Pretreatment liquid for inkjet ink, ink set, image recording method, laminate manufacturing method, image recorded matter, and laminate
The use of a urethane resin-based pretreatment liquid with specific molecular characteristics in inkjet ink systems addresses the challenges of boiling resistance and storage stability for laminates on non-permeable substrates, enhancing adhesion and durability.
Patent Information
- Application Number
- PCT/JP2024/010123
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-03-14
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional inkjet ink pretreatment liquids fail to provide adequate boiling resistance and storage stability for laminates, particularly when used on non-permeable substrates, leading to issues with image quality and substrate adhesion.
A pretreatment liquid containing a urethane resin with specific polyol and polyisocyanate units, a flocculant, and a counter cation, applied in combination with an inkjet ink to improve substrate adhesion and resistance, featuring a urethane resin with a weight average molecular weight of 5000 or more and a glass transition temperature between -60°C and 40°C.
The solution enhances the boiling resistance and storage stability of laminates by ensuring better adhesion and flexibility of the inkjet ink layers on non-permeable substrates, preventing hydrophilicity and maintaining hydrophobicity, thus improving the durability and longevity of the laminate.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Pretreatment liquid for inkjet ink, ink set, image recording method, method for manufacturing laminated body, image recorded material, and laminated body
[0001] The present disclosure relates to a pretreatment liquid for inkjet ink, an ink set, an image recording method, a method for manufacturing a laminated body, an image-recorded product, and a laminated body.
[0002] Various studies have been conducted on image recording methods using pretreatment liquids and inks. For example, Patent Document 1 discloses the following inkjet recording liquid set as an inkjet recording liquid set that exhibits excellent image quality, substrate adhesion, and ejection stability on low-absorbency or non-absorbency substrates, and also exhibits excellent hot water resistance on the image surface when formed into a coating film. The inkjet recording liquid set disclosed in Patent Document 1 is an inkjet recording liquid set that includes at least an inkjet ink and a pretreatment liquid, wherein the inkjet ink contains at least a pigment, an organic solvent, water, and a silicone-based surfactant, the pretreatment liquid contains at least water-insoluble resin fine particles and a pigment aggregating agent, and the silicone-based surfactant has a specific structure containing an ethylene oxide group or the like.
[0003] Patent Document 1: JP 2021-042264 A
[0004]
[0003] A laminate may be produced by applying an inkjet ink pretreatment liquid and an inkjet ink, in this order, to an impermeable substrate to record an image, and then laminating a substrate for lamination onto the image in the image recorded. This laminate may be required to have boil resistance (i.e., resistance to boiling treatment). Furthermore, the inkjet ink pretreatment liquid may be required to have storage stability.
[0005]
[0013] An object of one embodiment of the present disclosure is to provide a pretreatment liquid for inkjet inks that can improve the boil resistance of a laminated body when a laminated body is produced by applying an inkjet ink pretreatment liquid and an inkjet ink, in this order, to a non-permeable substrate to record an image, and laminating a laminating substrate onto the image in the obtained image recorded body, and that has excellent storage stability. Another object of another embodiment of the present disclosure is to provide an ink set that includes the pretreatment liquid for inkjet inks, and an ink set, an image recording method, a method for producing a laminated body, an image recorded body, and a laminated body that use the pretreatment liquid for inkjet inks.
[0006] The present disclosure includes the following aspects: <1> A method for producing a polymerizable composition comprising: a flocculant that is at least one selected from the group consisting of an organic acid and a polyvalent metal compound; water; and a urethane resin, wherein the urethane resin comprises a polyol unit, a polyisocyanate unit, and an —SO 3 - group relative to the total amount of the urethane resin, 3 - The content of —SO groups is 2% by mass to 6% by mass, 3 - <2> The pretreatment liquid for ink-jet ink according to <1>, wherein the urethane resin contains a partial structure represented by the following formula (I):
[0007]
[0008] In formula (I), * represents a bonding position; 1 is -NH- or -N(L 4 -Y 4 )-, L 4 represents a divalent group which is one kind selected from Group 1 consisting of an alkylene group, an alkenylene group, an alkynylene group, an arylene group, —O—, —NH—, and —C(═O)—, a divalent group formed by combining two or more kinds selected from Group 1, or a single bond; Y 4represents an alkyl group, an alkenyl group, an alkynyl group, an aryl group, a halogen atom, —OH, —OR 3 , -NH 2 , -NR 3 H, -NR 3 R 4 , or -C(=O)R 3 represents R 3 and R 4 each independently represents an alkyl group, an alkenyl group, an alkynyl group, or an aryl group; L 1 represents an alkylene group having 1 to 4 carbon atoms; Z + is -SO 3 - represents a counter cation for the group.
[0009] <3> The pretreatment liquid for inkjet ink according to <1> or <2>, wherein the weight average molecular weight of the urethane resin is 5,000 or more. <4> The pretreatment liquid for inkjet ink according to any one of <1> to <3>, wherein the glass transition temperature of the urethane resin is -60°C to 40°C. <5> The pretreatment liquid for inkjet ink according to any one of <1> to <4>, wherein the molar ratio of polyol units to polyisocyanate units in the urethane resin is 0.5 to 0.9. <6> The pretreatment liquid for inkjet ink according to any one of <1> to <4>, wherein the urethane resin is -SO 3 - <7> The pretreatment liquid for inkjet ink according to any one of <1> to <5>, wherein the urethane resin contains a counter cation for the —SO 2 group, and the pKa of the counter cation is 10.0 or more. 3 -<1> The inkjet ink pretreatment liquid according to any one of <1> to <6>, which contains a counter cation for the group, the counter cation being an organic base cation. <8> The inkjet ink pretreatment liquid according to any one of <1> to <7>, in which the polyol unit contains a polycarbonate diol unit. <9> An ink set comprising the inkjet ink pretreatment liquid according to any one of <1> to <8>, and an ink that is an inkjet ink containing water, a pigment, and a urethane resin. <10> An image recording method using the ink set according to <9>, which comprises: applying the inkjet ink pretreatment liquid onto a non-permeable substrate; and applying ink by inkjet recording onto the non-permeable substrate to which the inkjet ink pretreatment liquid has been applied. <11> A method for producing a laminated body, comprising: obtaining an image recorded article comprising an impermeable substrate and an image disposed on the impermeable substrate by the image recording method according to <10>; and laminating a substrate for lamination onto the side of the image recorded article on which the image is disposed to obtain a laminated body. <12> A laminated body comprising an impermeable substrate and an image disposed on the impermeable substrate, wherein the image comprises: a pretreatment layer disposed on the impermeable substrate, the pretreatment layer containing a flocculant that is at least one selected from the group consisting of organic acids and polyvalent metal compounds, and a urethane resin; and an ink layer disposed on the pretreatment layer, the urethane resin in the pretreatment layer containing a polyol unit, a polyisocyanate unit, and -SO 3 - group relative to the total amount of the urethane resin, 3 - The content of —SO groups is 2% by mass to 6% by mass, 3 - <13> A laminate comprising the image recorded material according to <12>, and a lamination substrate laminated onto an image of the image recorded material.
[0010] According to one embodiment of the present disclosure, there is provided a pretreatment liquid for inkjet inks that can improve the boil resistance of a laminated body when a laminated body is produced by applying a pretreatment liquid for inkjet inks and an inkjet ink, in this order, to a non-permeable substrate to record an image, and laminating a laminating substrate onto the image in the obtained image recorded body, and that has excellent storage stability. According to another embodiment of the present disclosure, there is provided an ink set including the pretreatment liquid for inkjet inks, as well as an ink set, an image recording method, a method for producing a laminated body, an image recorded body, and a laminated body that use the pretreatment liquid for inkjet inks.
[0011] The inkjet ink set for non-permeable substrates, the image recording method, the method for producing a laminate, the image-recorded product, and the laminate according to the present disclosure will be described in detail below.
[0012] In this specification, a numerical range indicated using "to" means a range that includes the numerical values before and after "to" as the minimum and maximum values, respectively. In the numerical ranges described in stages in this specification, the upper or lower limit value described in a certain numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. Furthermore, in the numerical ranges described in this specification, the upper or lower limit value described in a certain numerical range may be replaced with a value shown in the examples.
[0013] As used herein, the amount of each component in a composition refers to the total amount of the components in the composition unless otherwise specified, when the composition contains multiple substances corresponding to each component. In this specification, a combination of two or more preferred aspects is a more preferred aspect. As used herein, the term "process" includes not only independent processes, but also processes that cannot be clearly distinguished from other processes, as long as the intended purpose of the process is achieved.
[0014] In this specification, the term "image" refers to a film formed by applying a pretreatment liquid and an ink in this order, and the term "image recording" refers to the formation of an image (i.e., a film). The term "image" in this specification also includes a solid image.
[0015] In this specification, the term "(meth)acrylate" encompasses both acrylate and methacrylate, and the term "(meth)acrylic" encompasses both acrylic and methacrylic.
[0016] In this specification, "boiling treatment" refers to a treatment in which an object (specifically, a laminate) is immersed in water at 60 to 100°C and heated for a certain period of time (for example, 10 to 120 minutes).
[0017] [Pretreatment liquid for inkjet ink] The pretreatment liquid for inkjet ink of the present disclosure (hereinafter also simply referred to as "pretreatment liquid") contains: a flocculating agent which is at least one selected from the group consisting of organic acids and polyvalent metal compounds; water; and a urethane resin, wherein the urethane resin contains a polyol unit, a polyisocyanate unit, and a -SO 3 - group relative to the total amount of the urethane resin, 3 - The content of —SO groups is 2% by mass to 6% by mass, 3 - The pretreatment liquid has a group bonded to the end of the main chain of the urethane resin.
[0018] The pretreatment liquid according to the present disclosure can improve the boil resistance of a laminated body when a laminated body is produced by applying the pretreatment liquid and an inkjet ink (hereinafter also simply referred to as "ink") in this order to an impermeable substrate to record an image, and then laminating a laminating substrate onto the image in the obtained image recorded body. Furthermore, the pretreatment liquid according to the present disclosure has excellent storage stability.
[0019] The reason why the above-mentioned effect of improving the boil resistance of the laminated body is obtained is thought to be that the pretreatment liquid contains a urethane resin, which improves the flexibility of the layer derived from the pretreatment liquid and the adhesion to the non-permeable substrate. 3 - This is also thought to be due to the fact that the amount of —SO 3 groups is 6% by mass or less relative to the total amount of the urethane resin. 3 - By ensuring that the amount of groups is 6 mass% or less relative to the total amount of urethane resin, the hydrophilicity of the urethane resin is prevented from becoming too high (i.e., the hydrophobicity is maintained), and the urethane resin is prevented from swelling with water, which is thought to result in the prevention of a decrease in the boil resistance of the laminate.
[0020] On the other hand, the reason why the pretreatment liquid has excellent storage stability is that the urethane resin in the pretreatment liquid has a -SO 3 - group is bonded, and this -SO 3 - This is thought to be because the amount of -SO groups is 2% by mass or more relative to the total amount of the urethane resin. 3 - The —SO group is bonded to the end of the main chain of the urethane resin. 3 - This is thought to ensure freedom of movement of the groups, resulting in improved dispersion stability of the urethane resin in the pretreatment liquid, and ultimately improved storage stability of the pretreatment liquid.
[0021] Although a flocculant in a pretreatment liquid generally acts to reduce the dispersibility of a resin in the pretreatment liquid, the pretreatment liquid of the present disclosure is believed to have excellent storage stability despite being a pretreatment liquid containing a flocculant and a resin due to the above-mentioned reasons (actions).
[0022] Each component that can be contained in the pretreatment liquid will be described below.
[0023] <Water> The pretreatment liquid according to the present disclosure contains water. The water content is preferably 50% by mass or more, and more preferably 60% by mass or more, based on the total amount of the pretreatment liquid. The upper limit of the water content, although it depends on the amounts of other components, is preferably 90% by mass or less, and more preferably 80% by mass or less, based on the total amount of the pretreatment liquid.
[0024] The pretreatment liquid according to the present disclosure contains at least one flocculant selected from the group consisting of organic acids and polyvalent metal compounds. The flocculant in the pretreatment liquid flocculates components in the inkjet ink, contributing to improving image quality when an image is recorded by applying the pretreatment liquid and the inkjet ink in this order to a non-permeable substrate.
[0025] Preferred examples of the flocculant include the flocculants described in paragraphs 0122 to 0130 of WO 2020 / 195360.
[0026] Organic Acids Examples of organic acids include organic compounds having an acidic group.
[0027] Acidic groups include phosphate groups, phosphonate groups, phosphinate groups, sulfate groups, sulfonate groups, sulfinate groups, and carboxy groups.
[0028] Among these, from the viewpoint of the aggregation speed of the ink, the acidic group is preferably a phosphate group or a carboxy group, and more preferably a carboxy group.
[0029] It is preferable that at least a portion of the acidic groups is dissociated in the pretreatment liquid.
[0030] Examples of organic compounds having a carboxy group include (meth)acrylic acid, poly(meth)acrylic acid, acetic acid, formic acid, benzoic acid, glycolic acid, malonic acid, malic acid (preferably DL-malic acid), maleic acid, succinic acid, glutaric acid, pimelic acid, adipic acid, fumaric acid, citric acid, tartaric acid, phthalic acid, 4-methylphthalic acid, lactic acid, pyrrolidonecarboxylic acid, pyronecarboxylic acid, pyrrolecarboxylic acid, furancarboxylic acid, pyridinecarboxylic acid, coumaric acid, thiophenecarboxylic acid, and nicotinic acid.
[0031] Among these, from the viewpoint of the aggregation speed of the ink, the organic compound having a carboxy group is preferably a divalent or higher carboxylic acid (hereinafter also referred to as a polycarboxylic acid), and more preferably a dicarboxylic acid.
[0032] Specifically, the polycarboxylic acid is preferably malonic acid, malic acid, maleic acid, succinic acid, glutaric acid, pimelic acid, adipic acid, fumaric acid, tartaric acid, 4-methylphthalic acid, or citric acid, and more preferably malonic acid, malic acid, tartaric acid, succinic acid, glutaric acid, pimelic acid, adipic acid, or citric acid.
[0033] The organic acid preferably has a low pKa (for example, 1.0 to 5.0), which reduces the surface charge of particles such as pigments and resin particles in the ink, which are stabilized by weakly acidic functional groups such as carboxyl groups, by contacting them with an organic acid having an even lower pKa, thereby lowering dispersion stability.
[0034] The organic acid preferably has a low pKa, high solubility in water, and a valence of at least 2. Furthermore, the organic acid more preferably has a high buffering capacity in a pH range lower than the pKa of the functional group (e.g., carboxy group) that stabilizes the dispersion of the particles in the ink.
[0035] -Polyvalent Metal Compound- Examples of polyvalent metal compounds include polyvalent metal salts. Examples of polyvalent metal salts include organic acid polyvalent metal salts and inorganic acid polyvalent metal salts. Preferred organic acid polyvalent metal salts are polyvalent metal salts of the above-mentioned organic acids (e.g., formic acid, acetic acid, benzoic acid, etc.). Preferred inorganic acid polyvalent metal salts are polyvalent metal nitrates, polyvalent metal hydrochlorides, or polyvalent metal thiocyanates.
[0036] Examples of polyvalent metal salts include salts of alkaline earth metals (e.g., magnesium, calcium) of Group 2 of the periodic table, salts of transition metals (e.g., lanthanum) of Group 3 of the periodic table, salts of metals (e.g., aluminum) of Group 13 of the periodic table, and salts of lanthanides (e.g., neodymium). As the polyvalent metal salt, calcium salts, magnesium salts, or aluminum salts are preferred, and calcium salts or magnesium salts are more preferred.
[0037] The polyvalent metal compound is preferably an organic acid polyvalent metal salt, more preferably an organic acid calcium salt or an organic acid magnesium salt.
[0038] It is preferable that the polyvalent metal compound is at least partially dissociated into polyvalent metal ions and counter ions in the pretreatment liquid.
[0039] The content of the flocculant in the pretreatment liquid is preferably 0.1% by mass to 40% by mass, more preferably 0.1% by mass to 30% by mass, even more preferably 1% by mass to 20% by mass, and still more preferably 1% by mass to 10% by mass, relative to the total amount of the pretreatment liquid.
[0040] From the viewpoint of further improving the boil resistance of the laminate and the storage stability of the pretreatment liquid, it is more preferable that the flocculant contains an organic acid. In this case, the content of the organic acid in the total amount of the flocculant is preferably 50% by mass to 100% by mass, more preferably 60% by mass to 100% by mass, and even more preferably 80% by mass to 100% by mass.
[0041] <Urethane Resin> The pretreatment liquid of the present disclosure contains a polyol unit, a polyisocyanate unit, and a —SO 3 - The urethane resin contains a urethane resin containing a —SO group. 3 - The content of the —SO group is 2% by mass to 6% by mass. 3 - The group is bonded to the end of the main chain of the urethane resin.
[0042] In the present disclosure, the term "polyol unit" refers to a structural unit derived from a polyol, and the term "polyisocyanate unit" refers to a structural unit derived from a polyisocyanate. The urethane resin may contain only one type of polyol unit and one or more types of polyisocyanate unit.
[0043] Polyol units, polyisocyanate units, and -SO 3 - In other words, the urethane resin containing at least a polyol, a polyisocyanate, and a —SO3 - The urethane resin is a reaction product of a group-introducing compound (hereinafter also referred to as a "dispersing group-introducing compound") and a polyol and a polyisocyanate for forming the urethane resin. For details of the polyol and polyisocyanate for forming the urethane resin, reference can be made to, for example, the descriptions in paragraphs
[0031] to
[0036] of JP 2001-247787 A, the descriptions in paragraphs
[0033] to
[0118] of WO 2016 / 052053 A, and the descriptions in paragraphs
[0066] to
[0223] of WO 2016 / 152254 A.
[0044] (Polyisocyanate Unit and Polyisocyanate) The urethane resin contains at least one type of polyisocyanate unit. Preferred embodiments of the polyisocyanate unit and preferred embodiments of the polyisocyanate for forming the polyisocyanate unit will be described below. The polyisocyanate may be a polyisocyanate containing two isocyanate groups (i.e., a diisocyanate (i.e., a bifunctional isocyanate)), or a polyisocyanate containing three or more isocyanate groups (i.e., a trifunctional or higher isocyanate). The polyisocyanate is preferably a bifunctional to hexafunctional isocyanate.
[0045] The polyisocyanate unit preferably contains the following structural unit (P1).
[0046]
[0047] In the structural unit (P1), L 1 represents a divalent organic group having 1 to 20 carbon atoms, and * represents the bonding position.
[0048] L 1 Specific examples of the above include residues obtained by removing two isocyanate groups (NCO groups) from the bifunctional isocyanates according to the following specific examples.
[0049] Specific examples of the bifunctional isocyanate are as follows: However, the bifunctional isocyanate is not limited to the following specific examples.
[0050]
[0051] In addition, the bifunctional isocyanate may be a bifunctional isocyanate derived from the above specific examples, such as Duranate (registered trademark) D101, D201, and A101 (manufactured by Asahi Kasei Corporation).
[0052] The tri- or higher functional isocyanate is preferably a reaction product of at least one selected from the group consisting of bifunctional isocyanates and at least one selected from the group consisting of compounds containing three or more active hydrogen groups (e.g., tri- or higher functional polyol compounds, tri- or higher functional polyamine compounds, and tri- or higher functional polythiol compounds). The number of moles (number of molecules) of the bifunctional isocyanate to be reacted with the compound containing three or more active hydrogen groups is preferably 0.6 times or more, more preferably 0.6 to 5 times, even more preferably 0.6 to 3 times, and even more preferably 0.8 to 2 times the number of moles of active hydrogen groups (number of equivalents of active hydrogen groups) in the compound containing three or more active hydrogen groups.
[0053] Examples of the difunctional isocyanate for forming a trifunctional or higher isocyanate include the difunctional isocyanates according to the specific examples described above.
[0054] Examples of compounds containing three or more active hydrogen groups for forming trifunctional or higher isocyanates include the compounds described in paragraphs 0057 to 0058 of WO 2016 / 052053.
[0055] Examples of tri- or higher functional isocyanates include adduct-type tri- or higher functional isocyanates, isocyanurate-type tri- or higher functional isocyanates, biuret-type tri- or higher functional isocyanates, etc. Commercially available adduct-type tri- or higher functional isocyanates include Takenate (registered trademark) D-102, D-103, D-103H, D-103M2, P49-75S, D-110N, D-120N, D-140N, D-160N (all Mitsui Chemicals, Inc.), Desmodur (registered trademark) L75, UL57SP (Sumika Bayer Urethane Co., Ltd.), Coronate (registered trademark) HL, HX, L (Nippon Urethane Polymer Co., Ltd.), P301-75E (Asahi Kasei Corporation), etc. Commercially available isocyanurate-type trifunctional or higher isocyanates include Takenate (registered trademark) D-127N, D-170N, D-170HN, D-172N, D-177N (all Mitsui Chemicals, Inc.), Sumidur N3300, Desmodur (registered trademark) N3600, N3900, Z4470BA (all Sumika Bayer Urethane Co., Ltd.), Coronate (registered trademark) HX, HK (all Nippon Urethane Polymer Co., Ltd.), Duranate (registered trademark) TPA-100, TKA-100, TSA-100, TSS-100, TLA-100, TSE-100 (all Asahi Kasei Corporation), and the like. Commercially available biuret-type tri- or higher functional isocyanates include Takenate (registered trademark) D-165N and NP1100 (both manufactured by Mitsui Chemicals, Inc.), Desmodur (registered trademark) N3200 (manufactured by Sumika Bayer Urethane Co., Ltd.), and Duranate (registered trademark) 24A-100 (manufactured by Asahi Kasei Corporation).
[0056] At least one of the polyisocyanates may be a polyisocyanate containing a hydrophilic group. For details of polyisocyanates containing a hydrophilic group, see paragraphs
[0112] to
[0118] and
[0252] to
[0254] of WO 2016 / 052053. At least one of the polyisocyanates may be a polyisocyanate containing a polymerizable group. For details of isocyanates containing a polymerizable group, see paragraphs
[0084] to
[0089] ,
[0203] , and
[0205] of WO 2016 / 052053.
[0057] -Polyol Unit and Polyol- The urethane resin contains at least one polyol unit. Preferred embodiments of the polyol unit and preferred embodiments of the polyol for forming the polyol unit will be described below. The polyol may be a polyol containing two hydroxy groups (i.e., a diol), or a polyol containing three or more hydroxy groups.
[0058] The polyol unit preferably contains the following structural unit (P0).
[0059]
[0060] In the structural unit (P0), L 0 represents a divalent organic group, and * represents a bonding position.
[0061] In the structural unit (P0), L 0 The divalent organic group represented by the formula (I) may be a group consisting of carbon atoms and hydrogen atoms, or may be a group containing carbon atoms and hydrogen atoms and also containing a heteroatom (for example, an oxygen atom, a nitrogen atom, a sulfur atom, etc.). 0 The divalent organic group represented by the formula (I) may contain at least one of a hydrophilic group and a polymerizable group. 0 Specific examples of the group include residues obtained by removing hydrogen atoms from each of the two hydroxy groups in the diols exemplified below.
[0062] Specific examples of diols, which are preferred embodiments of polyols, are shown below, but the polyols are not limited to the following specific examples.
[0063]
[0064] In compounds (12) to (15), nC 7 H 15 , nC 9 H 19 , nC 11 H 23 , and nC 17 H 35represent a normal heptyl group, a normal nonyl group, a normal undecyl group, and a normal heptadecyl group, respectively. Compound (16) PPG is polypropylene glycol, and n is the number of repetitions. Compound (16-2) PEG is polyethylene glycol, and n is the number of repetitions. Compound (17) PEs is polyester diol, and n is the number of repetitions, and Ra and two Rb's are each independently a divalent hydrocarbon group having 2 to 25 carbon atoms. The n Ra's in compound (17) PEs may be the same or different. The (n+1) Rb's in compound (17) PEs may be the same or different. Compound (18) PC is polycarbonate diol, and n is the number of repetitions, and the (n+1) Rc's are each independently an alkylene group having 2 to 12 carbon atoms (preferably 3 to 8, more preferably 3 to 6). In compound (18) PC, the (n+1) Rc's may be the same or different. Compound (19) PCL is polycaprolactone diol, where n and m are the repeating numbers, and Rd is an alkylene group having 2 to 25 carbon atoms.
[0065] The polyol units in the urethane resin preferably contain polycarbonate diol units. This further improves the boil resistance of the laminate. In this case, the proportion of polycarbonate diol units in the total amount of polyol units is preferably 50% by mass to 100% by mass, more preferably 60% by mass to 100% by mass, and even more preferably 80% by mass to 100% by mass. The polycarbonate diol for forming the polycarbonate diol units is, for example, the aforementioned compound (18)PC.
[0066] Commercially available polycarbonate diols may be used, such as Duranol T5651 (manufactured by Asahi Kasei Corporation), Duranol T5652 (manufactured by Asahi Kasei Corporation), Duranol T6002 (manufactured by Asahi Kasei Corporation), Duranol T6001 (manufactured by Asahi Kasei Corporation), BENEBiOL HS0830B (manufactured by Mitsubishi Chemical Corporation), BENEBiOL HS0840H (manufactured by Mitsubishi Chemical Corporation), BENEBiOL NL1010DB (manufactured by Mitsubishi Chemical Corporation), and BENEBiOL NL2010DB (manufactured by Mitsubishi Chemical Corporation).
[0067] In the urethane resin, the molar ratio of polyol units to polyisocyanate units (hereinafter also referred to as the molar ratio [OH / NCO]) is preferably 0.4 to 1.0, more preferably 0.5 to 0.9, and even more preferably 0.6 to 0.8. When the molar ratio [OH / NCO] is 0.4 or more, the boil resistance of the laminate is further improved. When the molar ratio [OH / NCO] is 1.0 or less, the storage stability of the pretreatment liquid is further improved.
[0068] (-SO 3 - The urethane resin is -SO 3 - Contains the group —SO 3 - The —SO group functions as a dispersing group for dispersing the urethane resin in the pretreatment liquid. 3 - The -SO group is bonded to the end of the main chain of the urethane resin. 3 - The mobility of the groups is ensured, and as a result, the dispersion stability of the urethane resin and the storage stability of the pretreatment liquid are improved.
[0069] -SO relative to the total amount of urethane resin 3 - The content of —SO groups is 2% by mass to 6% by mass relative to the total amount of the urethane resin. 3 - By ensuring that the content of —SO 3 groups is 2% by mass or more, the storage stability of the pretreatment liquid can be improved. 3 -By making the content of -SO groups 6% by mass or less, the urethane resin is prevented from becoming too hydrophilic, and as a result, the boil resistance of the laminate is improved. 3 - The content of the group is preferably 3% to 5% by mass.
[0070] Urethane resin is SO 3 - The partial structure containing a group preferably contains a partial structure represented by the following formula (I).
[0071]
[0072] In formula (I), * represents a bonding position; 1 is -NH- or -N(L 4 -Y 4 )-, L 4 represents a divalent group which is one kind selected from the first group consisting of an alkylene group, an alkenylene group, an alkynylene group, an arylene group, —O—, —NH—, and —C(═O)—, a divalent group formed by combining two or more kinds selected from the first group, or a single bond; Y 4 represents an alkyl group, an alkenyl group, an alkynyl group, an aryl group, a halogen atom, —OH, —OR 3 , -NH 2 , -NR 3 H, -NR 3 R 4 , or -C(=O)R 3 represents R 3 and R 4 each independently represents an alkyl group, an alkenyl group, an alkynyl group, or an aryl group; L 1 represents an alkylene group having 1 to 4 carbon atoms; Z + is -SO 3 - represents a counter cation for the group.
[0073] Z + The counter cation represented by is —SO 3 - The counter cation may be bonded to the group or may not be bonded (i.e., may be dissociated). Preferred counter cations will be described later.
[0074] L 4 The number of carbon atoms in the alkylene group in L is preferably 1 to 4. 4 The number of carbon atoms in the alkenylene group in L is preferably 2 to 4. 4 The number of carbon atoms in the alkynylene group in L is preferably 2 to 4. 4 The arylene group preferably has 6 to 12 carbon atoms.
[0075] Y 4 The number of carbon atoms in the alkyl group in Y is preferably 1 to 4. 4 The number of carbon atoms in the alkenyl group in Y is preferably 2 to 4. 4 The number of carbon atoms in the alkynyl group in Y is preferably 2 to 4. 4 The number of carbon atoms in the aryl group in Y is preferably 6 to 12. 4 The halogen atom in is preferably a fluorine atom, a chlorine atom, a bromine atom, or an iodine atom.
[0076] R 3 and R 4 The number of carbon atoms in the alkyl group in each of R is preferably 1 to 4. 3 and R 4 The number of carbon atoms in the alkenyl group in each of R is preferably 2 to 4. 3 and R 4 The number of carbon atoms in the alkynyl group in each of R is preferably 2 to 4. 3 and R 4 The aryl group in each of the above preferably has 6 to 12 carbon atoms.
[0077] (-SO 3 - Compound for group introduction) -SO 3 - The -SO group is one of the raw materials used in the production of urethane resin. 3 - It can be introduced into the urethane resin by using a group-introducing compound. 3 - The group-introducing compound is —SO 3 -Examples of the active hydrogen group include an amino group (-NH 2 ), a secondary amino group (-NHR-; R is a substituent, for example, "L" in formula (I) 4 -Y 4 " group), a hydroxy group, etc.
[0078] -SO 3 - The group-introducing compound may be a compound represented by the following formula (IA).
[0079]
[0080] In formula (IA), L 1 and Z + respectively represent L in formula (I). 1 and Z + In formula (IA), R is a hydrogen atom or "L" in formula (I). 4 -Y 4 " is the basis.
[0081] -SO 3 - Specific examples of the group-introducing compound include 2-aminoethanesulfonic acid (also known as taurine), aminomethanesulfonic acid, 3-amino-1-propanesulfonic acid, and 2-(methylamino)ethanesulfonic acid.
[0082] (-SO 3 - Counter cation for the group) Urethane resin is -SO 3 - It may contain a counter cation for the —SO group. 3 - As a counter cation for the group (hereinafter also simply referred to as "counter cation"), Z + Examples of the cations include those represented by the following formula:
[0083] Examples of the counter cation include alkali metal cations, organic base cations, etc. From the viewpoint of further improving the boil resistance of the laminate, organic base cations are preferred as the counter cation.
[0084] The molecular weight of the organic base cation is preferably 73 to 600, more preferably 73 to 400, and even more preferably 73 to 200.
[0085] The organic base cation is preferably an organic ammonium cation.
[0086] From the viewpoint of further improving the storage stability of the pretreatment liquid, the pKa of the counter cation is preferably 9.0 or more, more preferably 10.0 or more. The upper limit of the pKa of the counter cation is, for example, 32.0, preferably 20.0, more preferably 15.0. The pKa refers to a value measured by neutralization titration at 25°C.
[0087] (Compound for introducing counter cation) —SO 3 - The counter cation for the group can be introduced into the urethane resin by using a compound for introducing a counter cation as one of the raw materials when producing the urethane resin. The compound for introducing a counter cation is a compound for introducing a proton (H + In other words, the counter cation is a compound in which one proton (H + ) is added to the cation.
[0088] Examples of compounds for introducing counter cations include diethylamine, triethylamine, diazabicycloundecene (DBU), dibutylamine, trimethylamine, triethanolamine, N-methyldiethanolamine, N,N-dimethylethanolamine, N,N-diisopropylethylamine, 2-aminoethanol, and 2-methylaminoethanol.
[0089] (Preferred Embodiments of Urethane Resin) Preferred embodiments of the urethane resin in the pretreatment liquid are shown below.
[0090] From the viewpoint of further improving the boil resistance of the laminate, the weight average molecular weight of the urethane resin is preferably 5,000 or more, more preferably 6,000 or more, and even more preferably 8,000 or more. From the viewpoint of further improving the storage stability of the pretreatment liquid, the weight average molecular weight of the urethane resin is preferably 50,000 or less, more preferably 40,000 or less, and even more preferably 30,000 or less. From the viewpoints mentioned above, a preferred range of the weight average molecular weight of the urethane resin is 5,000 to 50,000.
[0091] In this disclosure, the weight-average molecular weight is measured by gel permeation chromatography (GPC). GPC is performed using an HLC-8220GPC (manufactured by Tosoh Corporation) with three columns connected in series: TSKgeL SuperHZM-H, TSKgeL SuperHZ4000, and TSKgel SuperHZ2000 (all trade names manufactured by Tosoh Corporation), and THF (tetrahydrofuran) as the eluent. The conditions are a sample concentration of 0.45% by mass, a flow rate of 0.35 ml / min, a sample injection volume of 10 μl, and a measurement temperature of 40°C, and a differential refractive index detector is used. In addition, a calibration curve is prepared from eight samples of "Standard Sample TSK Standard, Polystyrene" manufactured by Tosoh Corporation: "F-40", "F-20", "F-4", "F-1", "A-5000", "A-2500", "A-1000", and "n-propylbenzene".
[0092] From the viewpoint of further improving the boil resistance of the laminate, the glass transition temperature of the urethane resin is preferably −60° C. to 40° C., more preferably −55° C. to 20° C., even more preferably −55° C. to 10° C., and even more preferably −55° C. to 0° C.
[0093] In the present disclosure, the glass transition temperature is measured using a differential scanning calorimeter, for example, a product named "DSC-60" manufactured by Shimadzu Corporation.
[0094] The urethane resin may be a water-soluble urethane resin or a water-insoluble urethane resin (i.e., urethane resin particles). Of these, from the viewpoint of increasing the strength of the layer formed by the pretreatment liquid, the urethane resin is preferably urethane resin particles.
[0095] In this disclosure, "water-soluble" means that 1 g or more dissolves in 100 g of water at 25° C. In this disclosure, "water-insoluble" means that the amount of dissolution in 100 g of water at 25° C. is less than 1 g.
[0096] The average particle size of the urethane resin particles is preferably 1 nm to 200 nm, more preferably 3 nm to 200 nm, and even more preferably 50 nm to 150 nm. The average particle size is determined by measuring the volume average particle size by dynamic light scattering using a particle size distribution analyzer, for example, a product name "Nanotrac UPA-EX150" manufactured by Nikkiso Co., Ltd.
[0097] The content of the urethane resin in the pretreatment liquid is preferably 1% by mass to 30% by mass, more preferably 3% by mass to 20% by mass, and even more preferably 5% by mass to 15% by mass, based on the total amount of the pretreatment liquid.
[0098] <Organic Solvent> The pretreatment liquid of the present disclosure may contain at least one organic solvent.
[0099] The type of organic solvent is not limited, and examples thereof include: monoalcohols having 1 to 4 carbon atoms; diols such as 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, 2-butene-1,4-diol, 2-ethyl-1,3-hexanediol, 2-methyl-2,4-pentanediol, 1,2-octanediol, 1,2-hexanediol, 1,2-pentanediol, and 4-methyl-1,2-pentanediol; triols such as glycerin, 1,2,6-hexanetriol, and trimethylolpropane; alkylene glycols such as ethylene glycol and propylene glycol; alkylene glycol monoalkyl ethers such as ethylene glycol monoalkyl ethers and propylene glycol monoalkyl ethers; polyalkylene glycols such as diethylene glycol, triethylene glycol, tetraethylene glycol, pentaethylene glycol, dipropylene glycol, and polyoxyethylene polyoxypropylene glycol; Examples thereof include polyalkylene glycol ethers such as diethylene glycol monoalkyl ether, triethylene glycol monoalkyl ether, tripropylene glycol monoalkyl ether, and polyoxypropylene glyceryl ether; 2-pyrrolidone, and N-methyl-2-pyrrolidone.
[0100] The content of the organic solvent is preferably 1% by mass to 20% by mass, and more preferably 3% by mass to 10% by mass, based on the total amount of the pretreatment liquid.
[0101] <Surfactant> The pretreatment liquid of the present disclosure may contain at least one surfactant.
[0102] The type of surfactant is not particularly limited, and may be any of anionic surfactants, cationic surfactants, betaine surfactants, and nonionic surfactants. Examples of surfactants include acrylic surfactants, fluorine-based surfactants, and silicone-based surfactants.
[0103] The content of the surfactant is preferably 0.1% by mass to 5% by mass, and more preferably 0.2% by mass to 1% by mass, based on the total amount of the pretreatment liquid.
[0104] <Other Components> The pretreatment liquid of the present disclosure may contain other components in addition to those described above, as necessary. Examples of other components that can be contained in the pretreatment liquid include known additives such as solid wetting agents, colloidal silica, inorganic salts, anti-fading agents, emulsion stabilizers, penetration enhancers, UV absorbers, preservatives, antifungal agents, pH adjusters, viscosity adjusters, rust inhibitors, chelating agents, and water-soluble polymer compounds (for example, the water-soluble polymer compounds described in paragraphs 0026 to 0080 of JP 2013-001854 A).
[0105] <Physical Properties> The pH of the pretreatment liquid is preferably 2.0 to 7.0, and more preferably 2.0 to 4.0. The pH is measured at 25°C using a pH meter, for example, a pH meter manufactured by Toa DKK Corporation (model number "HM-31").
[0106] From the viewpoint of the coatability of the pretreatment liquid, the viscosity of the pretreatment liquid is preferably 0.5 mPa·s to 10 mPa·s, and more preferably 1 mPa·s to 5 mPa·s. The viscosity is a value measured at 25°C using a viscometer. The viscosity is measured at 25°C using a viscometer, for example, a TV-22 type viscometer manufactured by Toki Sangyo Co., Ltd.
[0107] The surface tension of the pretreatment liquid is preferably 60 mN / m or less, more preferably 20 mN / m to 50 mN / m, and even more preferably 30 mN / m to 45 mN / m. The surface tension is a value measured at a temperature of 25°C. The surface tension is measured at 25°C using a surface tensiometer, for example, an automatic surface tensiometer (product name "CBVP-Z" manufactured by Kyowa Interface Science Co., Ltd.) by the plate method.
[0108] [Ink Set] The ink set of the present disclosure includes the pretreatment liquid of the present disclosure described above, and an ink that is an inkjet ink containing water, a pigment, and a urethane resin.
[0109] The ink set of the present disclosure includes the pretreatment liquid of the present disclosure described above, and therefore exhibits the same effects as the pretreatment liquid of the present disclosure described above.
[0110] <Ink> The ink set of the present disclosure includes inks that are inkjet inks containing water, a pigment, and a urethane resin. The ink set of the present disclosure may include only one type of ink, or two or more types of ink.
[0111] (Water) The ink contains water. The water content is preferably 10% by mass or more, more preferably 20% by mass or more, even more preferably 30% by mass or more, and particularly preferably 50% by mass or more, relative to the total amount of the ink. The upper limit of the water content relative to the total amount of the ink is determined appropriately depending on the contents of other components, but is, for example, 99% by mass, preferably 95% by mass, and more preferably 90% by mass.
[0112] (Urethane Resin) The ink contains at least one type of urethane resin. The urethane resin in the ink may be one type or two or more types. The urethane resin in the ink and the urethane resin in the pretreatment liquid may be the same type of urethane resin or different types of urethane resin.
[0113] The urethane resin in the ink is preferably a polyester-based urethane resin having an ester bond in the main chain, a polycarbonate-based urethane resin having a carbonate bond in the main chain, or a polyether-based urethane resin having an ether bond in the main chain.
[0114] The urethane resin in the ink may be a water-soluble urethane resin or a water-insoluble urethane resin (i.e., urethane resin particles). Of these, from the viewpoint of increasing the strength of the layer formed by the ink, the urethane resin is preferably urethane resin particles.
[0115] When the urethane resin in the ink is urethane resin particles, the average particle diameter of the urethane resin particles is preferably 1 nm to 200 nm, more preferably 3 nm to 200 nm, and even more preferably 5 nm to 50 nm, from the viewpoint of ejection stability. The average particle diameter of the urethane resin particles in the ink can be measured by the same method as that for the average particle diameter of the urethane resin particles in the pretreatment liquid.
[0116] The urethane resin in the ink may be anionic, cationic, or nonionic. From the viewpoint of improving the storage stability of the ink, the urethane resin is preferably anionic.
[0117] The weight average molecular weight (Mw) of the urethane resin in the ink is not particularly limited, but is preferably from 1,000 to 300,000, more preferably from 2,000 to 200,000, and even more preferably from 10,000 to 150,000. The weight average molecular weight of the urethane resin in the ink can be measured by the same method as that for the weight average molecular weight of the urethane resin in the pretreatment liquid.
[0118] The urethane resin in the ink may be a commercially available product, such as the Superflex series manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd., the Permarin UA series and U-Coat series manufactured by Sanyo Chemical Industries, Ltd., the Takelac series manufactured by Mitsui Chemicals, Inc., and the PUE series manufactured by Murayama Chemical Laboratory.
[0119] The content of the urethane resin in the ink is preferably 1% by mass to 20% by mass, more preferably 2% by mass to 15% by mass, and even more preferably 2% by mass to 10% by mass, based on the total amount of the ink.
[0120] (Pigment) The ink contains at least one pigment. The pigment contained in the ink may be a white pigment or a colored pigment. The ink may be a white ink containing a white pigment, or a colored ink containing a colored pigment.
[0121] In this disclosure, the term "color pigment" refers to a chromatic pigment or a black pigment. In this disclosure, the term "color ink" refers to a chromatic ink (e.g., cyan ink, magenta ink, yellow ink, etc.) or a black ink.
[0122] From the viewpoint of the concealing properties of the resulting image (i.e., the property of concealing the surface on which the image is to be recorded, such as the surface of a non-permeable substrate), the ink is preferably a white ink containing a white pigment. Here, the concealing properties of the image refer to the property of concealing the surface on which the image is to be recorded (e.g., the surface of a non-permeable substrate, the surface of an image formed as a base, etc.).
[0123] (White Pigment) Examples of white pigments include inorganic pigments such as titanium dioxide, barium sulfate, calcium carbonate, silica, zinc oxide, zinc sulfide, mica, talc, and pearl.
[0124] Among these, the white pigment is preferably titanium dioxide, barium sulfate, calcium carbonate, or zinc oxide, and more preferably titanium dioxide.
[0125] From the viewpoint of hiding power, the average primary particle diameter of the white pigment is preferably 150 nm or more, more preferably 200 nm or more, and from the viewpoint of ink jetting performance, the average primary particle diameter of the white pigment is preferably 400 nm or less, more preferably 350 nm or less.
[0126] In the present disclosure, the average primary particle diameter of the white pigment is a value measured using a transmission electron microscope (TEM). Specifically, 50 particles of the white pigment are randomly selected within the field of view observed with the TEM, and the primary particle diameters of the 50 particles are measured and averaged. As the transmission electron microscope, a 1200EX transmission electron microscope manufactured by JEOL Ltd. can be used.
[0127] From the viewpoints of image density and ejection performance, the content of the white pigment is preferably 2% by mass to 25% by mass, more preferably 5% by mass to 25% by mass, and even more preferably 10% by mass to 20% by mass, relative to the total amount of the ink.
[0128] The ink may contain a color pigment in addition to, or instead of, the white pigment. When the ink contains a color pigment, the type and content of the color pigment can be determined by referring to the section on the second ink described below.
[0129] (Pigment Dispersion Resin) The ink may contain at least one pigment dispersing resin. In the present disclosure, the pigment dispersing resin refers to a resin that has the function of dispersing a pigment. The pigment dispersing resin may be a random copolymer or a block copolymer. The pigment dispersing resin may also have a crosslinked structure. The ink may be prepared using a pigment dispersion containing a pigment and a pigment dispersing resin.
[0130] The pigment dispersing resin is preferably a random copolymer. The random copolymer preferably contains structural units derived from a hydrophobic monomer and structural units derived from a monomer containing an anionic group (hereinafter referred to as an "anionic group-containing monomer"). From the viewpoint of dispersion stability, the content ratio (x:y) of the structural units x derived from the hydrophobic monomer to the structural units y derived from the anionic group-containing monomer is preferably 8:1 to 1:1.
[0131] The random copolymer may contain only one type of structural unit derived from a hydrophobic monomer, or may contain two or more types of structural units derived from an anionic group-containing monomer.
[0132] The hydrophobic monomer preferably contains a monomer having a hydrocarbon group having 4 or more carbon atoms, more preferably contains an ethylenically unsaturated monomer having a hydrocarbon group having 4 or more carbon atoms, and even more preferably contains a (meth)acrylate having a hydrocarbon group having 4 or more carbon atoms. The hydrocarbon group may be any of a chain hydrocarbon group, an alicyclic hydrocarbon group, and an aromatic hydrocarbon group. The number of carbon atoms in the hydrocarbon group is more preferably 6 or more, and even more preferably 10 or more. The upper limit of the number of carbon atoms in the hydrocarbon group is, for example, 20.
[0133] Examples of (meth)acrylates having a chain hydrocarbon group having 4 or more carbon atoms include n-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, lauryl (meth)acrylate, and stearyl (meth)acrylate. The number of carbon atoms in the chain hydrocarbon group is more preferably 6 or more, even more preferably 8 or more, and particularly preferably 12 or more. Of these, the ethylenically unsaturated monomer having a chain hydrocarbon group having 4 or more carbon atoms is preferably lauryl (meth)acrylate or stearyl (meth)acrylate.
[0134] Examples of (meth)acrylates having an alicyclic hydrocarbon group having 4 or more carbon atoms include (bicyclo[2.2.1]heptyl-2-(meth)acrylic acid), 1-adamantyl (meth)acrylate, 2-adamantyl (meth)acrylate, 3-methyl-1-adamantyl (meth)acrylate, 3,5-dimethyl-1-adamantyl (meth)acrylate, 3-ethyladamantyl (meth)acrylate, 3-methyl-5-ethyl-1-adamantyl (meth)acrylate, 3,5,8-triethyl-1-adamantyl (meth)acrylate, 3,5-dimethyl-8-ethyl-1-adamantyl (meth)acrylate, 2-methyl-2-adamantyl (meth)acrylate, 2-ethyl-2-adamantyl (meth)acrylate, acrylate, 3-hydroxy-1-adamantyl(meth)acrylate, octahydro-4,7-menthanoinden-5-yl(meth)acrylate, octahydro-4,7-menthanoinden-1-ylmethyl(meth)acrylate, 1-menthyl(meth)acrylate, tricyclodecane(meth)acrylate, 3-hydroxy-2,6,6-trimethyl-bicyclo[3.1.1]heptyl(meth)acrylate, 3,7,7-trimethyl-4-hydroxy-bicyclo[4.1.0]heptyl(meth)acrylate, (nor)bornyl(meth)acrylate, isobornyl(meth)acrylate, 2,2,5-trimethylcyclohexyl(meth)acrylate, and cyclohexyl(meth)acrylate. The alicyclic hydrocarbon group preferably has 6 or more carbon atoms. Among these, the ethylenically unsaturated monomer having an alicyclic hydrocarbon group having 4 or more carbon atoms is preferably isobornyl (meth)acrylate or cyclohexyl (meth)acrylate.
[0135] Examples of (meth)acrylates having an aromatic hydrocarbon group having 4 or more carbon atoms include 2-naphthyl (meth)acrylate, phenoxyethyl (meth)acrylate, and benzyl (meth)acrylate. Of these, benzyl (meth)acrylate is preferred as the ethylenically unsaturated monomer having an aromatic hydrocarbon group having 4 or more carbon atoms.
[0136] The hydrophobic monomer may further contain a (meth)acrylate having a hydrocarbon group having 1 to 3 carbon atoms.
[0137] Examples of (meth)acrylates having a hydrocarbon group having 1 to 3 carbon atoms include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, and hydroxyethyl (meth)acrylate.
[0138] In particular, from the viewpoint of improving the dispersion stability of the white pigment, the structural units derived from hydrophobic monomers contained in the pigment dispersing resin preferably include a structural unit derived from a (meth)acrylate having a chain hydrocarbon group with 4 or more carbon atoms and a structural unit derived from a (meth)acrylate having an aromatic hydrocarbon group with 4 or more carbon atoms.
[0139] Examples of the anionic group in the anionic group-containing monomer include a carboxy group, a salt of a carboxy group, a sulfo group, a salt of a sulfo group, a phosphoric acid group, a salt of a phosphoric acid group, a phosphonic acid group, and a salt of a phosphonic acid group.
[0140] Counter ions in salts include alkali metal ions such as sodium ion, potassium ion, and lithium ion; alkaline earth metal ions such as calcium ion and magnesium ion; and ammonium ion.
[0141] Among these, the anionic group is preferably a carboxy group or a salt of a carboxy group.
[0142] Examples of carboxy group-containing monomers include (meth)acrylic acid, β-carboxyethyl acrylate, fumaric acid, itaconic acid, maleic acid, and crotonic acid.
[0143] From the viewpoint of dispersion stability, the anionic group-containing monomer is preferably (meth)acrylic acid or β-carboxyethyl acrylate, and more preferably (meth)acrylic acid.
[0144] The ratio of the content of the white pigment to the content of the pigment dispersing resin is preferably 1:0.04 to 1:3, more preferably 1:0.05 to 1:1, and even more preferably 1:0.05 to 1:0.5, on a mass basis.
[0145] From the viewpoint of dispersion stability, the acid value of the pigment dispersing resin is preferably 100 mgKOH / g or more, more preferably 120 mgKOH / g or more, while from the viewpoint of dispersion stability, the acid value of the pigment dispersing resin is preferably 300 mgKOH / g or less, more preferably 230 mgKOH / g or less.
[0146] When the ink contains a pigment dispersion resin, the content of the pigment dispersion resin relative to the total amount of the ink is preferably 0.1% by mass to 10% by mass, more preferably 0.3% by mass to 5% by mass, and even more preferably 0.5% by mass to 2.5% by mass.
[0147] (Organic Solvent) The ink preferably contains an organic solvent, which improves ejection stability. The organic solvent contained in the color ink may be one type or two or more types.
[0148] Examples of the organic solvent include the same organic solvents as those contained in the pretreatment liquid. From the viewpoint of ejection stability, the organic solvent preferably contains at least one selected from the group consisting of alkylene glycols and alkylene glycol monoalkyl ethers.
[0149] The content of the organic solvent is preferably 10% by mass to 40% by mass, and more preferably 15% by mass to 30% by mass, based on the total amount of the ink.
[0150] (Additives) The ink may contain additives such as surfactants, water-soluble resins, co-sensitizers, ultraviolet absorbers, antioxidants, anti-fading agents, conductive salts, and basic compounds, as needed.
[0151] (Physical Properties) From the viewpoint of improving ejection stability, the pH (25°C) of the ink is preferably from 7 to 10, and more preferably from 7.5 to 9.5. The pH of the color ink can be measured in the same manner as the pH of the pretreatment liquid.
[0152] The viscosity of the ink (30°C) is preferably 0.5 mPa·s to 30 mPa·s, more preferably 2 mPa·s to 20 mPa·s, more preferably 2 mPa·s to 15 mPa·s, and even more preferably 3 mPa·s to 10 mPa·s. The viscosity of the color ink can be measured in the same manner as the viscosity of the pretreatment liquid.
[0153] The surface tension of the ink (at 25°C) is preferably 60 mN / m or less, more preferably 20 mN / m to 50 mN / m, and even more preferably 30 mN / m to 45 mN / m. The surface tension can be measured in the same manner as for the pretreatment liquid.
[0154] <First ink, second ink> The ink set of the present disclosure may include the above-described white ink (hereinafter also referred to as the "first ink"), which is an inkjet ink containing water, a white pigment, and a urethane resin, and a colored ink (hereinafter also referred to as the "second ink"), which is an inkjet ink containing water, a colored pigment, and a urethane resin. In this case, the ink set may include two or more types of white ink, or may include two or more types of colored ink (for example, a combination of cyan ink, magenta ink, yellow ink, and black ink).
[0155] That is, one specific aspect of the ink set of the present disclosure is an aspect including: a pretreatment liquid of the present disclosure; a first ink as a white ink, which is an inkjet ink containing water, a white pigment, and a resin having a carboxy group; and a second ink as a colored ink, which is an inkjet ink containing water, a color pigment, and a resin having a carboxy group.
[0156] Preferred aspects of the second ink are the same as preferred aspects of the first ink (i.e., white ink), except that it contains a color pigment as an essential component. For example, preferred aspects of the type and content of each component in the second ink are the same as preferred aspects of the type and content of each component in the first ink.
[0157] (Coloring Pigment) The coloring pigment may be either an organic pigment or an inorganic pigment that is usually commercially available. Examples of the coloring pigment include those described in "Pigment Dictionary" edited by Seijiro Ito (published in 2000), "Industrial Organic Pigments" by W. Herbst and K. Hunger, and JP-A Nos. 2002-12607, 2002-188025, 2003-26978, and 2003-342503.
[0158] The color pigment may be a water-insoluble pigment that can be dispersed in water with the aid of a dispersant, or may be a self-dispersing pigment. A self-dispersing pigment is a pigment that can be dispersed in water without the aid of a dispersant. A self-dispersing pigment is a compound in which at least one hydrophilic group selected from the group consisting of a carbonyl group, a hydroxyl group, a carboxyl group, a sulfo group, a phosphate group, and salts thereof is chemically bonded to the surface of the pigment directly or via another group.
[0159] The type of color pigment is not particularly limited, and examples thereof include cyan pigments, magenta pigments, yellow pigments, and black pigments.
[0160] From the viewpoints of image density and ejection properties of the second ink, the content of the color pigment is preferably 1% by mass to 20% by mass, more preferably 1% by mass to 15% by mass, and even more preferably 1% by mass to 10% by mass, relative to the total amount of the second ink.
[0161] [Image Recording Method] The image recording method of the present disclosure includes: a step of applying a pretreatment liquid of the present disclosure onto a non-permeable substrate (hereinafter also referred to as a "pretreatment liquid applying step"); and a step of applying an ink containing water, a pigment, and a urethane resin (i.e., an inkjet ink; the same applies hereinafter) onto the area of the non-permeable substrate to which the pretreatment liquid has been applied, by an inkjet recording method (hereinafter also referred to as an "ink applying step").
[0162] The image recording method of the present disclosure uses the pretreatment liquid of the present disclosure described above, and therefore has the same effects as the pretreatment liquid of the present disclosure described above.
[0163] The image recording method of the present disclosure may be carried out using the ink set of the present disclosure described above.
[0164] The ink used in the ink application step is the same as the ink described in the section on the ink set of the present disclosure, and preferred embodiments are also the same. From the viewpoint of the concealing properties of the image, the ink used in the ink application step is preferably a white ink containing a white pigment.
[0165] <Pretreatment Liquid Application Step> The pretreatment liquid application step is a step of applying the pretreatment liquid in the ink set of the present disclosure (i.e., the pretreatment liquid of the present disclosure) onto a non-permeable substrate.
[0166] (Impermeable substrate) In the present disclosure, the impermeability of an impermeable substrate refers to a property in which the water absorption rate over 24 hours measured in accordance with ASTM D570-98 (2018) is 2.5% or less. Here, the unit of water absorption rate, "%", is based on mass. The water absorption rate is preferably 1.0% or less, and more preferably 0.5% or less.
[0167] Examples of materials for the impermeable substrate include glass, metals (e.g., aluminum, zinc, copper, etc.), and resins (e.g., polyvinyl chloride, cellulose diacetate, cellulose triacetate, cellulose propionate, cellulose butyrate, cellulose acetate butyrate, cellulose nitrate, polyethylene terephthalate, polyethylene, polystyrene, polypropylene, polycarbonate, polyvinyl acetal, nylon, acrylic resin, etc.).
[0168] The material of the impermeable substrate is preferably a resin, that is, the impermeable substrate is preferably a resin substrate.
[0169] Among these, from the viewpoint of versatility, the material of the impermeable substrate is preferably polypropylene, polyethylene, polyethylene terephthalate, nylon, acrylic resin, or polyvinyl chloride.
[0170] The shape of the impermeable substrate is preferably a sheet (film) or plate, and examples of such a shape of the impermeable substrate include a glass plate, a metal plate, a resin sheet (resin film), a plastic-laminated paper, a metal-laminated or metal-deposited paper, and a metal-laminated or metal-deposited plastic sheet (plastic film).
[0171] Examples of impermeable resin substrates include resin sheets (resin films), and specific examples include flexible packaging materials for packaging foods and the like, and floor guide panels in mass retailers.
[0172] Examples of impermeable substrates include not only sheet-shaped (film-shaped) or plate-shaped impermeable substrates, but also textiles (woven fabrics) and nonwoven fabrics formed from impermeable fibers.
[0173] The thickness of the impermeable substrate is preferably 0.1 μm to 1,000 μm, more preferably 0.1 μm to 800 μm, and even more preferably 1 μm to 500 μm.
[0174] The non-permeable substrate may be subjected to a hydrophilization treatment. Examples of hydrophilization treatments include, but are not limited to, corona treatment, plasma treatment, flame treatment, heat treatment, abrasion treatment, light irradiation treatment (e.g., UV treatment), and flame treatment. Corona treatment can be carried out using, for example, a Corona Master (product name "PS-10S", manufactured by Shinko Electric Meter Co., Ltd.). The conditions for the corona treatment may be appropriately selected depending on the type of non-permeable substrate, etc.
[0175] The non-permeable substrate may be a transparent non-permeable substrate. Here, "transparent" means that the transmittance of visible light in the wavelength range of 400 nm to 700 nm is 80% or more (preferably 90% or more). When the non-permeable substrate is a transparent non-permeable substrate, an image is easily visible through the non-permeable substrate from the non-image recording surface side of the non-permeable substrate. For example, when the non-permeable substrate is a transparent non-permeable substrate, when an image is recorded on the non-permeable substrate by applying a pretreatment liquid, a second ink as a colored ink, and a first ink as a white ink in this order, a colored image (e.g., a pattern image such as letters or figures) against a white image (e.g., a solid image) is easily visible through the non-permeable substrate from the non-image recording surface side of the non-permeable substrate.
[0176] (Application of Pretreatment Liquid) The method for applying the pretreatment liquid is not particularly limited, and examples thereof include known methods such as a coating method, a dipping method, and an inkjet recording method.
[0177] Examples of the coating method include known coating methods using a bar coater, extrusion die coater, air doctor coater, blade coater, rod coater, knife coater, squeeze coater, reverse roll coater, and the like.
[0178] (Heat-Drying of Pretreatment Liquid) The pretreatment liquid application step may include applying the pretreatment liquid onto the non-permeable substrate and heat-drying the pretreatment liquid applied onto the non-permeable substrate. Examples of means for heat-drying the pretreatment liquid include known heating means such as a heater, known air blowing means such as a dryer, and a combination of these.
[0179] Examples of methods for heating and drying the pretreatment liquid include a method of applying heat using a heater or the like from the side opposite to the surface of the non-permeable substrate to which the pretreatment liquid has been applied, a method of applying warm air or hot air to the surface of the non-permeable substrate to which the pretreatment liquid has been applied, a method of applying heat using an infrared heater from the side of the non-permeable substrate to which the pretreatment liquid has been applied or the side opposite to the surface to which the pretreatment liquid has been applied, and a combination of these methods.
[0180] The heating temperature during heating and drying of the pretreatment liquid is preferably 35° C. or higher, and more preferably 40° C. or higher. There is no particular upper limit to the heating temperature, but it is preferably 100° C., more preferably 90° C., and even more preferably 70° C.
[0181] The time for heat drying is not particularly limited, but is preferably 0.5 to 60 seconds, more preferably 0.5 to 20 seconds, and even more preferably 0.5 to 10 seconds.
[0182] Ink Application Step: The ink application step is a step of applying ink by inkjet recording onto the non-permeable substrate to which the pretreatment liquid has been applied. In this step, the components in the ink are aggregated on the non-permeable substrate by the action of the aggregating agent in the pretreatment liquid, thereby forming an image.
[0183] (Application of ink) There are no particular limitations on the ink ejection method used in inkjet recording, and any of the well-known methods may be used, such as a charge control method that uses electrostatic attraction to eject ink, a drop-on-demand method (pressure pulse method) that uses the vibration pressure of a piezoelectric element, an acoustic inkjet method that converts an electric signal into an acoustic beam and irradiates the ink with it, thereby ejecting the ink using radiation pressure, and a thermal inkjet (Bubble Jet (registered trademark)) method that heats the ink to form bubbles and uses the resulting pressure.
[0184] As an inkjet recording method, in particular, the method described in JP-A-54-59936 can be effectively used, in which ink subjected to the action of thermal energy undergoes a sudden change in volume, and the ink is ejected from the nozzles by the force caused by this state change. As an inkjet recording method, the method described in paragraphs 0093 to 0105 of JP-A-2003-306623 can also be applied.
[0185] Application of ink to a non-permeable substrate by ink jet recording is carried out by ejecting the ink from the nozzles of an ink jet head.
[0186] Inkjet head methods include the shuttle method, in which a short serial head is scanned across the width of the recording medium to perform recording, and the line method, which uses a line head in which recording elements are arranged to cover the entire area of one side of the recording medium.
[0187] The line method allows for image recording over the entire surface of a recording medium by scanning the recording medium in a direction intersecting the arrangement direction of the recording elements. The line method eliminates the need for a transport system, such as a carriage that scans a short head, as in the shuttle method. Furthermore, compared to the shuttle method, the line method does not require complex scanning control of the carriage movement and the recording medium, and only the recording medium moves. Therefore, the line method achieves faster image recording speeds than the shuttle method.
[0188] The ink is preferably applied using an inkjet head having a resolution of 300 dpi or more (more preferably 600 dpi or more, and even more preferably 800 dpi or more), where dpi stands for dots per inch, and 1 inch is 2.54 cm.
[0189] From the viewpoint of obtaining a high-definition image, the amount of ink droplets ejected is preferably 1 pL (picoliter) to 10 pL, and more preferably 1.5 pL to 6 pL.
[0190] The amount of ink applied to the area on the non-permeable substrate where the pretreatment liquid has been applied is preferably 3.0 g / m 2 ~15.0g / m 2 , more preferably 5.0 g / m 2 ~12.0g / m 2 is.
[0191] (Heat Drying) The ink application step may include applying ink by an inkjet method onto the non-permeable substrate to which the pretreatment liquid has been applied, and heating and drying the applied ink.
[0192] The heat drying method is not particularly limited, and examples thereof include infrared (IR) drying, hot air drying, and heat drying using a heating device (e.g., a heater, a hot plate, a heating furnace, etc.). The heat drying method may be a combination of two or more of these. Heat drying can be performed by heating the ink from at least one of the image recording side and the non-image recording side of the non-permeable substrate.
[0193] The heating temperature for drying the ink by heating is preferably 35° C. or higher, more preferably 40° C. or higher, even more preferably 50° C. or higher, and even more preferably 60° C. or higher. There is no particular upper limit to the heating temperature, but 100° C. is preferred, and 90° C. is more preferred.
[0194] The heating time for heating and drying the ink is not particularly limited, but is preferably 1 to 180 seconds, more preferably 1 to 120 seconds, and even more preferably 1 to 60 seconds.
[0195] An example of the image recording method of the present disclosure when using inks of two or more colors is an image recording method that uses the first ink (i.e., white ink) and second ink (i.e., colored inks) described above. The image recording method according to this example includes the steps of: applying the pretreatment liquid of the present disclosure onto a non-permeable substrate; and applying the first ink (i.e., white ink) and the second ink (i.e., colored inks) described above, respectively, onto the region of the non-permeable substrate to which the pretreatment liquid has been applied, by inkjet recording.
[0196] The step of applying the pretreatment liquid onto the impermeable substrate is as described above.
[0197] According to the image recording method of this embodiment, a multi-color image can be recorded using a first ink (i.e., white ink) and a second ink (i.e., colored ink). Examples of multi-color images include a colored image (e.g., a pattern image such as letters or figures) against a white background (e.g., a solid image). The order in which the first ink (i.e., white ink) and the second ink (i.e., colored ink) are applied can be any order. For example, when the image is viewed from the image-recording side, the first ink (i.e., white ink) is applied first, followed by the second ink (i.e., colored ink). When the image is viewed from the non-image-recording side through a non-permeable substrate, the second ink (i.e., colored ink) is applied first, followed by the first ink (i.e., white ink). This allows, for example, a multi-color image to be recorded on the non-permeable substrate, in which a pattern image (e.g., letters or figures) recorded with colored inks and a solid white image recorded with white ink so as to cover the pattern image are arranged in this order.
[0198] In the step of applying the first ink and the second ink, the method of applying each of the first ink and the second ink by an inkjet recording method is as described above. Furthermore, the step of applying the first ink and the second ink may include heating and drying the ink after applying at least one of the first ink and the second ink. The preferred conditions for the heating and drying are as described above. For example, an embodiment of this step may include applying the second ink (i.e., colored ink), applying the first ink (i.e., white ink), and drying in this order. In this embodiment, the second ink may or may not be heated and dried between the applications of the second ink.
[0199] [Method for manufacturing a laminated body] The method for manufacturing a laminated body of the present disclosure includes the steps of: obtaining an image recorded matter comprising an impermeable substrate and an image disposed on the impermeable substrate by the image recording method of the present disclosure described above; and laminating a laminating substrate onto the side of the image recorded matter on which the image is disposed, to obtain a laminated body.
[0200] The method for producing a laminate according to the present disclosure includes the image recording method according to the present disclosure, and therefore has the same effects as those of the image recording method according to the present disclosure. Specifically, a laminate having excellent boil resistance can be obtained.
[0201] For the step of obtaining an image recorded material, reference can be made to the image recording method of the present disclosure. The step of obtaining a laminated body is a step of laminating a laminating substrate on the side of the image recorded material on which the image is arranged to obtain a laminated body. Lamination can be performed by, for example, a method of overlapping and attaching the laminating substrate to the side on which the image is arranged of the image recorded material via another layer (e.g., an adhesive layer), or a method of overlapping and attaching the laminating substrate to the side on which the image is arranged of the image recorded material through a laminator. In the latter case, a commercially available laminator can be used.
[0202] The lamination temperature when laminating is not particularly limited. For example, when the image-recorded material and the substrate for lamination are attached via another layer (for example, an adhesive layer), the temperature may be in the range of 20°C or higher. Furthermore, when a laminator is used, the temperature of the laminating rolls may be in the range of 20°C to 80°C. The pressure between the pair of laminating rolls may be appropriately selected as needed.
[0203] The substrate for lamination is preferably a resin substrate, and is not particularly limited, but examples thereof include substrates made of thermoplastic resins.
[0204] The resin substrate may be, for example, a substrate formed by molding a thermoplastic resin into a sheet shape, and preferably contains polypropylene, polyethylene terephthalate, nylon, polyethylene, or polyimide.
[0205] The shape of the resin substrate is not particularly limited, but a sheet-like resin substrate is preferred. The thickness of the resin substrate is preferably 10 μm to 200 μm, more preferably 10 μm to 100 μm.
[0206] In the step of obtaining a laminate, the lamination substrate may be laminated directly onto the image-bearing side of the image-recorded product, or may be laminated via another layer (for example, an adhesive layer).
[0207] When the substrate for lamination is directly laminated onto the side of the image-recorded product on which the image is disposed, the lamination can be carried out by a known method such as thermocompression bonding or heat fusion bonding.
[0208] Furthermore, when laminating a substrate for lamination via an adhesive layer onto the side of an image recorded material on which an image is disposed, the lamination can be carried out, for example, by applying an adhesive to the side of the image recorded material on which the image is disposed, then placing the substrate for lamination on the side, and then bonding the image recorded material and the substrate for lamination together.
[0209] Furthermore, lamination via an adhesive layer on the image-bearing side of the image-recorded product can also be carried out by a method such as extrusion lamination (i.e., sandwich lamination).
[0210] The adhesive layer preferably contains an isocyanate. When the adhesive layer contains an isocyanate, the adhesion between the adhesive layer and the image is further improved, and therefore the boiling resistance can be further improved.
[0211] [Image Recorded Material] The image recorded material of the present disclosure comprises an impermeable substrate and an image disposed on the impermeable substrate, wherein the image comprises: a pretreatment layer disposed on the impermeable substrate, the pretreatment layer containing a flocculant that is at least one selected from the group consisting of an organic acid, an organic acid salt, a polyvalent metal compound, and a metal complex, and a urethane resin; and an ink layer disposed on the pretreatment layer, the ink layer containing a pigment (for example, at least one of a white pigment and a colored pigment) and a urethane resin, wherein the urethane resin in the pretreatment layer contains a polyol unit, a polyisocyanate unit, and a polyalkylene glycol monoalkyl ether unit.
[0212] The image recorded matter of the present disclosure can be produced by the image recording method of the present disclosure, and therefore a laminated article with excellent boil resistance can be produced.
[0213] For the components in the pretreatment layer and the components in the ink layer, the components of the pretreatment liquid, the components of the first ink, and the components of the second ink described above can be referenced as appropriate.
[0214] The laminate of the present disclosure comprises the image recorded matter of the present disclosure described above and a lamination substrate laminated onto the image of the image recorded matter.
[0215] The laminated body of the present disclosure can be produced by the method for producing a laminated body of the present disclosure. Therefore, the laminated body has excellent boil resistance. Preferred embodiments of the substrate for lamination are as described above.
[0216] The present disclosure will be described in more detail below with reference to examples, but the present disclosure is not limited to the following examples as long as it does not depart from the gist of the disclosure. The following description will be centered on Example 2.
[0217] Example 2 Preparation of Aqueous Dispersion of Urethane Resin Particles for Pretreatment Liquid Isophorone diisocyanate (IPDI) (26.6 g), Duranol T5651 (polycarbonate diol, manufactured by Asahi Kasei Corporation; hereinafter also referred to as T5651) (80.7 g), and ethyl acetate (74.9 g) were charged into a three-necked flask and heated to 70° C. 0.1 g of Neostan U-600 (inorganic bismuth catalyst, manufactured by Nitto Kasei Corporation; hereinafter also referred to as U-600) was added thereto, and the mixture was stirred at 70° C. for 3 hours. After stirring, the temperature of the liquid was lowered to 60°C, and a solution containing a mixture of diazabicycloundecene (DBU) (6.6 g) as a counter cation-introducing compound, methanol (123.6 g), and 2-aminoethanesulfonic acid (taurine) (5.0 g) as a dispersing group-introducing compound was added thereto and stirred at 60°C for 1 hour. Next, ethyl acetate (82.8 g) was added thereto and stirred at 60°C for 1 hour. After stirring for 1 hour, the mixture was allowed to cool to room temperature, and then the concentration was adjusted using ethyl acetate to obtain a 30% by mass solution of urethane A (solvent: a mixed solvent of methanol and ethyl acetate). Distilled water (100 g) was added to the obtained 30% by mass solution of urethane A, and the mixture was emulsified at room temperature for 30 minutes at 7000 rpm using a homogenizer to obtain an emulsion. The obtained emulsion was heated to 50°C and stirred at 50°C for 5 hours, whereby ethyl acetate was distilled off from the liquid. The liquid from which ethyl acetate had been distilled was diluted with distilled water to a solid content of 25% by mass, thereby obtaining an aqueous dispersion of urethane resin particles (solid content 25% by mass). 3 - group, and the counter cation is one molecule of diazabicycloundecene and a proton (H + ) and one organic ammonium cation.
[0218] Table 1 shows the type of polyol (hereinafter also referred to as "OH"), the type of polyisocyanate (hereinafter also referred to as "NCO"), the molar ratio [OH / NCO], the type of dispersing group-introducing compound, the type of dispersing group, the position of the dispersing group, and -SO 3 -The molar ratio [OH / NCO] indicates the molar ratio of polyol units to polyisocyanate units. 3 - Regarding the position of the dispersing group, "terminal" means that the dispersing group is bonded to the terminal of the main chain of the urethane resin. The position of the dispersing group is determined by the type of dispersing group-introducing compound. When the dispersing group-introducing compound is a compound containing one active hydrogen group (for example, an amino group, a hydroxy group, etc.; the same applies below), (for example, the above-mentioned taurine), the dispersing group is bonded to the terminal of the main chain of the urethane resin; when the dispersing group-introducing compound is a compound containing two active hydrogen groups (for example, N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonic acid, described below), the dispersing group is bonded to a side chain of the urethane resin. -SO 3 - The amount of -SO 3 - It means the content (mass%) of the group (dispersing group).
[0219] <Preparation of Pretreatment Liquid> A pretreatment liquid having the following composition was prepared using the aqueous dispersion of urethane resin particles and the components listed below other than the urethane resin particles.
[0220] - Composition of pretreatment liquid - Ethanol: 5% by mass Urethane resin particles: 10% by mass Flocculant shown in Table 1: 5% by mass Surfactant (product name "Olfine E1010", manufactured by Nissin Chemical Industry Co., Ltd.): 0.5% by mass Triisopropanolamine: 0.5% by mass Water: the remaining amount to make the total pretreatment liquid 100% by mass
[0221] <Synthesis of Pigment Dispersion Resin 1> 100 g of dipropylene glycol was added to a three-neck flask equipped with a stirrer and a condenser and heated to 85°C under a nitrogen atmosphere. Solution 1 was prepared by mixing 14.0 g of stearyl methacrylate, 35.3 g of benzyl methacrylate, 20.0 g of hydroxyethyl methacrylate, 30.7 g of methacrylic acid, and 0.55 g of 2-mercaptopropionic acid. Solution 2 was prepared by dissolving 1.0 g of t-butylperoxy-2-ethylhexanoate (product name "Perbutyl O", manufactured by NOF Corporation) in 20 g of dipropylene glycol. Solution 1 was added dropwise to the three-neck flask over 4 hours, and solution 2 over 5 hours. After the dropwise addition, the mixture was allowed to react for an additional 2 hours, and then the temperature was raised to 95°C and heated and stirred for 3 hours to allow all unreacted monomers to react. The disappearance of the monomers was monitored by nuclear magnetic resonance ( 1 The resulting reaction solution was heated to 70°C, and 12.0 g of dimethylethanolamine was added, followed by the addition of propylene glycol and stirring to obtain a 30% by mass solution of pigment dispersion resin 1. The structural unit of the resulting pigment dispersion resin 1 was 1 The molecular weight was confirmed by H-NMR. The weight average molecular weight (Mw) determined by GPC was 28,000. The mass ratio of the structural units in pigment dispersion resin 1 was stearyl methacrylate-derived structural units / benzyl methacrylate-derived structural units / hydroxyethyl methacrylate-derived structural units / methacrylic acid-derived structural units = 14 / 35.3 / 20 / 30.7. However, the above mass ratio does not include dimethylaminoethanol. The acid value of pigment dispersion resin 1 was 200 mgKOH / g.
[0222] <Preparation of Pigment Dispersion 1> Pigment Dispersion 1 was prepared using a ready mill, Model LSG-4U-08 (manufactured by Imex Co., Ltd.). 45 parts by mass of titanium dioxide particles (average primary particle diameter: 210 nm, product name "PF-690", manufactured by Ishihara Sangyo Kaisha, Ltd.) serving as a white pigment, 15 parts by mass of a 30% by mass solution of the above-described pigment dispersion resin 1, and 40 parts by mass of ultrapure water were added to a zirconia container. 40 parts by mass of 0.5 mm diameter zirconia beads (Toraceram beads, manufactured by TORAY Corporation) were then added and gently mixed with a spatula. The zirconia container containing the resulting mixture was placed in a ready mill, and dispersion was carried out for 5 hours at a rotation speed of 1,000 rpm (revolutions per minute). After dispersion was complete, the beads were removed by filtration using a filter cloth, yielding Pigment Dispersion 1 having a white pigment concentration of 45% by mass.
[0223] <Preparation of White Ink> A white ink having the following composition was prepared using pigment dispersion liquid 1 and the components listed below other than pigment dispersion resin 1 and the white pigment.
[0224] -Composition of white ink- White pigment... 15% by mass Pigment dispersion resin 1... 1.5% by mass 1,2-propanediol (PG)... 20% by mass Propylene glycol monomethyl ether (PGmME)... 1% by mass Propylene glycol monopropyl ether (PGmPE)... 1% by mass Surfynol 104 (manufactured by Nissin Chemical Industry Co., Ltd.; acetylene glycol-based surfactant)... 1% by mass BYK-345 (manufactured by BYK; silicone-based surfactant)... 1% by mass PVP K-15 (manufactured by ASHLAND; polyvinylpyrrolidone)... 0.1% by mass Snowtex XS (manufactured by Nissan Chemical Industries, Ltd.; colloidal silica)... 0.05% by mass as solids Permarin UA-368 (Sanyo Chemical Industries, Ltd.; resin emulsion containing polycarbonate-based urethane resin)... 4% by mass as solids Water: The remaining amount to make the total 100% by mass
[0225] <Image Recording> Image recording was performed using the pretreatment liquid and white ink. An inkjet recording apparatus was prepared, which included a conveying system for continuously conveying a long substrate, a wire bar coater for applying the pretreatment liquid to the substrate, and an inkjet head for applying the ink. Furthermore, a non-permeable polyethylene terephthalate (PET) substrate ("FE2001" manufactured by Futamura Chemical Co., Ltd., 12 μm thick, 780 mm wide, and 4000 m long; hereinafter referred to as "non-permeable substrate A") was prepared as the substrate.
[0226] The above pretreatment liquid was applied to the non-permeable substrate A at a rate of about 1.7 g / m using a wire bar coater. 2 The white ink was applied in the form of a solid image from an inkjet head while continuously conveying the non-permeable substrate A at 50 m / min using an inkjet recording device. The applied white ink was dried with hot air at 80°C for 30 seconds to record a solid image, thereby obtaining an image recording.
[0227] - Ink application conditions - Inkjet head: 1200 dpi / 30 inch wide piezo full line head Amount of ink ejected from inkjet head: 3.0 pL (picoliters) Driving frequency: 41 kHz (substrate conveying speed: 50 m / min)
[0228] [Evaluation] The storage stability of the pretreatment liquid and the boiling resistance of the image recording material were evaluated. The evaluation methods are as follows. The evaluation results are shown in Table 1.
[0229] (Storage Stability of Pre-Treatment Liquid) The viscosity of the pre-treatment liquid prepared and then allowed to stand at 25°C for 1 hour (hereinafter referred to as "viscosity before storage") and the viscosity of the pre-treatment liquid prepared and then stored in a sealed state at 60°C for 14 days (hereinafter referred to as "viscosity after storage") were measured. Both the viscosity before storage and the viscosity after storage were measured using a VISCOMETER TV-22 (manufactured by TOKI SANGYO CO., LTD.) at 25°C and 100 rpm (revolutions per minute). Here, a sealed state refers to a state in which the contents are sealed in a container and, when stored at 50°C for 14 days, the amount of weight loss of the contents is less than 1% by mass. The viscosity increase was calculated by subtracting the viscosity before storage from the viscosity after storage. The smaller the viscosity increase, the better the storage stability. The evaluation criteria are as follows.
[0230] - Evaluation criteria for storage stability of pre-treatment liquid - A: The viscosity increase was less than 0.3 mPa s. B: The viscosity increase was 0.3 mPa s or more and less than 1.0 mPa s. C: The viscosity increase was 1.0 mPa s or more and less than 2.0 mPa s. D: The viscosity increase was 2.0 mPa s or more.
[0231] (Boiling resistance of laminated body) Using a dry laminating machine (product name "FL2", manufactured by Fuji Machine Industry Co., Ltd.), a dry laminating adhesive (main agent TM-320 (isocyanate) / curing agent CAT-13B (alcohol compound); manufactured by Toyo-Morton Co., Ltd.) was applied onto the solid image of the image recorded material, and a linear low-density polyethylene film (product name "LL-XMTN", manufactured by Futamura Chemical Co., Ltd., thickness 40 μm) was placed thereon as a laminating substrate. In this state, the laminating substrate and the image recorded material were bonded together to obtain a laminated body.
[0232] The resulting laminate was aged at 40°C for 48 hours. Two sample pieces, each 200 mm long and 200 mm wide, were cut out from the aged laminate. The cut-out sample pieces were overlapped and heat-sealed on three sides to obtain a bag. The resulting bag was filled with pure water and then heat-sealed.
[0233] The sealed bag was placed in an autoclave (small sterilizer) for retort foods (product name "SR-240", manufactured by Tommy Seiko Co., Ltd.) and subjected to boiling treatment at 95°C for 40 minutes. After boiling treatment, the bag was removed and the condition of the bag was visually observed. Specifically, boil resistance was evaluated based on the deformation of the bag and the presence or absence of laminate lifting. The evaluation criteria are as follows. Laminate lifting refers to a state in which lifting occurs due to peeling of the image or laminate substrate.
[0234] - Evaluation criteria for boil resistance of laminate - A: No deformation or laminate lifting was observed. B: No laminate lifting, but deformation was observed. C: Laminate lifting was observed in one or more places. D: Laminate lifting was observed over the entire surface of the sample piece.
[0235] [Examples 1 and 3 to 20, and Comparative Examples 1 to 4] The type of flocculant in the pretreatment liquid, the raw materials of the urethane resin particles (specifically, the type of polyol, the type of polyisocyanate, the molar ratio [OH / NCO], the type of compound for introducing dispersing groups, -SO 3 - The same operations as in Example 2 were carried out, except that at least one of the following was changed as shown in Table 1: the amount of the urethane resin in the urethane resin particles, the type of the compound for introducing a counter cation, and the weight average molecular weight of the urethane resin in the urethane resin particles. The weight average molecular weight of the urethane resin in the urethane resin particles was changed by changing the reaction time.
[0236] The meanings of the abbreviations in Table 1 are as follows: IPDI: isophorone diisocyanate HMDI: hexamethylene diisocyanate HXDI: 1,3-bis(isocyanatomethyl)cyclohexane PCD: polycarbonate diol (trade name Duranol T5651 (manufactured by Asahi Kasei Corporation), molecular weight 1000) PPG: polypropylene glycol (molecular weight 1000) PTMG: polytetramethylene glycol (trade name PTMG1000 (manufactured by Mitsubishi Chemical Corporation), molecular weight 1000) TCD: tricyclo[5.2.1.0] 2,6] Decane dimethanol DMPA ... Dimethylolpropionic acid BES ... N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonic acid SSNa ... Sodium styrenesulfonate DBU ... Diazabicycloundecene NEt 3 … Triethylamine
[0237] The molar ratio [OH / NCO] (i.e., the molar ratio of polyol units to polyisocyanate units) was adjusted by adjusting the molar ratio of polyol charged to polyisocyanate. 3 - The amount (dispersing group) was adjusted by adjusting the amount of the compound for introducing dispersing groups.
[0238] Example 21 The same procedure as in Example 2 was carried out, except that the urethane resin particles in the white ink were changed to acrylic resin particles. The white ink of Example 21 was prepared using Movinyl 972 (manufactured by Japan Coating Resins Co., Ltd.), an aqueous dispersion of acrylic resin particles.
[0239] Comparative Example 5 The same procedure as in Example 2 was carried out, except that the urethane resin particles in the pretreatment liquid were replaced with acrylic resin particles. The acrylic resin particles used in the pretreatment liquid of Comparative Example 5 were prepared as follows: Distilled water (256.1 g), Olfine E1020 (0.9 g), sodium persulfate (NPS) (1.6 g), and sodium bicarbonate (0.6 g) were placed in a three-neck flask and heated to 85° C. under a nitrogen atmosphere. Solution 1 was prepared by mixing styrene (10.5 g), stearyl methacrylate (18.8 g), hydroxyethyl methacrylate (18.8 g), benzyl acrylate (24.8 g), and dodecanethiol (0.26 g). Solution 2 was prepared by mixing sodium styrene sulfonate (SSNa) (6.0 g) and distilled water (28.4 g). Solution 3 was prepared by mixing NPS (1.0 g), distilled water (24.0 g), and sodium bicarbonate (0.6 g). Solutions 1, 2, and 3 were each added dropwise to the three-neck flask over a period of 4 hours. After the addition, the mixture was stirred at 85°C for 2 hours, then allowed to cool to room temperature. The concentration was then adjusted with distilled water to obtain an aqueous dispersion of acrylic resin particles (solid content 20% by mass).
[0240]
[0241] As shown in Table 1, the dispersing group is —SO 3 - A pretreatment liquid containing a urethane resin containing a -SO group, 3 - The content of —SO groups is 2% by mass to 6% by mass, 3 - In each example in which a pretreatment liquid in which the group was bonded to the end of the main chain of the urethane resin was used, the pretreatment liquid had excellent storage stability, and the laminate had excellent boil resistance.
[0242] The results of the comparative examples for each example were as follows: 3 - In Comparative Example 1, in which a pretreatment liquid containing a urethane resin having a carboxy group instead of a -SO group was used, the storage stability of the pretreatment liquid was reduced. 3- In Comparative Example 2, where the content of -SO groups was less than 2 mass %, the storage stability of the pretreatment liquid was reduced. 3 - In Comparative Example 3, where the content of —SO groups was more than 6% by mass, the boil resistance of the laminate was reduced. 3 - In Comparative Example 4, which used a pretreatment liquid in which the group was bonded to a side chain of the urethane resin rather than to the end of the main chain, the storage stability of the pretreatment liquid was reduced. In Comparative Example 5, which used a pretreatment liquid containing an acrylic resin instead of a urethane resin, the boil resistance of the laminate was reduced.
[0243] The results of Examples 2 and 4 show that when the weight average molecular weight of the urethane resin in the pretreatment liquid is 5,000 or more (Example 2), the boil resistance of the laminate is further improved.
[0244] The results of Examples 2, 5, 11, and 12 show that when the glass transition temperature (Tg) of the urethane resin in the pretreatment liquid is −60° C. to 40° C. (Examples 2 and 11), the boil resistance of the laminate is further improved.
[0245] The results of Examples 13 and 14 show that the boil resistance of the laminate is further improved when the molar ratio [OH / NCO] (i.e., the molar ratio of polyol units to polyisocyanate units) is 0.5 or higher (Example 13). The results of Examples 2 and 6 show that the storage stability of the pretreatment liquid is further improved when the molar ratio [OH / NCO] is 0.9 or lower (Examples 2 and 13).
[0246] From the results of Examples 2 and 7, it is clear that the -SO 3 - It can be seen that when the pKa of the counter cation to the group is 10.0 or more (Example 2), the storage stability of the pretreatment liquid is further improved.
[0247] From the results of Examples 2 and 8, it is clear that the -SO 3 -It can be seen that when the counter cation to the group is an organic base cation (Example 2), the boil resistance of the laminate is further improved.
[0248] The results of Examples 2, 9, and 10 show that when the polyol units in the urethane resin in the pretreatment liquid contain polycarbonate diol units (Example 2), the boil resistance of the laminate is further improved.
[0249] Example 101 (Evaluation of Multi-Color Images) <Preparation of Colored Inks> Colored inks (specifically, cyan ink, magenta ink, yellow ink, and black ink) having the compositions shown in Table 2 were prepared.
[0250]
[0251] In Table 2, the numerical value of each component indicates its content (mass %) in the corresponding ink, and the "remaining amount," which is the amount of water, indicates the remaining amount to make the total 100 mass %. In Table 2, the details of the components after PG (1,2-propanediol) are the same as those of the white ink components described above.
[0252] APD4000C and the like in Table 2 are pigment dispersions, and the details are as follows: In Table 2, the amount of pigment dispersion indicates the solid content (total amount of pigment and pigment dispersant). APD4000C ... Projet Cyan APD4000 (manufactured by FUJIFILM Imaging Colorants, cyan pigment dispersion, pigment concentration: 20% by mass) APD4000M ... Projet Magenta APD4000 (manufactured by FUJIFILM Imaging Colorants, magenta pigment dispersion, pigment concentration: 20% by mass) APD1000R ... Projet Red APD1000 (manufactured by FUJIFILM Imaging Colorants, red pigment dispersion, pigment concentration: 16% by mass) APD4000Y ... Projet Yellow APD4000 (manufactured by FUJIFILM Imaging Colorants, yellow pigment dispersion, pigment concentration: 20% by mass) APD4000K ... Projet Black APD4000 (FUJIFILM Imaging Colorants, black pigment dispersion, pigment concentration: 15% by mass
[0253] <Image Recording> Image recording was performed using the pretreatment liquid in any one of Examples 1 to 21 and Comparative Examples 1 to 5, the white ink in Example 1, and the colored inks shown in Table 2 above (specifically, cyan ink, magenta ink, yellow ink, and black ink). Specifically, each of the following image recordings A to D was performed to obtain a solid image. In the following image recordings A to D, the pretreatment liquid application conditions, drying conditions after application of the pretreatment liquid, ink application conditions, and drying conditions after application of the ink were the same as those in the image recording of Example 1.
[0254] Image recording A: Image recording carried out in the order of applying a pretreatment liquid, drying, applying cyan ink, applying white ink, and drying. Image recording B: Image recording carried out in the order of applying a pretreatment liquid, drying, applying cyan ink, applying magenta ink, applying yellow ink, applying black ink, applying white ink, and drying. Image recording C: Image recording carried out in the order of applying a pretreatment liquid, drying, applying cyan ink, drying, applying white ink, and drying. Image recording D: Image recording carried out in the order of applying a pretreatment liquid, drying, applying cyan ink, applying magenta ink, applying yellow ink, applying black ink, drying, applying white ink, and drying.
[0255] Using each image recorded product obtained in image recording A to D, a laminate was produced and the boil resistance of the laminate was evaluated in the same manner as in Example 1. As a result, it was confirmed that when the pretreatment liquid in Examples 1 to 21 was used, the boil resistance of the laminate was excellent, similar to Examples 1 to 21 (i.e., image recording with a single color of white ink), regardless of whether image recording A to D was performed.
[0256] The disclosure of Japanese Patent Application No. 2023-050204, filed on March 27, 2023, is incorporated herein by reference in its entirety. All documents, patent applications, and technical standards mentioned herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard was specifically and individually indicated to be incorporated by reference.
Claims
1. A method for producing a polymerizable composition comprising: a flocculant which is at least one selected from the group consisting of an organic acid and a polyvalent metal compound; water; and a urethane resin, the urethane resin comprising a polyol unit, a polyisocyanate unit, and a -SO 3 - group relative to the total amount of the urethane resin, 3 - The content of the -SO group is 2% by mass to 6% by mass, 3 - a group is bonded to an end of a main chain of the urethane resin.
2. The ink-jet ink pretreatment liquid according to claim 1, wherein the urethane resin contains a partial structure represented by the following formula (I): In formula (I), * represents a bonding position; 1 is -NH- or -N(L 4 -Y 4 )-, L 4 represents a divalent group which is one type selected from the first group consisting of an alkylene group, an alkenylene group, an alkynylene group, an arylene group, -O-, -NH-, and -C(=O)-, a divalent group formed by bonding two or more types selected from the first group, or a single bond; 4 represents an alkyl group, an alkenyl group, an alkynyl group, an aryl group, a halogen atom, -OH, -OR 3 , -NH 2 , -NR 3 H, -NR 3 R 4 or -C(=O)R 3 represents 3 and R 4 each independently represents an alkyl group, an alkenyl group, an alkynyl group, or an aryl group; L 1 represents an alkylene group having 1 to 4 carbon atoms; Z + is -SO 3 - represents a counter cation for the group.
3. The ink-jet ink pretreatment liquid according to claim 1, wherein the urethane resin has a weight average molecular weight of 5,000 or more.
4. The ink-jet ink pretreatment liquid according to claim 1, wherein the urethane resin has a glass transition temperature of -60°C to 40°C.
5. The pretreatment liquid for ink-jet ink according to claim 1, wherein in the urethane resin, a molar ratio of the polyol unit to the polyisocyanate unit is 0.5 to 0.
9.
6. The urethane resin is 3 - The ink-jet ink pretreatment liquid according to claim 1 , further comprising a counter cation for the group, the counter cation having a pKa of 10.0 or more.
7. The urethane resin is 3 - The ink-jet ink pretreatment liquid according to claim 1 , further comprising a counter cation for the group, the counter cation being an organic base cation.
8. The inkjet ink pretreatment liquid according to claim 1, wherein the polyol unit comprises a polycarbonate diol unit.
9. An ink set comprising: the pretreatment liquid for ink-jet ink according to any one of claims 1 to 8; and an ink, which is an ink-jet ink containing water, a pigment, and a urethane resin.
10. An image recording method using the ink set according to claim 9, comprising: a step of applying the ink-jet ink pretreatment liquid onto a non-permeable substrate; and a step of applying the ink by an ink-jet recording method onto the non-permeable substrate to which the ink-jet ink pretreatment liquid has been applied.
11. A method for producing a laminated body, comprising: a step of obtaining an image recorded product comprising the non-permeable substrate and an image disposed on the non-permeable substrate by the image recording method according to claim 10; and a step of laminating a substrate to the side of the image recorded product on which the image is disposed, to obtain a laminated body.
12. A method for producing a printing medium comprising: a non-permeable substrate; and an image disposed on the non-permeable substrate, the image comprising: a pretreatment layer disposed on the non-permeable substrate, the pretreatment layer containing a flocculant, the flocculant being at least one selected from the group consisting of organic acids and polyvalent metal compounds, and a urethane resin; and an ink layer disposed on the pretreatment layer, the ink layer containing a pigment and a urethane resin, the urethane resin in the pretreatment layer being a polyol unit, a polyisocyanate unit, and -SO 3 - group relative to the total amount of the urethane resin, 3 - The content of the -SO group is 2% by mass to 6% by mass, 3 - a group is bonded to an end of a main chain of the urethane resin.
13. A laminate comprising: the image recorded matter according to claim 12; and a lamination substrate laminated onto the image of the image recorded matter.
Citation Information
Patent Citations
Recording method and device therefor
JP1979059936A
Coloring fine-particle dispersoid, ink-jet ink, and ink jet recording method
JP2001247787A
Photopolymerization composition, photopolymerizable color composition and color filter
JP2002012607A
Actinic energy ray-curable ink-jet ink
JP2002188025A
Recording liquid
JP2003026978A