear surfaces of the polyester substrate, with the polyurethane layer adhered to the polyester substrate.
[0013] In this embodiment, the polyester substrate is formed from a polyester having aromatic dicarboxylic acid and ethylene glycol as constituent components (monomers). That is, the polyester forming the polyester substrate is obtained by polycondensation of aromatic dicarboxylic acid and ethylene glycol.
[0014] The aromatic dicarboxylic acid constituting the polyester is a dicarboxylic acid having an aromatic ring, and the aromatic ring may be an aromatic ring consisting of only hydrocarbons or a heteroaromatic ring. Examples of aromatic dicarboxylic acids include terephthalic acid, isophthalic acid, phthalic acid, naphthalenedicarboxylic acid (e.g., 1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 1,8-naphthalenedicarboxylic acid), diphenyldicarboxylic acid (e.g., 4,4'-diphenyldicarboxylic acid), and furandicarboxylic acid (e.g., 2,5-furandicarboxylic acid), and any one of these may be used, or two or more may be used in combination.
[0015] The polyester may contain a polycarboxylic acid other than the aromatic dicarboxylic acid as a constituent component. The polyester may also contain a diol other than ethylene glycol as a constituent component. However, the polyester has an aromatic dicarboxylic acid as the main component of the polycarboxylic acid component and an ethylene glycol as the main component of the diol component. The molar ratio of the aromatic dicarboxylic acid in the polycarboxylic acid component is preferably 80 mol % or more. The molar ratio of ethylene glycol in the diol component is preferably 80 mol % or more.
[0016] The polyester substrate preferably contains only the above polyester as a resin, but may contain other resins as long as the effect of the polyester substrate is not impaired. For example, it is preferable that the polyester accounts for 80 mass% or more of the total resin components. The polyester substrate may also contain various additives such as organic or inorganic lubricants, antioxidants, heat stabilizers, ultraviolet absorbers, and antistatic agents.
[0017] Examples of preferred polyester substrates include polyethylene terephthalate (PET) substrates, polyethylene naphthalate (PEN) substrates, and polyethylene furanoate (PEF) substrates. The PET substrate is a polyester substrate formed of polyethylene terephthalate obtained by polycondensing terephthalic acid and ethylene glycol. The PEN substrate is a polyester substrate formed of polyethylene naphthalate obtained by polycondensing naphthalenedicarboxylic acid (specifically, 2,6-naphthalenedicarboxylic acid) and ethylene glycol. The PEF substrate is a polyester substrate formed of polyethylene furanoate obtained by polycondensing furandicarboxylic acid (specifically, 2,5-furandicarboxylic acid) and ethylene glycol. PEF and PEN are known as alternative materials to PET, and in this embodiment, a PEN substrate or a PEF substrate can be suitably used instead of the PET substrate.
[0018] The shape of the polyester substrate or coating substrate is not particularly limited, and may be, for example, a film, a sheet, or a plate, or may be molded into a predetermined shape.
[0019] The polyurethane layer is a resin layer laminated on at least one of the front and back surfaces of the polyester substrate. The polyurethane forming the polyurethane layer is obtained by reacting a polyol with a polyisocyanate, and is a polymer having a urethane bond in the molecule.
[0020] The polyol is not particularly limited, and examples thereof include polymer polyols such as polyester polyols (e.g., aliphatic polyester polyols, aromatic polyester polyols), polycarbonate polyols, polyether polyols (e.g., polytetramethylene glycol), and polybutadiene polyols. As the polyol, low molecular weight polyhydric alcohols (preferably dihydric alcohols, trihydric alcohols) such as ethylene glycol, propylene glycol, propanediol, butanediol, pentanediol, 3-methyl-1,5-pentanediol, hexanediol, neopentyl glycol, diethylene glycol, triethylene glycol, dipropylene glycol, tripropylene glycol, bisphenol A, bisphenol F, bisphenol S, hydrogenated bisphenol A, trimethylolpropane, glycerin, and pentaerythritol may be used together with or separately from the above polymer polyols. These polyols may be used alone or in combination of two or more.
[0021] The polyisocyanate is not particularly limited, and examples thereof include aliphatic polyisocyanates, alicyclic polyisocyanates, and aromatic polyisocyanates. Examples of aliphatic polyisocyanates include tetramethylene diisocyanate, dodecamethylene diisocyanate, hexamethylene diisocyanate (HDI), 2,2,4-trimethylhexamethylene diisocyanate, and lysine diisocyanate. Examples of alicyclic polyisocyanates include isophorone diisocyanate (IPDI), dicyclohexylmethane 4,4'-diisocyanate (hydrogenated MDI), hydrogenated xylylene diisocyanate, 1,4-cyclohexane diisocyanate, methylcyclohexylene diisocyanate, and 1,3-bis(isocyanatemethyl)cyclohexane. Examples of aromatic polyisocyanates include tolylene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), polymeric MDI, xylylene diisocyanate (XDI), and naphthalene diisocyanate. Also, isocyanurate, adduct, biuret, allophenate, and carbodiimide of these polyisocyanates may be used. Also, these polyisocyanates may be used alone or in combination of two or more.
[0022] The polyurethane layer may be a layer formed by a water-based polyurethane resin or a layer formed by a solvent-based polyurethane resin. In one embodiment, in the case of a water-based polyurethane resin, the polyurethane layer may be a layer formed by an anionic polyurethane having an anionic hydrophilic group, a layer formed by a cationic polyurethane having a cationic hydrophilic group, or a layer formed by an uncharged nonionic polyurethane having a hydrophilic segment.
[0023] In one embodiment, the acid value of the polyurethane forming the polyurethane layer is preferably 0 to 40 mgKOH / g, more preferably 10 to 35 mgKOH / g. By having an acid value of 40 mgKOH / g or less, the release agent according to this embodiment can enhance the releasability effect. Examples of polyurethanes having such an acid value include anionic polyurethane resins having an anionic hydrophilic group such as a carboxy group, which can be obtained, for example, by adding a compound having an anionic hydrophilic group and an active hydrogen group to the monomer component.
[0024] In this specification, the acid value (mgKOH / g) of polyurethane refers to a value measured based on JIS K0070:1992 (neutralization titration method).
[0025] In one embodiment, the polyurethane forming the polyurethane layer is preferably polyurethane containing polyester polyol as a raw material. That is, the polyurethane layer is preferably formed from polyurethane obtained by reacting a polyol containing polyester polyol with a polyisocyanate. A polyurethane using such a polyester polyol is less likely to be dissolved by the release agent according to the present embodiment, that is, the insolubility of the polyurethane layer can be improved. In this case, the amount of polyester polyol in the polyol constituting the polyurethane is not particularly limited, and may be, for example, 70% by mass or more, or 80 to 99% by mass relative to 100% by mass of the polyol.
[0026] In addition to the polyurethane, the polyurethane layer may contain various additives such as an antioxidant, an antistatic agent, a surfactant, an antifoaming agent, and a surface conditioner.
[0027] The thickness of the polyurethane layer is not particularly limited, and may be, for example, 0.05 to 500 μm, 0.5 to 100 μm, or 1 to 50 μm.
[0028] The release agent according to this embodiment contains at least one organic solvent selected from the group consisting of dialkylene glycol monoalkyl ether acetates, dialkylene glycol diacetates, and trialkylene glycol diacetates.
[0029] As the dialkylene glycol monoalkyl ether acetate, it is preferable to use a compound represented by the following general formula (1). [ka] In formula (1), R 1 represents an alkyl group having 1 to 6 carbon atoms, and R 2 R represents an alkanediyl group having 2 to 4 carbon atoms. An alkanediyl group is a divalent chain-type saturated hydrocarbon group, and is also called an alkylene group. 1 R is more preferably an alkyl group having 1 to 4 carbon atoms. 2 is more preferably an alkanediyl group having 2 or 3 carbon atoms.
[0030] Specific examples of dialkylene glycol monoalkyl ether acetates include diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol monopropyl ether acetate, diethylene glycol monobutyl ether acetate, diethylene glycol monohexyl ether acetate, and other diethylene glycol monoalkyl ether acetates, dipropylene glycol monomethyl ether acetate, dipropylene glycol monoethyl ether acetate, dipropylene glycol monopropyl ether acetate, dipropylene glycol monobutyl ether acetate, dipropylene glycol monohexyl ether acetate, and other dipropylene glycol monoalkyl ether acetates, dibutylene glycol monomethyl ether acetate, dibutylene glycol monoethyl ether acetate, and other dibutylene glycol monoalkyl ether acetates. These may be used alone or in combination of two or more.
[0031] As the dialkylene glycol diacetate and trialkylene glycol diacetate, it is preferable to use a compound represented by the following general formula (2). [ka] In formula (2), R 3 R represents an alkanediyl group having 2 to 4 carbon atoms, and n represents 2 or 3. 3 is more preferably an alkanediyl group having 2 or 3 carbon atoms. n is more preferably 2.
[0032] Specific examples of dialkylene glycol diacetates include diethylene glycol diacetate, dipropylene glycol diacetate, and dibutylene glycol diacetate. These may be used alone or in combination of two or more.
[0033] Specific examples of the trialkylene glycol diacetate include triethylene glycol diacetate, tripropylene glycol diacetate, and tributylene glycol diacetate. These may be used alone or in combination of two or more.
[0034] The stripping agent according to the present embodiment is a liquid agent containing the organic solvent, and is also called a stripping treatment liquid. The stripping agent may be composed of only the organic solvent, or may contain other solvents together with the organic solvent. As the other solvent, various organic solvents that do not dissolve the polyurethane layer can be used, and examples thereof include alkanes having 5 to 20 carbon atoms such as n-decane and n-tridecane, alcohols having 1 to 18 carbon atoms such as ethanol, n-propyl alcohol, isopropyl alcohol, and ethylene glycol, and esters having 4 to 8 carbon atoms such as ethyl acetate. As the other solvent, water may also be used.
[0035] From the viewpoint of enhancing the effect of this embodiment, it is preferable that the release agent contains at least one organic solvent selected from the group consisting of the dialkylene glycol monoalkyl ether acetate, dialkylene glycol diacetate, and trialkylene glycol diacetate in an amount of 40% by mass or more (i.e., 40 to 100% by mass). The amount of the organic solvent is more preferably 60 to 100% by mass, even more preferably 80 to 100% by mass, and even more preferably 86 to 100% by mass. The content of the other solvent is, for example, preferably 60% by mass or less, more preferably 40% by mass or less, even more preferably 20% by mass or less, and even more preferably 14% by mass or less. The release agent may be composed of only the solvent as described above, but may also contain additives such as surfactants.
[0036] In one embodiment, when dialkylene glycol monoalkyl ether acetate is used in combination with dialkylene glycol diacetate and / or trialkylene glycol diacetate, the ratio of the two is not particularly limited.For example, the mass ratio of dialkylene glycol monoalkyl ether acetate (A) to dialkylene glycol diacetate and / or trialkylene glycol diacetate (B) may be (A) / (B)=20 / 80 to 80 / 20, or 30 / 70 to 70 / 30.
[0037] The method for peeling the polyurethane layer from the coated substrate using the release agent is not particularly limited as long as it is a method for treating the release agent so that the polyurethane layer can be peeled off.
[0038] Preferably, the coating substrate having the polyurethane layer formed on the polyester substrate is immersed in the release agent, and the polyurethane layer is peeled off from the polyester substrate. In this case, the substrate may be left to stand for a predetermined time while immersed, or the release agent may be stirred while immersed. The surface of the coating substrate (the surface on which the polyurethane layer is formed) may be wiped in the release agent in which the substrate is immersed or after being removed from the release agent, thereby peeling off the polyurethane layer.
[0039] The release agent according to the present embodiment can be used to peel off a polyurethane layer from a coating substrate in which a polyurethane layer is provided on a polyester substrate in various fields including optical applications such as liquid crystal displays for televisions and computer monitors, and release films (release sheets). For example, when recycling a product incorporating a coating substrate, the release agent can be used to peel off a polyurethane layer from a coating substrate recovered from the product, and the polyester substrate can be recycled. Alternatively, the polyester substrate can be recycled by using scraps generated in the manufacturing process of a product using a coating substrate as a processing target. Alternatively, when a coating substrate in which a polyurethane layer is provided on a polyester substrate is used as a release film for forming a resin film, the release agent can be used to peel off a polyurethane layer from the release film, and the polyester substrate can be recycled. EXAMPLES
[0040] The present invention will be described in more detail below based on examples and comparative examples, but the present invention is not limited thereto.
[0041] The release agents having the compositions (parts by mass) shown in Table 1 below were evaluated for their releasability, resistance to attack of the resin substrate, and insolubility of the polyurethane layer when used to treat a coating film consisting of the resin substrate and polyurethane layer shown in Table 1.
[0042] The organic solvents used in the release agents are as follows: ·Diethylene glycol monobutyl ether acetate Dipropylene glycol monomethyl ether acetate ·Diethylene glycol diacetate ·Triethylene glycol diacetate Isopropyl alcohol Diethylene glycol dibutyl ether N,N-Dimethylformamide n-Decane ·ethanol
[0043] Regarding the types of resin substrates in Table 1, "PET" is a 99 μm thick polyethylene terephthalate (PET) film ("Lumirror T-60" manufactured by Toray Industries, Inc.). "PEN" is a 50 μm thick polyethylene naphthalate (PEN) film ("Teonex Q51" manufactured by Toyobo Co., Ltd.). "PC" is a 2 mm thick polycarbonate (PC) plate ("Standard test plate PC (polycarbonate)" manufactured by Nippon Test Panel Co., Ltd.). "ABS" is a 2 mm thick ABS plate ("Standard test plate ABS" manufactured by Nippon Test Panel Co., Ltd.).
[0044] Regarding the types of polyurethane layers in Table 1, "PU1" is an aqueous dispersion of polyurethane (acid value: 35 mg KOH / g) prepared according to Synthesis Example 1 below. "PU2" is an aqueous dispersion of polyurethane (acid value: 34 mg KOH / g) prepared according to Synthesis Example 2 below. "PU3" is an aqueous dispersion of polyurethane (acid value: 11 mg KOH / g) prepared according to Synthesis Example 3 below.
[0045] The raw materials used in Synthesis Examples 1 to 3 are as follows. [Polyol] Polyester polyol (a-1): A polyol with a number average molecular weight of 1000 and an acid value of 0.5 mg KOH / g. The synthesis method is as follows: In a reaction vessel equipped with a stirrer, a thermometer, a reflux condenser, a dropping tank, and a nitrogen gas inlet tube, 38.29 parts by mass of isophthalic acid, 19.94 parts by mass of adipic acid, 27.8 parts by mass of 1,6-hexanediol, and 13.97 parts by mass of ethylene glycol were charged, and the mixture was heated to 250° C. with stirring under a nitrogen stream. The reaction was continued until the acid value became 5 mgKOH / g or less, to obtain polyester polyol (a-1).
[0046] Polyester polyol (a-2): A polyol with a number average molecular weight of 2000 and an acid value of 0.5 mg KOH / g. The synthesis method is as follows: In a reaction vessel equipped with a stirrer, a thermometer, a reflux condenser, a dropping tank, and a nitrogen gas inlet tube, 52.41 parts by mass of isophthalic acid, 8.77 parts by mass of adipic acid, 26.58 parts by mass of 1,6-hexanediol, and 12.24 parts by mass of ethylene glycol were charged, and the mixture was heated to 250° C. with stirring under a nitrogen stream. The reaction was continued until the acid value became 5 mgKOH / g or less, to obtain polyester polyol (a-2).
[0047] Polyol (a-3): "Newpol BPE-20NK" (registered trademark) manufactured by Sanyo Chemical Industries, Ltd. Dimethylolpropionic acid: 2,2-dimethylolpropionic acid, Perstorp's "Bis-MPA" (registered trademark) (functional groups: 2, molecular weight: 134.13) Trimethylolpropane
[0048] [Polyisocyanate] ·MDI: 4,4'-diphenylmethane diisocyanate ·TDI: Tolylene diisocyanate
[0049] [Blocking agents and neutralizing agents] Dibutylamine (blocking agent) ·Triethylamine (neutralizer) Ammonia (neutralizer)
[0050] [Synthesis Example 1: Synthesis of PU1] As polyol, 64.89 parts by mass of polyester polyol (a-1), 0.5 parts by mass of trimethylolpropane, and 8.40 parts by mass of dimethylolpropionic acid, 26.21 parts by mass of TDI as polyisocyanate, and 100 parts by mass of methyl ethyl ketone were mixed and reacted at 70 to 75 ° C for 120 minutes to obtain a urethane prepolymer solution. This urethane prepolymer solution was cooled to 35 ° C, and neutralized by adding 0.46 parts by mass of dibutylamine as a blocking agent and 6.02 parts by mass of triethylamine as a neutralizing agent, and then emulsified and dispersed using a homogenizer while gradually adding 320 parts by mass of water. Thereafter, methyl ethyl ketone was distilled off to obtain a polyurethane water dispersion (PU1) with a solid content of 25% by mass.
[0051] [Synthesis Example 2: Synthesis of PU2] As the polyol, 49.74 parts by mass of polyol (a-3), 0.6 parts by mass of trimethylolpropane, and 8.21 parts by mass of dimethylolpropionic acid, 41.45 parts by mass of TDI as polyisocyanate, and 100 parts by mass of methyl ethyl ketone were mixed and reacted at 70 to 75 ° C for 120 minutes to obtain a urethane prepolymer solution. This urethane prepolymer solution was cooled to 35 ° C, and neutralized by adding 2.42 parts by mass of dibutylamine as a blocking agent and 0.99 parts by mass of ammonia as a neutralizing agent, and then emulsified and dispersed using a homogenizer while gradually adding 320 parts by mass of water. Thereafter, the methyl ethyl ketone was distilled off to obtain a polyurethane water dispersion (PU2) with a solid content of 25% by mass.
[0052] [Synthesis Example 3: Synthesis of PU3] As a polyol, 81.45 parts by mass of polyester polyol (a-2), 2.63 parts by mass of dimethylol propionic acid, 15.92 parts by mass of MDI as a polyisocyanate, and 100 parts by mass of methyl ethyl ketone were mixed and reacted at 70 to 75 ° C for 120 minutes to obtain a urethane prepolymer solution. This urethane prepolymer solution was cooled to 35 ° C, and neutralized by adding 0.11 parts by mass of dibutylamine as a blocking agent and 1.88 parts by mass of triethylamine as a neutralizing agent, and then emulsified and dispersed using a homogenizer while gradually adding 180 parts by mass of water. Thereafter, the methyl ethyl ketone was distilled off to obtain a polyurethane water dispersion (PU3) with a solid content of 40% by mass.
[0053] The evaluation method of the release agent is as follows. [Removability (evaluation of ease of peeling)] (Preparation of coating film) The resin substrate was degreased with isopropyl alcohol, and then an aqueous dispersion of polyurethane was applied to the substrate using a bar coater to a dry thickness of 10 μm. The substrate was then dried at 80°C for 10 minutes and further dried at 120°C for 10 minutes to obtain a coating film on which a polyurethane film (polyurethane layer) was formed. (Evaluation method) 40 mL of each release agent was placed in a 50 mL glass vial. A coating film measuring 2 cm x 5 cm was immersed in 40 mL of each of the release agents and left to stand at room temperature for 10 minutes. After 10 minutes, the coating film was removed from the release agent and the surface was wiped once or three times with a paper rag. The state of peeling of the polyurethane coating after wiping was observed and evaluated according to the following criteria. (Evaluation Criteria) A: The polyurethane coating was completely removed with one wipe. B: After one wipe, some film remained, but after three wipes, the polyurethane film was completely removed. C: The polyurethane film could not be completely removed even after wiping three times.
[0054] [Resistance of resin substrate to corrosion] In the evaluation of the releasability, the surface condition of the resin substrate after wiping with the paper cloth was observed and evaluated according to the following criteria. ◯: The surface of the resin substrate is not damaged. ×: The surface of the resin substrate was roughened and corroded.
[0055] [Insolubility of polyurethane layer] A polyurethane aqueous dispersion was applied onto release paper to a dry thickness of approximately 200-300 μm, and then dried at 40°C for 24 hours, then at 80°C for 6 hours, and then at 120°C for 30 minutes to produce a polyurethane film. A polyurethane film measuring 2 cm x 2 cm was immersed in 50 mL of each release agent for 24 hours, removed from the release agent, dried, and the mass of the polyurethane film was measured. The ratio of the mass (W2) remaining after immersion in the release agent to the initial mass (W1) was calculated (mass retention = (W2 / W1) x 100%). A mass retention of 80% or more was considered to be acceptable, and a mass retention of less than 80% was considered to be unacceptable.
[0056] [Table 1]
[0057] The results are shown in Table 1. In Comparative Example 1, diethylene glycol monobutyl ether acetate was used as the release agent, but the resin substrate was a polycarbonate film, and therefore the polyurethane layer had poor releasability. In Comparative Example 2, the resin substrate was an ABS resin film, and therefore although the polyurethane layer could be peeled off, the resin substrate was corroded by the release agent.
[0058] Comparative Examples 3 to 5 are examples in which a coating substrate having a polyurethane layer laminated on a PET film was treated. Comparative Example 3, in which isopropyl alcohol was used as the release agent, and Comparative Example 4, in which diethylene glycol dibutyl ether was used, showed poor releasability of the polyurethane layer. On the other hand, Comparative Example 5, in which N,N-dimethylformamide was used as the release agent, showed excellent releasability and was less likely to damage the resin substrate, but the polyurethane layer was dissolved. If the polyurethane layer was dissolved to a large extent in this way, the release agent was poor in terms of repeated use.
[0059] Example 1 is an example in which diethylene glycol monobutyl ether acetate was used as the release agent. Example 2 is an example in which dipropylene glycol monomethyl ether acetate was used as the release agent. Example 3 is an example in which diethylene glycol diacetate was used as the release agent. Example 4 is an example in which triethylene glycol diacetate was used as the release agent. Examples 10 and 11 are examples in which the type of polyurethane layer was changed from Example 1. Example 12 is an example in which PEN was used as the polyester base material, whereas Example 1 used PET as the polyester base material. These Examples 1 to 4 and 10 to 12 had excellent release properties for the polyurethane layer, did not easily attack the polyester base material, and did not easily dissolve the polyurethane layer, and were excellent in repeated use of the release agent.
[0060] Examples 5 and 6 are examples in which dialkylene glycol monoalkyl ether acetate and dialkylene glycol diacetate are used in combination as a release agent, and while they are unlikely to attack the polyester substrate and hardly dissolve the polyurethane layer, as in Examples 1 to 4, they were able to peel off the polyurethane layer. Examples 7 to 9 are examples in which dialkylene glycol monoalkyl ether acetate and other organic solvents are used in combination as a release agent. Even when other organic solvents are used in combination in this way, the effects of releasability, resistance to attack of the resin substrate, and non-solubility of the polyurethane layer were obtained.
[0061] In addition, the various numerical ranges described in the specification can be arbitrarily combined with their upper and lower limits, and all such combinations are considered to be preferred numerical ranges described in the specification. In addition, a numerical range described as "X to Y" means from X to Y.
[0062] Although several embodiments of the present invention have been described above, these embodiments are presented as examples and are not intended to limit the scope of the invention. These embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the gist of the invention. These embodiments and their omissions, substitutions, modifications, etc. are included in the scope and gist of the invention as well as the invention and its equivalents described in the claims.
Claims
1. A release agent for releasing a polyurethane layer from a coating substrate, the coating substrate being a polyester substrate formed of a polyester containing an aromatic dicarboxylic acid and ethylene glycol as constituent components and coated with a polyurethane layer, comprising: A release agent comprising 40 mass % or more of at least one member selected from the group consisting of dialkylene glycol monoalkyl ether acetate, dialkylene glycol diacetate, and trialkylene glycol diacetate.
2. 2. The release agent according to claim 1, wherein the polyurethane forming the polyurethane layer has an acid value of 0 to 40 mgKOH / g.
3. 2. The release agent according to claim 1, wherein the polyurethane forming the polyurethane layer is a polyurethane containing polyester polyol as a raw material.
4. 2. The release agent of claim 1, wherein the polyester substrate is a polyethylene terephthalate substrate, a polyethylene naphthalate substrate, or a polyethylene furanoate substrate.
5. The at least one selected from the group consisting of dialkylene glycol monoalkyl ether acetate, dialkylene glycol diacetate, and trialkylene glycol diacetate is at least one selected from the group consisting of a compound represented by the following general formula (1) and a compound represented by the following general formula (2): [Formula 1] In formula (1), R 1 represents an alkyl group having 1 to 6 carbon atoms; R 2 represents an alkanediyl group having 2 to 4 carbon atoms, and in formula (2), R 3 The stripping agent according to claim 1, wherein represents an alkanediyl group having 2 to 4 carbon atoms, and n represents 2 or 3.
6. A stripping method using the stripping agent according to any one of claims 1 to 5, A peeling method comprising the steps of: immersing a coated substrate, which is a polyester substrate formed from a polyester containing an aromatic dicarboxylic acid and ethylene glycol as constituent components and is coated with a polyurethane layer, in the release agent, and peeling off the polyurethane layer from the polyester substrate.
Citation Information
Patent Citations
Agent for softening coating and agent for peeling coating
JP2000063716A
Gas barrier film
JP2017222151A
Aqueous resin composition, coating agent and article
JP2018104535A
Compositions and methods for cleaning urethane molds
US20210040421A1
Methods of recycling and compositions used therein
US5840772A