Etching liquid for silicon nitrides, method for processing substrate and method for producing semiconductor element

A silicon nitride etching solution using non-fluorine boron compounds and acidic components effectively addresses the volatility and selectivity issues in existing solutions, ensuring stable and efficient etching of silicon nitride in semiconductor manufacturing.

WO2024204794A1PCT designated stage expired Publication Date: 2024-10-03TOKUYAMA CORP

Patent Information

Application Number
PCT/JP2024/013247
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-29
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing silicon nitride etching solutions, particularly those containing fluorine-bearing boron compounds, suffer from reduced etching performance over time due to volatility of hydrogen fluoride and equipment corrosion, making it difficult to selectively etch silicon nitride without damaging silicon oxide.

Method used

A silicon nitride etching solution comprising sulfuric acid or organic acids, a boron compound without fluorine, and water, with a pH of 5.0 or less when diluted, and a boron compound concentration between 0.10% and 30.0% by mass, which enhances etching selectivity and stability.

Benefits of technology

The solution efficiently and selectively etches silicon nitride relative to silicon and silicon oxide, maintaining etching performance over time and preventing equipment corrosion, thereby improving semiconductor manufacturing processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

Disclosed is an etching liquid for silicon nitrides, the etching liquid containing water, a boron compound, and one or more acids that are selected from the group consisting of sulfuric acid and organic acids, wherein: the boron compound does not contain a fluorine atom; the concentration of the boron compound is 0.10% by mass to 30.00% by mass (inclusive); and the pH as measured at 24°C after being diluted 10 times with water in terms of the mass ratio is 5.0 or less.
Need to check novelty before this filing date? Find Prior Art

Description

Silicon nitride etching solution, substrate processing method, and semiconductor device manufacturing method

[0001] The present invention relates to a silicon nitride etching solution, a substrate processing method, and a semiconductor device manufacturing method.

[0002] In recent years, silicon nitride has been used as a material for forming 3D-NAND flash memory and transistors with a structure known as GAA (Gate All Around). In the process of fabricating 3D-NAND flash memory, silicon nitride must be efficiently etched due to the structure in which silicon oxide and silicon nitride are alternately stacked. For this reason, an etching solution capable of efficiently etching silicon nitride is required. Furthermore, in the process of fabricating GAA-structure transistors, in the silicon nitride etching step, silicon oxide and other materials may come into contact with the etching solution at the same time as the material to be etched. In such cases, efficient etching of silicon nitride is required.

[0003] As an etching solution capable of selectively etching silicon nitride relative to silicon oxide, Patent Document 1 proposes an etching solution containing water, sulfuric acid, and a boron compound.

[0004] JP 2010-87154 A

[0005] The etching solution of Patent Document 1 can efficiently etch silicon nitride. However, all of the boron compounds in Patent Document 1 contain fluorine. Fluorine-containing boron compounds generate hydrogen fluoride upon hydrolysis. As a result, it is presumed that the etching solution of Patent Document 1 contains hydrogen fluoride. Furthermore, because the etching solution of Patent Document 1 is strongly acidic, it is presumed that hydrogen fluoride exists mainly as free hydrogen fluoride rather than as fluoride ions. Free hydrogen fluoride is characterized by its tendency to volatilize from the etching solution. Therefore, issues remain: etching performance deteriorates when the same etching solution is used for a long period of time; and materials that are corroded by hydrogen fluoride gas cannot be used for components of the etching equipment.

[0006] Therefore, an object of the present invention is to provide a silicon nitride etching solution capable of selectively and efficiently etching silicon nitride relative to silicon and silicon oxide films without using a fluorine-containing boron compound, a substrate processing method, and a semiconductor device manufacturing method.

[0007] The present inventors have conducted extensive research in view of the above-mentioned problems, and have found that silicon nitride can be efficiently etched by using an etching solution that contains one or more acids selected from the group consisting of sulfuric acid and organic acids, a fluorine-free boron compound, and water, and that has a pH within a predetermined range when diluted.

[0008] Item 1. A silicon nitride etching solution comprising one or more acids selected from the group consisting of sulfuric acid and organic acids, a boron compound, and water, wherein the boron compound is a boron compound containing no fluorine atoms, the concentration of the boron compound is 0.10% by mass or more and 30.00% by mass or less, and the pH measured at 24°C after a 10-fold mass dilution with water is 5.0 or less. Item 2. The silicon nitride etching solution according to Item 1, wherein the acid has a pKa at 25°C of -5 or more and 2 or less. Item 3. The silicon nitride etching solution according to Item 1 or 2, wherein at least one of the boiling point and decomposition temperature at 1 atmosphere of the acid is 150°C or more and 400°C or less. Item 4. The silicon nitride etching solution according to any one of Items 1 to 3, wherein the organic acid is one or more organic acids selected from sulfonic acid compounds and carboxylic acid compounds. Item 5. The silicon nitride etching solution according to any one of Items 1 to 4, wherein the total concentration of the acid is 60% by mass or more and 90% by mass or less. Item 6. The silicon nitride etching solution according to any one of Items 1 to 5, wherein the boron compound is one or more boron compounds selected from boric acid, boric acid anhydride, and boric acid polymers. Item 7. The silicon nitride etching solution according to any one of Items 1 to 6, further comprising one or more basic compounds selected from the group consisting of ammonia, amines, and tetraalkylammonium hydroxides. Item 8. The silicon nitride etching solution according to any one of Items 1 to 7, further comprising one or more silicon etching inhibitors selected from the group consisting of nonionic compounds, anionic compounds having a hydrophobic group, cationic compounds having a hydrophobic group, and amphoteric compounds having a hydrophobic group, wherein the concentrations of the compounds contained as the acid are all 10% by mass or more, and the concentrations of the compounds contained as the etching inhibitors are all less than 10% by mass. Item 9. The silicon nitride etching solution according to Item 8, wherein the etching inhibitor comprises one or more compounds selected from the group consisting of cationic compounds having a hydrophobic group and aromatic ring compounds having an electron-withdrawing group.Item 10. The silicon nitride etching solution according to Item 9, wherein the cationic compound is a cationic compound having two or more cationic sites in its structure. Item 11. The silicon nitride etching solution according to Item 9 or 10, wherein the aromatic ring compound having an electron-withdrawing group is an aromatic ring compound having one or more electron-withdrawing groups selected from the group consisting of a chloro group, a fluoro group, a trifluoromethyl group, a carboxyl group, and a nitro group. Item 12. The silicon nitride etching solution according to Item 11, wherein the aromatic ring compound having an electron-withdrawing group is an aromatic ring compound having two or more electron-withdrawing groups selected from the group consisting of a chloro group, a fluoro group, a trifluoromethyl group, a carboxyl group, and a nitro group. Item 13. A method for producing an etching solution, comprising a composition preparation step of preparing a composition containing one or more acids selected from the group consisting of sulfuric acid and organic acids, a boron compound not containing a fluorine atom, and water. Item 14. A method for treating a substrate containing silicon nitride, comprising an etching step of etching the silicon nitride using the silicon nitride etching solution according to any one of Items 1 to 12. Item 15. The method for treating a substrate according to Item 14, wherein the etching temperature in the etching step is 120 to 185°C. Item 16. The method for treating a substrate according to Item 14 or 15, wherein the substrate further contains at least one material selected from the group consisting of silicon and silicon oxide, and the etching step is a step of selectively etching silicon nitride with respect to at least one material selected from the group consisting of silicon and silicon oxide using the etching solution. Item 17. A method for manufacturing a semiconductor device using a substrate containing silicon nitride, comprising an etching step of etching silicon nitride using the silicon nitride etching solution according to any one of Items 1 to 12. Item 18. The method for manufacturing a semiconductor device according to Item 17, wherein the etching temperature in the etching step is 120 to 185°C.Item 19. The method for manufacturing a semiconductor device according to Item 17 or 18, wherein the substrate further contains at least one selected from the group consisting of silicon and silicon oxide, and the etching step is a step of selectively etching silicon nitride with respect to at least one selected from the group consisting of silicon and silicon oxide using the etching solution.

[0009] According to the present invention, it is possible to provide a silicon nitride etching solution that can selectively and efficiently etch silicon nitride relative to silicon and silicon oxide films without using a fluorine compound, and it is also possible to provide a substrate processing method and a semiconductor device manufacturing method by using the etching solution.

[0010] Although the present invention will be described in detail below with reference to the preferred embodiments, the present invention is not limited to these embodiments as long as they do not depart from the spirit of the present invention. Furthermore, the present invention can be implemented by modifying it as desired within the scope of the present invention.

[0011] In this specification, a numerical range expressed using "to" means a range that includes the numerical values ​​before and after "to" as the lower and upper limits, and "A to B" means a range that is greater than or equal to A and less than or equal to B. Furthermore, when a numerical range is described in stages, the upper and lower limits of each numerical range can be arbitrarily combined. Furthermore, in this specification, the expression "A or B" can be interpreted as "at least one selected from the group consisting of A and B." Furthermore, although multiple embodiments are described in this specification, various conditions in each embodiment may be mutually applied to the extent applicable. Furthermore, in this specification, the expression "etching selectivity of B to A" means "the ratio of the etching rate for removing B to the etching rate for removing A" (etching rate for removing B / etching rate for removing A). Furthermore, in this specification, "concentration" refers to the content of each component in a solution. Therefore, "concentration" can express not only the content of a solute in a solution but also the content of a solvent, such as water, in a solution.

[0012] 1. Etching Solution An etching solution according to one embodiment of the present invention is an etching solution for efficiently removing silicon nitride (SiN). Specifically, the etching solution for etching silicon nitride (also simply referred to as "etching solution" or "silicon nitride etching solution") contains one or more acids selected from the group consisting of sulfuric acid and organic acids (hereinafter also referred to as "specific acids"), a boron compound, and water, wherein the boron compound is a boron compound that does not contain fluorine atoms, the concentration of the boron compound is 0.10 mass% or more and 30.00 mass% or less, and the pH measured at 24°C after 10-fold dilution with water is 5.0 or less. Therefore, the etching solution can be used for etching silicon nitride in the manufacture of semiconductor devices, etc.

[0013] The etching solution disclosed in Patent Document 1 contains a fluorine-containing boron compound, and is therefore presumed to contain hydrogen fluoride produced by hydrolysis of the boron compound. In particular, because the etching solution of Patent Document 1 is strongly acidic, it is presumed that hydrogen fluoride exists primarily as easily volatile free hydrogen fluoride, rather than as fluoride ions. In contrast, the etching solution of the present embodiment uses a boron compound that does not contain fluorine atoms, and therefore does not produce easily volatile free hydrogen fluoride, thereby enabling efficient etching of silicon nitride. Furthermore, the etching solution of the present embodiment has a pH of 5.0 or less when diluted 10 times by mass and measured at 24°C. This makes it difficult for a drop in at least one of the boiling point and decomposition temperature (hereinafter also referred to as "boiling point, etc.") of the etching solution, which would occur due to an excessively high pH (i.e., an excessively low specific acid concentration), to occur. This makes it easier to control the temperature conditions during etching. Therefore, the etching solution of the present embodiment is particularly useful as an etching solution used, for example, when etching silicon nitride for microfabrication in the manufacture of semiconductor devices. The etching solution according to this embodiment contains silicon (Si) and silicon oxide (SiO 2) has a high etching selectivity of silicon nitride to at least one selected from the group consisting of silicon and silicon oxide. Therefore, it is particularly useful as an etching solution for etching silicon nitride from a substrate, etc., having at least one selected from the group consisting of silicon and silicon oxide, and silicon nitride. Furthermore, in the etching solution according to this embodiment, the etching selectivity of silicon nitride to silicon can be improved by using a boron compound that does not contain fluorine atoms, and further, the etching selectivity of silicon nitride to silicon oxide can be improved by setting the concentration of the boron compound that does not contain fluorine atoms within a predetermined range. In this specification, "efficient etching" means a high etching rate, unless otherwise specified.

[0014] [Fluorine Atom-Free Boron Compound] The etching solution contains a fluorine atom-free boron compound. By including a fluorine atom-free boron compound, the etching rate of silicon nitride can be increased.

[0015] The inventors speculate as follows about the reason for this. When an aqueous solution containing a specific acid is used as an etching solution, the inventors have confirmed from an Arrhenius plot of the etching rate of silicon nitride that the slope of the etching rate of silicon nitride with respect to increasing temperature (corresponding to activation energy) is smaller at etching temperatures higher than a specific temperature (e.g., 150°C in the case of a sulfuric acid aqueous solution with a concentration of 75% by mass) than at temperatures lower than the specific temperature. In other words, at temperatures higher than the specific temperature, the increase in the etching rate of silicon nitride with respect to increasing temperature tends to be smaller. This indicates that when an aqueous solution containing a specific acid is used as an etching solution, the rate-determining process of silicon nitride etching changes around the specific temperature.

[0016] Furthermore, the etching temperature (change point) at which the rate-determining process changes tends to shift to a lower temperature as the concentration of the specific acid in the aqueous solution increases. Based on these findings, it is believed that the rate-determining process at temperatures higher than the change point is a process in which an increase in water content contributes to an increase in the etching rate of silicon nitride. One of the processes in which an increase in water content is thought to contribute to an increase in the etching rate of silicon nitride is the dissolution of silicic acid compounds produced by the etching reaction. The inventors speculate that the rate-determining process at temperatures higher than the change point is the dissolution of the silicic acid compounds.

[0017] On the other hand, when an aqueous solution containing a fluorine-free boron compound was used as an etching solution, the slope of the silicon nitride etching rate (corresponding to the activation energy) with increasing temperature in an Arrhenius plot of the silicon nitride etching rate did not change between temperatures lower than the specific temperature and higher than the specific temperature. From this, the inventors speculate that the inclusion of a fluorine-free boron compound promotes the dissolution of the silicic acid compound produced by the etching reaction. The inventors speculate that the promotion of dissolution of the silicic acid compound is due to the fact that, while etching with a specific acid aqueous solution causes the silicic acid compound to oligomerize and become less soluble, or to recombine with silicon atoms on the silicon substrate surface and become less soluble, the inclusion of a fluorine-free boron compound causes the silicic acid compound to combine with the boron compound to form borosilicate, improving the solubility of the compound in water and suppressing the oligomerization of the silicic acid compound and its recombination with silicon atoms on the silicon substrate surface.

[0018] The boron compound does not contain fluorine atoms. When a fluorine compound is contained in an etching solution having a pH in the above-described range according to this embodiment, free hydrogen fluoride may be generated. As described above, free hydrogen fluoride is easily volatilized from the etching solution, which causes fluctuations in the etching characteristics of the etching solution. Furthermore, the presence of hydrogen fluoride in the etching solution not only increases the etching rate of silicon nitride, but also significantly increases the etching rate of silicon oxide, making it difficult to etch only silicon nitride. Furthermore, from the same perspective, the etching solution preferably does not contain a compound that generates hydrogen fluoride, and more preferably does not contain a compound that contains fluorine atoms.

[0019] The boron compound is a compound that contains boron (B) as a constituent element.The boron compound that does not contain fluorine atoms in the etching solution is not particularly limited, but from the viewpoint of bonding with silicate compound, it is preferably at least one or more compounds selected from the group consisting of boric acid compounds and boronic acid compounds, and examples thereof include boric acid, boric acid salts, boric acid anhydride (boron oxide), metaboric acid, perboric acid, hypoboric acid, and boric acid multimers, but from the viewpoint of stability, it is more preferably boric acid, boric acid salts, boric acid anhydride, and boric acid multimers, and even more preferably boric acid, boric acid anhydride, and boric acid multimers. Examples of boric acid compounds include one or more compounds selected from the group consisting of boric acid, borate salts, boric anhydride, and boric acid polymers; and borate esters such as trimethyl boric acid, triethyl boric acid, triisopropyl boric acid, tributyl boric acid, trihexyl boric acid, tri-o-toluyl boric acid, and trimethylboroxine. Examples of boronic acid compounds include one or more compounds selected from the group consisting of alkylboronic acids such as ethylboronic acid, propylboronic acid, propylboronic acid, butylboronic acid, isobutylboronic acid, pentylboronic acid, hexylboronic acid, heptylboronic acid, octylboronic acid, cyclopentylboronic acid, and cyclohexylboronic acid; and arylboronic acids such as phenylboronic acid, naphthaleneboronic acid, anthraceneboronic acid, and phenylenediboronic acid. The fluorine-free boron compound contained in the etching solution may be one type or two or more types.

[0020] Among these, one or more compounds selected from the group consisting of boric acid, boric acid salts, boric acid anhydride, and boric acid polymers are preferred in terms of the effect of suppressing the generation of by-products in the etching solution, and boric acid is more preferred in terms of ease of handling. Borates are salts of boric acid or boric acid polymers, and include metal salts such as sodium tetraborate or sodium perborate, or non-metal salts such as ammonium borate, with non-metal salts being preferred. The cation in the boric acid salt is preferably an ammonium ion. Therefore, specific examples of borates include various ammonium salts such as unsubstituted ammonium salts, primary ammonium salts, secondary ammonium salts, tertiary ammonium salts, and quaternary ammonium salts, and among these, unsubstituted ammonium salts are particularly preferred in terms of suppressing a decrease in the boiling point of the etching solution. Examples of the unsubstituted ammonium salt include ammonium pentaborate octahydrate.

[0021] The concentration (content) of the fluorine-free boron compound in the etching solution is not particularly limited as long as it is 0.10% by mass or more. A higher concentration of the boron compound improves the etching performance of the etching solution, which tends to increase the etching rate of silicon nitride and improve the productivity of semiconductor devices. Therefore, the concentration of the fluorine-free boron compound in the etching solution is preferably 0.20% by mass or more, more preferably 0.40% by mass or more, even more preferably 0.80% by mass or more, and particularly preferably 1.00% by mass or more. The upper limit of the concentration is not particularly limited, but may be 30.00% by mass or less, 20.00% by mass or less, 15.00% by mass or less, or 10.00% by mass or less, in terms of the solubility of the fluorine-free boron compound in water. That is, the concentration is preferably 0.10 mass % or more and 30.00 mass % or less, more preferably 0.10 mass % or more and 20.00 mass % or less, even more preferably 0.10 mass % or more and 15.00 mass % or less, still more preferably 0.40 mass % or more and 15.00 mass % or less, still more preferably 0.80 mass % or more and 15.00 mass % or less, and most preferably 0.80 mass % or more and 10.00 mass % or less. When the concentration of the boron compound not containing fluorine atoms is in the above range, silicon nitride can be etched at a sufficient etching rate.

[0022] [Specific Acid] The etching solution contains one or more acids (specific acids) selected from the group consisting of sulfuric acid and organic acids, and as the specific acid, an organic acid may be used alone, sulfuric acid may be used alone, or both may be used in combination. In addition, sulfuric acid and organic acid may be present in a free state in the etching solution, or may be present by forming a salt with a basic compound, but from the viewpoint of effectively increasing the boiling point, etc., they are preferably present in a free state.

[0023] Furthermore, from the viewpoint of being able to selectively etch silicon nitride relative to silicon and silicon oxide, organic acids are preferably used. The inventors speculate as follows about the reason why the effects of the present invention can be obtained when sulfuric acid and organic acids are used.

[0024] While the surface of hydrogen-terminated silicon is hydrophobic, the surfaces of hydroxyl-terminated silicon and silicon oxide formed during the silicon etching process are hydrophilic. Therefore, water readily approaches these surfaces, and etching due to a nucleophilic substitution reaction between silicon atoms and water readily proceeds. However, when an organic acid is included as the specific acid, a dehydration condensation reaction is presumably caused between the hydroxyl groups on the silicon or silicon oxide surface and the organic acid. In this case, the hydrophobic groups (also referred to as "hydrophobic groups") of the organic acid face outward (toward the liquid phase), making the silicon or silicon oxide surface hydrophobic. This makes it difficult for water to approach the silicon or silicon oxide surface, slowing down etching of the silicon or silicon oxide. Furthermore, when an etching inhibitor for silicon or silicon oxide is separately added, using an organic acid as the specific acid can make the substrate surface hydrophobic, thereby increasing the adsorption of the etching inhibitor. On the other hand, although hydroxyl-terminated silicon on a silicon nitride surface also undergoes a dehydration condensation reaction with an organic acid, the silicon nitride maintains its hydrophilicity due to the presence of nitrogen sites on the surface. That is, under strongly acidic conditions, the nitrogen sites are protonated and become cationic, resulting in high hydrophilicity, and it is presumed that the organic acid can maintain its hydrophilicity even when bonded to the silicon site. Furthermore, since the silicon atom density on the silicon nitride surface is lower than that on the silicon surface, the density of the bonded organic acid is also low, and steric hindrance is small, so it is presumed that the approach of nucleophiles such as water is not easily hindered. Therefore, when an organic acid is included as the specific acid, etching of silicon or silicon oxide is selectively suppressed relative to etching of silicon nitride, and silicon nitride can be selectively etched relative to silicon or silicon oxide.

[0025] Furthermore, when sulfuric acid is included as the specific acid, sulfuric acid is adsorbed onto the surface of silicon or silicon oxide, and the surface charge of each becomes negative. This makes it easier for aromatic ring compounds having electron-withdrawing groups, i.e., compounds having electron-deficient aromatic rings, and cationic compounds to be adsorbed, thereby enabling efficient suppression of etching.

[0026] Etching of silicon nitride proceeds by protonating the nitrogen sites of the silicon nitride, followed by nucleophilic attack by water or hydroxide ions on the silicon sites. Therefore, if the pH of the etching solution is too high (i.e., if the concentration of the specific acid is too low), the rate of protonation of the nitrogen sites significantly decreases, and the etching rate of silicon nitride tends to decrease. Furthermore, if the pH of the etching solution is too high (i.e., if the concentration of the specific acid is too low), the boiling point of the etching solution decreases, making it difficult to control the temperature conditions. Since silicon etching proceeds solely through nucleophilic attack by water or hydroxide ions, the etching rate tends to increase when the pH of the etching solution is high.

[0027] Therefore, the pH at 24°C of an etching solution diluted 10 times by mass with water is 5.0 or less (0.0 to 5.0). More preferably, the pH is greater than 0.0 and less than 4.0, even more preferably greater than 0.0 and less than 3.0, particularly preferably greater than 0.0 and less than 2.0, and even more preferably greater than 0.1 and less than 1.0. The pH refers to a value measured by the glass electrode method described below. The reason for diluting the etching solution 10 times is to avoid unstable pH measurement due to the high concentration of components other than water in the etching solution. Furthermore, the size of the object to be measured for the pH is not particularly limited. The entire amount of manufactured or sold etching solution may be diluted 10 times with water, or a portion of the etching solution (e.g., 10 g or 10% by mass of the etching solution) may be taken and diluted 10 times with water.

[0028] When the pH of the etching solution is within the above range, protonation of the nitrogen sites of silicon nitride proceeds sufficiently quickly, thereby enabling efficient etching of silicon nitride. Furthermore, in terms of adjusting the boiling point and pH of the etching solution, the total concentration of one or more acids selected from the group consisting of organic acids and sulfuric acid in the etching solution is preferably 60% by mass or more and 95% by mass or less, more preferably 60% by mass or more and 90% by mass or less, even more preferably 65% ​​by mass or more and 90% by mass or less, particularly preferably 70% by mass or more and 90% by mass or less, and even more preferably 70% by mass or more and 85% by mass or less.

[0029] The pKa of the specific acid is not particularly limited, but is preferably -5 or more and 2 or less at 25°C, more preferably -5 or more and 1 or less, even more preferably -5 or more and 0 or less, and particularly preferably -5 or more and -1 or less. If the pKa is equal to or greater than the lower limit of the above range, a decrease in the etching rate of silicon nitride due to polymerization of silicic acid, which is the product of etching of each silicon compound, can be suppressed. Furthermore, if the pKa is equal to or less than the upper limit of the above range, dehydration condensation with hydroxyl groups on hydroxyl-terminated silicon surfaces or silicon oxide surfaces is facilitated, thereby efficiently suppressing etching of silicon and silicon oxide. Note that a lower pKa of the specific acid is also preferable in that it can increase the boiling point of the etching solution at a lower specific acid concentration. Note that when the specific acid is a polyvalent acid, the specific acid will have multiple pKa levels, and it is preferable that the pKa of any of these levels satisfies the above range, and it is more preferable that the lowest pKa of these levels satisfies the above range.

[0030] The boiling point, etc., of the specific acid (NBP, boiling point at 1 atmosphere, etc.) is not particularly limited, but from the viewpoint of suppressing a change in the concentration of the specific acid due to volatilization of the specific acid even when the etching treatment is performed while heating the etching solution for a long period of time, it is preferably 150°C or higher, more preferably 200°C or higher, even more preferably 250°C or higher, and particularly preferably 300°C or higher. On the other hand, there is no need to set an upper limit for the boiling point, etc., and it may be 400°C or lower, or may be 350°C or lower. It is preferably 150°C or higher and 400°C or lower, more preferably 200°C or higher and 400°C or lower, even more preferably 250°C or higher and 400°C or lower, and particularly preferably 300°C or higher and 400°C or lower.

[0031] (Sulfuric acid) The etching solution may contain sulfuric acid as a specific acid. By including sulfuric acid, hydrogen ions are generated, which allows the pH of the etching solution to be adjusted. Furthermore, sulfuric acid has a very low pKa of -3 at 25°C, and has two hydroxyl groups, so it has a strong interaction with water. In other words, by including sulfuric acid, it is easy to suppress boiling of water, and it is easy to increase the boiling point of the etching solution.

[0032] Although the form of sulfuric acid is not particularly limited, as described below, since the etching solution preferably has a low metal concentration, it is preferable to use sulfuric acid with as few metal impurities and insoluble impurities as possible, and a commercially available product can be purified and used as necessary. In addition, a high-purity aqueous sulfuric acid solution generally available for use in the electronics industry can also be used, and in producing the etching solution, this solution can be mixed directly with water and other components.

[0033] (Organic Acid) The etching solution may contain an organic acid as a specific acid. As with sulfuric acid, the inclusion of an organic acid generates hydrogen ions, which allows the pH of the etching solution to be adjusted. In this specification, the organic acid does not include a boron compound.

[0034] The organic acid is not particularly limited, and examples thereof include butanoic acid, pentanoic acid, hexanoic acid, heptanoic acid, octanoic acid, isobutanoic acid, isopentanoic acid, isohexanoic acid, isoheptanoic acid, isooctanoic acid, 2-cyclobutylacetic acid, cyclopentanecarboxylic acid, cyclohexanecarboxylic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, tridecanedioic acid, methylsuccinic acid, tetramethylsuccinic acid, benzoic acid, nitrobenzoic acid, and dinitrobenzoic acid. Carboxylic acid compounds such as benzoic acid, chloronitrobenzoic acid, chlorodinitrobenzoic acid, phthalic acid, chlorophthalic acid, nitrophthalic acid, terephthalic acid, chloroterephthalic acid, or nitroterephthalic acid (the listed aromatic carboxylic acid compounds include their respective isomers); methanesulfonic acid, ethanesulfonic acid, propanesulfonic acid, butanesulfonic acid, pentanesulfonic acid, hexanesulfonic acid, heptanesulfonic acid, octane sulfonic acid, hydroxyethanesulfonic acid sulfonic acid compounds such as hydroxypropanesulfonic acid, hydroxybutanesulfonic acid, hydroxypentanesulfonic acid, hydroxyhexanesulfonic acid, hydroxyheptanesulfonic acid, hydroxyoctane sulfonic acid, aminoethanesulfonic acid, aminopropanesulfonic acid, aminobutanesulfonic acid, aminopentanesulfonic acid, aminohexanesulfonic acid, aminoheptanesulfonic acid, aminooctane sulfonic acid, benzenesulfonic acid, nitrobenzenesulfonic acid, dinitrobenzenesulfonic acid, or pyridinesulfonic acid (the aromatic sulfonic acid compounds listed include their respective isomers); or phosphorus compounds such as phosphonic acid compounds such as ethylphosphonic acid, propylphosphonic acid, butylphosphonic acid, pentylphosphonic acid, heptylphosphonic acid, octylphosphonic acid, isopropylphosphonic acid, isobutylphosphonic acid, isopentylphosphonic acid, isoheptylphosphonic acid, or isooctylphosphonic acid.

[0035] Among these, from the viewpoint of being able to efficiently etch silicon nitride, one or more organic acids selected from sulfonic acid compounds and carboxylic acid compounds are preferred, sulfonic acid compounds are more preferred, alkylsulfonic acids are even more preferred, and methanesulfonic acid is particularly preferred from the viewpoint of increasing the boiling point of the etching solution.

[0036] As with sulfuric acid, an etching solution containing an organic acid preferably has a low metal concentration, and therefore, it is preferable to use an organic acid with as few metal impurities and insoluble impurities as possible, and a commercially available product can be purified and used as needed.

[0037] [Water] The etching solution contains water. If water is not contained, the etching rate tends to decrease. Depending on the type and amount of other components, the concentration (content) of water in the etching solution is preferably 5.0 mass% or more and less than 40.0 mass%, more preferably 10.0 mass% or more and less than 40.0 mass%, even more preferably 10.0 mass% or more and less than 35.0 mass%, and particularly preferably 10.0 mass% or more and less than 30.0 mass%. Furthermore, for example, the remainder other than the specific acid and the fluorine-free boron compound contained in the etching solution may be water. Furthermore, when the etching solution contains components such as a silicon or silicon oxide etching inhibitor or a basic compound, the remainder other than the specific acid, the fluorine-free boron compound, and these components may be water.

[0038] The type of water is not particularly limited, but it is preferable to use high-purity water with few impurities. Water with few impurities can be easily produced and obtained as ultrapure water for semiconductor manufacturing. The amount of impurities in the etching solution can be evaluated by electrical resistivity. Specifically, the electrical resistivity is preferably 0.10 MΩ·cm or more, more preferably 15.00 MΩ·cm or more, and even more preferably 18.00 MΩ·cm or more. The upper limit is not particularly limited, but may be 18.25 MΩ·cm or less. That is, preferably, for example, 0.10 MΩ·cm or more to 18.25 MΩ·cm or less, 15.00 MΩ·cm or more to 18.25 MΩ·cm or less, or 18.00 MΩ·cm or more to 18.25 MΩ·cm or less. As described above, such water with few impurities can be easily produced and obtained as ultrapure water for semiconductor manufacturing. Furthermore, ultrapure water has significantly fewer impurities that do not affect (have little contribution to) the electrical resistivity, making it highly suitable as a raw material for etching solutions.

[0039] Furthermore, among the metals, it is preferable that any one metal selected from the group consisting of Fe, Cu, Mn, Cr, and Zn is present in a small amount, and the concentration of any one metal selected from this group in the water used as a raw material is preferably 0.01 ppt to 1.00 ppb, more preferably 0.01 ppt to 0.50 ppb, even more preferably 0.01 ppt to 0.20 ppb, and particularly preferably 0.01 ppt to 0.1 ppb, on a mass basis. In particular, it is preferable that this range is satisfied for all of the metals Fe, Cu, Mn, Cr, and Zn.

[0040] [Other Components] The etching solution may further contain components (other components) other than the above-described components, within the range in which the effects of the present invention can be obtained, examples of which are shown below.

[0041] (Basic Compound) The etching solution may or may not further contain a basic compound. By adding a basic compound, the pH of the etching solution can be increased. As described above, etching of silicon nitride proceeds by protonating the nitrogen sites of the silicon nitride, followed by nucleophilic attack of water or hydroxide ions on the silicon sites. Therefore, under conditions in which the nucleophilic reaction by hydroxide ions is rate-limiting in etching of silicon nitride, the etching rate of silicon nitride may be improved by adding a basic compound to the etching solution to increase the pH.

[0042] The basic compound is not particularly limited as long as it reacts with the specific acid to form a salt of the specific acid, but is preferably ammonia or an organic base, or a salt thereof, and more preferably one or more selected from the group consisting of ammonia, amine, and tetraalkylammonium hydroxide. The salt is preferably a salt of an acid having a pKa equal to or higher than the pKa of the specific acid with ammonia or an organic base. When the acid is a polyvalent acid, even if the first pKa is lower than the pKa of the specific acid, the second or third pKa may be equal to or higher than the pKa of the specific acid. Examples of organic bases include onium hydroxide and organic amines.

[0043] Examples of onium hydroxides include ammonium hydroxides such as primary ammonium hydroxide, secondary ammonium hydroxide, tertiary ammonium hydroxide, or quaternary ammonium hydroxide, phosphonium hydroxide, sulfonium hydroxide, iminium hydroxide containing a multiple bond, or diazenium hydroxide. Among these, ammonium hydroxide is preferred, and quaternary ammonium hydroxide is more preferred from the viewpoint of good stability against specific acids (particularly sulfuric acid) and the ability to enhance the stability of the etching solution over time.

[0044] As the quaternary ammonium hydroxide, for example, one or more selected from the group consisting of tetramethylammonium hydroxide, ethyltrimethylammonium hydroxide, propyltrimethylammonium hydroxide, butyltrimethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, trimethyl-2-hydroxyethylammonium hydroxide, dimethylbis(2-hydroxyethyl)ammonium hydroxide, methyltris(2-hydroxyethyl)ammonium hydroxide, phenyltrimethylammonium hydroxide, and benzyltrimethylammonium hydroxide can be used.

[0045] As the organic amine, one or more selected from the group consisting of primary amines, secondary amines, and tertiary amines can be used.

[0046] Examples of primary or secondary amines include ethylenediamine, 1,3-diaminopropane, 1,4-diaminobutane, 1,5-diaminopentane, 1,6-diaminohexane, 1,7-diaminoheptane, 1,8-diaminooctane, 1,1,3,3-tetramethylguanidine, diethylenetriamine, dipropylenetriamine, bis(hexamethylene)triamine, N,N,N-trimethyldiethylenetriamine, and N,N-bis(3-aminopropyl)ethylenediamine. One or more selected from the group consisting of amine, 2-(2-aminoethoxy)ethanol, 2-amino-2-methyl-1-propanol, 4-amino-1-butanol, 5-amino-1-pentanol, 6-amino-1-hexanol, N-(2-aminoethyl)propanolamine, N-(2-hydroxypropyl)ethylenediamine, azetidine, pyrrolidine, piperidine, hexamethyleneimine, pentamethyleneimine, and octamethyleneimine can be used.

[0047] Specific examples of tertiary amines include one or more selected from the group consisting of 2-(dimethylamino)ethanol, 3-(dimethylamino)-1-propanol, 4-dimethylamino-1-butanol, 2-(diethylamino)ethanol, triethylamine, methylpyrrolidine, methylpiperidine, 1,8-diazabicyclo[5.4.0]undec-7-ene, and 1,5-diazabicyclo[4.3.0]non-5-ene.

[0048] The organic amine is preferably at least one selected from the group consisting of ethylenediamine, 1,3-diaminopropane, 1,4-diaminobutane, 1,5-diaminopentane, 1,6-diaminohexane, 1,1,3,3-tetramethylguanidine, diethylenetriamine, dipropylenetriamine, bis(hexamethylene)triamine, 2-(2-aminoethoxy)ethanol, 2-amino-2-methyl-1-propanol, 4-amino-1-butanol, 5-amino-1-pentanol, 6-amino-1-hexanol, N-(2-aminoethyl)propanolamine, pyrrolidine, piperidine, hexamethyleneimine, and pentamethyleneimine. More preferred examples include one or more selected from the group consisting of ethylenediamine, 1,3-diaminopropane, 1,4-diaminobutane, 1,5-diaminopentane, 1,6-diaminohexane, 1,1,3,3-tetramethylguanidine, diethylenetriamine, dipropylenetriamine, bis(hexamethylene)triamine, 2-(2-aminoethoxy)ethanol, 2-amino-2-methyl-1-propanol, pyrrolidine, and piperidine.

[0049] Such basic compounds may be selected and used according to the target and purpose of etching, taking into account their known characteristics. As mentioned above, from the viewpoint of stability against specific acids, quaternary ammonium hydroxide is more preferable among the above. On the other hand, from the viewpoint of suppressing a decrease in the boiling point of the etching solution due to the addition of a basic compound, a compound having a small molar mass relative to the number of nitrogen atoms (molar mass / number of nitrogen atoms) is preferred. Specifically, ammonia or a polyamine compound is preferred. Examples of polyamine compounds include ethylenediamine, diaminopropane, diethylenetriamine, and dipropylenetriamine.

[0050] In the etching solution, one kind of basic compound may be used alone, or a plurality of different kinds may be used in combination.

[0051] Furthermore, as will be described later, since a low metal concentration is preferable in an etching solution, it is preferable to use a basic compound containing as few metal impurities and insoluble impurities as possible. If necessary, commercially available products can be purified by recrystallization, column purification, ion exchange purification, filtration, or the like before use. When using quaternary ammonium hydroxide as the basic compound, some types are manufactured and sold at extremely high purity for semiconductor manufacturing, and it is preferable to use such a compound. Note that high-purity quaternary ammonium hydroxides commonly sold for semiconductor manufacturing can be used as a solution such as an aqueous solution. When producing an etching solution, this solution can be directly mixed with water and other components.

[0052] The concentration of the basic compound in the etching solution is not particularly limited, but is preferably 0.05 molar equivalents or more relative to the specific acid in the etching solution. The greater the molar equivalent number relative to the specific acid in the etching solution, the higher the pH of the etching solution (i.e., the higher the hydroxide ion concentration), which tends to increase the etching rate of silicon nitride and improve the productivity of semiconductor devices. Therefore, the concentration of the basic compound relative to the specific acid in the etching solution is more preferably 0.05 molar equivalents or more, even more preferably 0.10 molar equivalents or more, and particularly preferably 0.25 molar equivalents or more. The upper limit is not particularly limited, but may be 1.50 molar equivalents or less, 1.00 molar equivalents or less, or 0.75 molar equivalents or less, in order to suppress a decrease in the boiling point of the etching solution due to the addition of the basic compound. That is, preferred ranges include, for example, 0.05 molar equivalents or more and 1.50 molar equivalents or less, 0.10 molar equivalents or more and 1.00 molar equivalents or less, 0.10 molar equivalents or more and 0.75 molar equivalents or less, and 0.25 molar equivalents or more and 0.75 molar equivalents or less. Note that the above ranges are ranges when the specific acid and the basic compound react in a 1:1 ratio, and when the specific acid and the basic compound react in a 2:1 ratio or a 3:1 ratio, the upper and lower limits of the concentration range of the basic compound are half or one-third, respectively. Specific examples of the range of the basic compound when the specific acid and the basic compound react in a 2:1 ratio include, for example, 0.025 molar equivalents or more and 0.750 molar equivalents or less, 0.050 molar equivalents or more and 0.500 molar equivalents or less, 0.050 molar equivalents or more and 0.375 molar equivalents or less, and 0.125 molar equivalents or more and 0.375 molar equivalents or less.

[0053] (Silicon or Silicon Oxide Etching Inhibitor) The etching solution may further contain a silicon or silicon oxide etching inhibitor (hereinafter also simply referred to as "etching inhibitor"). The inclusion of a silicon or silicon oxide etching inhibitor may inhibit the etching of silicon or silicon oxide, thereby further improving the etching selectivity of silicon nitride relative to silicon or silicon oxide. Even when a silicon or silicon oxide etching inhibitor is contained, the etching selectivity of silicon nitride relative to silicon or silicon oxide can be improved by adding a boron compound that does not contain fluorine atoms, as described above. That is, the effect of using a silicon or silicon oxide etching inhibitor on the reduction in etching selectivity of silicon nitride relative to silicon or silicon oxide can be reduced. Organic acids as specific acids are used in the hope of achieving an etching inhibitory effect on silicon or silicon oxide by bonding with hydroxyl groups on the surface of silicon or silicon oxide, while etching inhibitors are used in the hope of achieving an etching inhibitory effect on silicon or silicon oxide by adsorption to the surface of silicon or silicon oxide through hydrophobic and electrostatic interactions.

[0054] The silicon or silicon oxide etching inhibitor is not particularly limited as long as it is a compound that adsorbs to the surface of silicon or silicon oxide. Specific examples of the silicon or silicon oxide etching inhibitor include one or more selected from nonionic compounds, anionic compounds having a hydrophobic group, cationic compounds having a hydrophobic group, and amphoteric compounds having a hydrophobic group. Among these, anionic compounds having a hydrophobic group, cationic compounds having a hydrophobic group, and amphoteric compounds having a hydrophobic group are preferred from the viewpoint of good stability against specific acids (especially sulfuric acid) and improving the stability of the etching solution over time. In terms of adsorption to the surface of silicon or silicon oxide, anionic compounds having a hydrophobic group and cationic compounds having a hydrophobic group are more preferred. Here, the hydrophobic group refers to a functional group having a hydrocarbon chain such as an alkyl group or an aryl group.

[0055] The range of types of "anionic compounds" may overlap with the above-mentioned "specific acids." However, the specific acids serve as base components, while the anionic compounds serve as additives, i.e., auxiliary agents, and thus their respective roles are different. Therefore, they can be distinguished by their concentrations. Specifically, the concentrations of the compounds contained as specific acids are all 10% by mass or more, and the concentrations of the compounds contained as etching inhibitors are all less than 10% by mass. Note that, for example, some organic acids containing aromatic rings, such as nitrobenzoic acid, can be treated as the above-mentioned organic acids, but can also be treated as etching inhibitors, as described below. To distinguish between these, the concentrations of the compounds contained as specific acids and the compounds contained as etching inhibitors may be used, as described above, or the organic acids may be limited to "organic acids not containing aromatic rings." In this case, for example, if an etching solution contains 60% by mass of methanesulfonic acid and 5% by mass of hexanesulfonic acid, methanesulfonic acid is treated as the specific acid, and hexanesulfonic acid is treated as the etching inhibitor. Furthermore, if an etching solution contains 60% by mass of sulfuric acid and 5% by mass of methanesulfonic acid, sulfuric acid is treated as a specific acid and methanesulfonic acid is treated as an etching inhibitor. In this specification, the expressions "any" and "any" are used not only when referring to multiple entities but also when referring to a single entity. Specifically, when the expression "the concentrations of all compounds contained as A are 10% by mass or less" is used, if there are two or more compounds contained as A, it means that the concentrations of each of the two or more compounds are 10% by mass or less. When there is one or more compounds contained as A, it means that the concentration of that one compound is 10% by mass or less. When the expression "the concentration of any of the compounds contained as A is 10% by mass or less" is used, if there are two or more compounds contained as A, it means that the concentration of any one of the two or more compounds is 10% by mass or less. When there is one or more compounds contained as A, it means that the concentration of that one compound is 10% by mass or less.

[0056] Examples of anionic compounds having a hydrophobic group include carboxylic acid compounds such as butanoic acid, pentanoic acid, hexanoic acid, heptanoic acid, octanoic acid, isobutanoic acid, isopentanoic acid, isohexanoic acid, isoheptanoic acid, isooctanoic acid, 2-cyclobutylacetic acid, cyclopentanecarboxylic acid, cyclohexanecarboxylic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, tridecanedioic acid, methylsuccinic acid, tetramethylsuccinic acid, benzoic acid, nitrobenzoic acid, dinitrobenzoic acid, chloronitrobenzoic acid, chlorodinitrobenzoic acid, phthalic acid, chlorophthalic acid, nitrophthalic acid, terephthalic acid, chloroterephthalic acid, and nitroterephthalic acid (the listed aromatic carboxylic acid compounds include their respective isomers); sulfonic acid compounds such as methanesulfonic acid, ethanesulfonic acid, propanesulfonic acid, butanesulfonic acid, pentanesulfonic acid, hexanesulfonic acid, heptanesulfonic acid, octane sulfonic acid, hydroxyethanesulfonic acid, hydroxypropanesulfonic acid, hydroxybutanesulfonic acid, hydroxypentanesulfonic acid, hydroxyhexanesulfonic acid, hydroxyheptanesulfonic acid, hydroxyoctane sulfonic acid, aminoethanesulfonic acid, aminopropanesulfonic acid, aminobutanesulfonic acid, aminopentanesulfonic acid, aminohexanesulfonic acid, aminoheptanesulfonic acid, aminooctane sulfonic acid, toluenesulfonic acid, aminobenzenesulfonic acid, benzenesulfonic acid, nitrobenzenesulfonic acid, dinitrobenzenesulfonic acid, or pyridinesulfonic acid (the aromatic sulfonic acid compounds listed include their respective isomeric compounds); or Examples thereof include phosphorus compounds such as phosphonic acid compounds such as ethylphosphonic acid, propylphosphonic acid, butylphosphonic acid, pentylphosphonic acid, heptylphosphonic acid, octylphosphonic acid, isopropylphosphonic acid, isobutylphosphonic acid, isopentylphosphonic acid, isoheptylphosphonic acid, and isooctylphosphonic acid.

[0057] Examples of nonionic compounds include glycols such as ethylene glycol, propylene glycol, and dipropylene glycol, and polyol compounds having multiple hydroxyl groups such as glycerin; glycol ether compounds such as alkylene glycol monoalkyl esters such as ethylene glycol monopropyl ether, ethylene glycol monomethyl ether, diethylene glycol monoethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, and diethylene glycol n-butyl ether, and alkylene glycol dialkyl esters such as diethylene glycol dimethyl ether, diethylene glycol methyl ethyl ether, and diethylene glycol diethyl ether; and aromatic ring compounds such as chlorobenzene, dichlorobenzene, trichlorobenzene, fluorobenzene, difluorobenzene, trifluorobenzene, trifluoromethylbenzene, chlorotrifluoromethylbenzene, nitrobenzene, dinitrobenzene, chloronitrobenzene, chlorodinitrobenzene, nitropyridine, and hydroxynitropyridine (the listed aromatic compounds include their respective isomers).

[0058] Examples of cationic compounds having a hydrophobic group include tetramethylammonium chloride, tetramethylammonium bromide, tetraethylammonium chloride, tetraethylammonium bromide, tetrapropylammonium chloride, tetrapropylammonium bromide, tetrabutylammonium chloride, tetrabutylammonium bromide, dodecyltrimethylammonium chloride, dodecyltrimethylammonium bromide, decyltrimethylammonium chloride, and decyltrimethylammonium bromide. Examples of suitable quaternary ammonium salts include halogen salts of quaternary ammonium, sulfate salts of quaternary ammonium, and hydrogen sulfate salts of quaternary ammonium, such as quaternary ammonium bromide, decamethonium dichloride, decamethonium dibromide, hexamethonium dichloride, hexamethonium dibromide, 1,1'-(decane-1,10-diyl)bis[4-aza-1-azoniabicyclo[2.2.2]octane]dibromide, and 1,1'-(decane-1,10-diyl)bis[4-aza-1-azoniabicyclo[2.2.2]octane]dichloride. The sulfate salts of quaternary ammonium may be produced by reacting quaternary ammonium hydroxide with sulfuric acid, and then incorporated into the etching solution. As mentioned above, sulfuric acid is considered a specific acid when it is present in the etching solution at 10% by mass or more.

[0059] The cationic compound is preferably a cationic compound having two or more cationic sites in its structure from the viewpoint of increasing the adsorptive power (increasing the adsorption probability and decreasing the desorption probability). Examples include decamethonium dichloride, decamethonium dibromide, hexamethonium dichloride, hexamethonium dibromide, 1,1'-(decane-1,10-diyl)bis[4-aza-1-azoniabicyclo[2.2.2]octane]dibromide, and 1,1'-(decane-1,10-diyl)bis[4-aza-1-azoniabicyclo[2.2.2]octane]dichloride. Among these, cationic compounds in which the number of carbon atoms in the alkyl chain between the two cationic sites is 8 or less are more preferred in terms of stability at high temperatures and against sulfuric acid. Specific examples include hexamethonium dichloride and hexamethonium dibromide.

[0060] Examples of amphoteric compounds having a hydrophobic group include amino acid compounds such as methylglycine, ethylglycine, alanine, β-alanine, leucine, isoleucine, proline, hydroxyproline, N-methylproline, α-methylproline, and tyrosine.

[0061] The etching inhibitor for silicon or silicon oxide can be one or more compounds selected from the group consisting of the compounds listed above.

[0062] From the viewpoint described below, the etching solution preferably contains, as an etching inhibitor, one or more compounds selected from the group consisting of cationic compounds having hydrophobic groups and aromatic ring compounds having electron-withdrawing groups. Among the compounds listed above, compounds that adsorb to the substrate surface due to either or both of hydrophobic and electrostatic interactions can be preferably used. Because the surface of hydrogen-terminated silicon is hydrophobic and the surface of silicon nitride is hydrophilic, using a compound that adsorbs to the substrate surface due to hydrophobic interactions as an etching inhibitor can selectively suppress etching of silicon relative to etching of silicon nitride. In particular, when an organic acid is used as the specific acid, the silicon surface and silicon oxide surface to which the organic acid is bonded are hydrophobic. Therefore, using a compound that adsorbs to the substrate surface due to hydrophobic interactions as an etching inhibitor can efficiently suppress etching of silicon or silicon oxide. Furthermore, particularly when sulfuric acid is used as the specific acid, the surface charge of the silicon or silicon oxide surface is negatively charged, and therefore aromatic ring compounds having electron-withdrawing groups, i.e., compounds having electron-deficient aromatic rings, and cationic compounds are easily adsorbed, thereby efficiently suppressing etching. On the other hand, since the silicon nitride surface is positively charged due to the protonation of the nitrogen sites and is hydrophilic, aromatic ring compounds having electron-withdrawing groups, i.e., compounds having an electron-deficient aromatic ring, cationic compounds, and compounds that adsorb to the substrate surface due to hydrophobic interactions are unlikely to be adsorbed to the silicon nitride surface. When the etching solution contains a high concentration of sulfuric acid, it is preferable to use a compound that is highly stable against sulfuric acid as the etching inhibitor.

[0063] As the cationic compound, the above-mentioned cationic compounds having a hydrophobic group can be used.

[0064] Furthermore, the aromatic ring compound having an electron-withdrawing group is preferably an aromatic ring compound having one or more electron-withdrawing groups selected from the group consisting of an amino group (under acidic conditions), a chloro group, a fluoro group, a trifluoromethyl group, a carboxyl group, and a nitro group. The aromatic ring in the aromatic ring compound having an electron-withdrawing group is not particularly limited as long as it has aromaticity, and may be a benzene-based aromatic ring or a non-benzene-based aromatic ring such as a heteroaromatic ring. Among these, a benzene-based aromatic ring is preferred because of its high stability against high-temperature sulfuric acid, and a benzene ring is more preferred because the aromatic ring can be easily made electron-deficient by introducing an electron-withdrawing group. Specific examples of aromatic ring compounds having a preferred electron-withdrawing group include aromatic ring compounds such as chlorobenzene, dichlorobenzene, trichlorobenzene, fluorobenzene, difluorobenzene, trifluorobenzene, trifluoromethylbenzene, chlorotrifluoromethylbenzene, nitrobenzene, dinitrobenzene, chloronitrobenzene, chlorodinitrobenzene, nitropyridine, hydroxynitropyridine, and N8,N8,3-trimethyl-2,8-phenazinediamine, which are listed as examples of compounds included in the nonionic compounds described above (the listed aromatic compounds include their respective isomeric compounds). Among these, the aromatic ring compound having an electron-withdrawing group is more preferably an aromatic ring compound having two or more electron-withdrawing groups selected from the group consisting of a chloro group, a fluoro group, a trifluoromethyl group, a carboxyl group, and a nitro group. Specific examples include aromatic ring compounds such as chlorodinitrobenzoic acid, chloronitrobenzoic acid, dinitrobenzoic acid, trichlorobenzoic acid, trinitrobenzoic acid, and chlorodifluorobenzoic acid (the listed aromatic compounds include their respective isomers). Here, the term "aromatic ring compound having two or more electron-withdrawing groups" refers to an aromatic ring compound in which the electron-withdrawing groups substituted on the aromatic ring compound may be the same or different, and two or more of the electron-withdrawing groups are substituted. Among these, aromatic ring compounds having two or more nitro groups are more preferred in terms of stability against high temperatures and sulfuric acid.Specific examples include trinitrobenzoic acid, chlorodinitrobenzoic acid, and dinitrobenzoic acid (the aromatic compounds listed include their respective isomers).

[0065] The compound adsorbed to the substrate surface by hydrophobic interaction is not particularly limited as long as it has a hydrophobic group. Specific examples of compounds highly stable against specific acids include carboxylic acid compounds such as butanoic acid, pentanoic acid, hexanoic acid, heptanoic acid, octanoic acid, isobutanoic acid, isopentanoic acid, isohexanoic acid, isoheptanoic acid, isooctanoic acid, 2-cyclobutylacetic acid, cyclopentanecarboxylic acid, cyclohexanecarboxylic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, tridecanedioic acid, methylsuccinic acid, tetramethylsuccinic acid, methylglycine, ethylglycine, alanine, β-alanine, leucine, isoleucine, proline, hydroxyproline, N-methylproline, α-methylproline, and tyrosine; and sulfonic acid compounds such as ethanesulfonic acid, propanesulfonic acid, butanesulfonic acid, pentanesulfonic acid, hexanesulfonic acid, heptanesulfonic acid, octane sulfonic acid, hydroxyethanesulfonic acid, hydroxypropanesulfonic acid, hydroxybutanesulfonic acid, hydroxypentanesulfonic acid, hydroxyhexanesulfonic acid, hydroxyheptanesulfonic acid, hydroxyoctane sulfonic acid, aminoethanesulfonic acid, aminopropanesulfonic acid, aminobutanesulfonic acid, aminopentanesulfonic acid, aminohexanesulfonic acid, aminoheptanesulfonic acid, and aminooctane sulfonic acid.

[0066] Examples of compounds that are adsorbed to the substrate surface by the effects of both hydrophobic and electrostatic interactions include aromatic ring compounds having an electron-withdrawing group, such as nitrobenzene, dinitrobenzene, chloronitrobenzene, chlorodinitrobenzene, benzenesulfonic acid, nitrobenzenesulfonic acid, dinitrobenzenesulfonic acid, nitropyridine, hydroxynitropyridine, pyridinesulfonic acid, benzoic acid, nitrobenzoic acid, dinitrobenzoic acid, chloronitrobenzoic acid, chlorodinitrobenzoic acid, phthalic acid, chlorophthalic acid, nitrophthalic acid, terephthalic acid, chloroterephthalic acid, nitroterephthalic acid, or aromatic compounds such as N8,N8,3-trimethyl-2,8-phenazinediamine (the listed compounds include their respective isomers); or tetramethylammonium chloride, tetramethylammonium bromide, tetraethylammonium chloride, tetraethylammonium bromide, and the like. Examples of the quaternary ammonium halide salts include quaternary ammonium sulfates and quaternary ammonium hydrogen sulfate salts, such as tetrapropylammonium chloride, tetrapropylammonium bromide, tetrabutylammonium chloride, tetrabutylammonium bromide, dodecyltrimethylammonium chloride, dodecyltrimethylammonium bromide, decyltrimethylammonium chloride, decyltrimethylammonium bromide, decamethonium chloride, decamethonium bromide, hexamethonium chloride, hexamethonium bromide, 1,1'-(decane-1,10-diyl)bis[4-aza-1-azoniabicyclo[2.2.2]octane]dibromide, and 1,1'-(decane-1,10-diyl)bis[4-aza-1-azoniabicyclo[2.2.2]octane]dichloride.

[0067] The total concentration of the etching inhibitor in the etching solution is not particularly limited, but may be, for example, 0.001% by mass or more and 20.000% by mass or less, preferably 0.005% by mass or more and 15.000% by mass or less, more preferably 0.005% by mass or more and less than 10.000% by mass, even more preferably 0.010% by mass or more and less than 10.000% by mass, particularly preferably 0.010% by mass or more and less than 7.500% by mass, and even more particularly preferably 0.020% by mass or more and less than 7.500% by mass. Furthermore, the concentration of each compound contained in the etching solution as an etching inhibitor is less than 10% by mass, and may be 0.001% by mass or more but less than 10% by mass, preferably 0.005% by mass or more but less than 10.000% by mass, more preferably 0.010% by mass or more but less than 7.500% by mass, even more preferably 0.020% by mass or more but less than 7.500% by mass, and particularly preferably 0.020% by mass or more but less than 5.000% by mass. If the total concentration of the etching inhibitor and the concentration of each compound are equal to or greater than the lower limit of the above range, a sufficient effect of inhibiting the etching of silicon or silicon oxide can be obtained. Furthermore, if these concentrations are equal to or less than the upper limit of the above range, a sufficient specific acid concentration and water content can be ensured, and thus a sufficient etching rate of silicon nitride can be ensured.

[0068] The etching solution is preferably a homogeneous solution in which all of the components are dissolved. Furthermore, in order to prevent contamination during etching, the number of particles of 200 nm or larger in the etching solution is preferably 100 particles / mL or less, more preferably 50 particles / mL or less. The lower limit is not particularly limited, but may be 0 particles / mL or more. This amount may be, for example, preferably 0 particles / mL or more and 100 particles / mL or less, or 0 particles / mL or more and 50 particles / mL or less. Furthermore, the etching solution may contain a gas such as hydrogen or oxygen for reasons of manufacturing the etching solution.

[0069] In etching using an etching solution, if the etching solution contains metal, it will affect the object to be treated (not limited to the silicon surface to be etched), often resulting in a decrease in the quality of the final product.

[0070] Therefore, it is preferable that no metal is intentionally added to the etching solution, and it is more preferable that the metal concentration in the etching solution is below the impurity level, and it is even more preferable that the etching solution is substantially free of metal (below the detection limit). However, the etching solution may contain metal. The metal here includes non-ionic metals (particulate metals) such as elemental metals and metal ions (ionic metals). For example, the total concentration of metals in the etching solution is preferably 1 ppm or less by mass, and more preferably 1 ppb or less. The lower limit is not particularly limited, and the total concentration of metals may be, for example, 0 ppm or more and 1 ppm or less, 0 ppb or more and 1 ppb or less, or more than 0 ppm and 1 ppm or less, or more than 0 ppb and 1 ppb or less. More specifically, the concentrations of Ag, Al, Ba, Ca, Cd, Co, Cr, Cu, Fe, K, Li, Mg, Mn, Na, Ni, Pb, and Zn in the etching solution are preferably 1 ppm or less by mass, and more preferably 1 ppb or less. The lower limit is not particularly limited, and the concentrations of the above metals may be, for example, 0 ppm to 1 ppm, 0 ppb to 1 ppb, or more than 0 ppm to 1 ppm, or more than 0 ppb to 1 ppb by mass. The metals listed here are metals that are considered to affect the quality of chemicals used in semiconductor manufacturing. In other words, the quality of the etching solution can be improved by having the concentrations of the metals within the above ranges.

[0071] The etching solution according to this embodiment can be suitably used as an etching solution in the manufacture of semiconductor devices, which includes an etching step of etching silicon nitride, such as a silicon nitride single crystal film. The silicon nitride single crystal film includes those produced by epitaxial growth.

[0072] 2. Method for Producing Etching Solution The method for producing the etching solution is not particularly limited, and may be, for example, a method including a composition preparation step of preparing a composition containing a specific acid, a boron compound not containing a fluorine atom, and water. Furthermore, these steps may be combined into one step.

[0073] The method for preparing the composition is not particularly limited, and examples thereof include a method in which the specific acid, the fluorine-free boron compound, water, and other optional components are mixed together, and the specific acid, the fluorine-free boron compound, and other optional components are dissolved in water. In the dissolution, it is preferable that each component is dissolved uniformly.

[0074] The method for producing an etching solution may also include an aging step in which a composition containing a specific acid, a boron compound containing no fluorine atoms, and water is heated. The heating temperature in the aging step is preferably equal to or higher than the temperature in the etching step, and the upper limit of the heating temperature may be appropriately determined taking into account the heat resistance temperature of the components of the equipment used in the aging step. That is, the heating temperature is preferably in the range of 100°C to 200°C, more preferably in the range of 120°C to 200°C, even more preferably in the range of 165°C to 200°C, and particularly preferably in the range of 180°C to 200°C. The heating time in the aging step varies depending on the heating temperature, so it is not possible to determine an optimal range. However, considering productivity, the heating time is preferably in the range of 1 to 100 hours, more preferably in the range of 3 to 100 hours, even more preferably in the range of 5 to 100 hours, and particularly preferably in the range of 10 to 100 hours. The heating in the aging step may be performed intermittently by repeating heating and cooling. When heating in the aging step is performed intermittently, the heating time is the total time maintained at the heating temperature.

[0075] As raw materials for the etching solution, such as the specific acid, the boron compound not containing fluorine atoms, and water, those described in the section on etching solution can be used.

[0076] The production of the etching solution preferably includes a step of mixing and dissolving the raw materials, and then passing the mixture through a filter with a size of several nanometers to several tens of nanometers to remove particles. If necessary, the step of removing particles may be carried out multiple times.

[0077] Furthermore, various known treatments that are carried out to obtain necessary physical properties in the production of chemicals for semiconductor manufacturing, such as reducing dissolved oxygen in the etching solution by bubbling with an inert gas such as high-purity nitrogen gas, can be carried out.

[0078] In the mixing and dissolving steps, and also for storing the etching solution, it is preferable to use a container or device formed of or coated with a material known as an inner wall material for semiconductor manufacturing chemicals, specifically a material that does not easily leach contaminants into the etching solution, such as polyfluoroethylene or high-purity polypropylene. It is also preferable to clean these containers or devices in advance.

[0079] 3. Method for Manufacturing a Semiconductor Element A second embodiment of the present invention relates to a method for manufacturing a semiconductor element using a substrate containing silicon nitride, which includes an etching step of etching the silicon nitride using the etching solution of the first embodiment (also simply referred to as a "method for manufacturing a semiconductor element").

[0080] Since the etching solution of the first embodiment can selectively etch silicon nitride relative to at least one selected from the group consisting of silicon and silicon oxide, the method for manufacturing a semiconductor device described above may be a method for manufacturing a semiconductor device using a substrate containing at least one selected from the group consisting of silicon and silicon oxide and silicon nitride, and may include an etching step of selectively etching silicon nitride relative to at least one selected from the group consisting of silicon and silicon oxide using the etching solution of the first embodiment. In the following description, an example of each condition of the embodiment will be described, but the present invention is not limited to this condition.

[0081] The method for manufacturing a semiconductor device can be a known method for manufacturing a semiconductor device, except that it includes an etching step of selectively etching silicon nitride with respect to at least one selected from the group consisting of silicon and silicon oxide using the etching solution of the first embodiment. For example, the method may include one or more steps selected from the group consisting of a wafer fabrication step, an oxide film formation step, a transistor formation step, a wiring formation step, and a CMP step, and may also include other known steps used in semiconductor manufacturing methods.

[0082] The etching step of selectively etching silicon nitride with respect to at least one selected from the group consisting of silicon and silicon oxide using the etching solution of the first embodiment is not particularly limited, and examples thereof include a contacting step of bringing the etching solution into contact with a substrate containing at least one selected from the group consisting of silicon and silicon oxide and silicon nitride. By including such a step, it is possible to selectively remove silicon nitride from a device structure in which silicon oxide is used as an insulating film, silicon and silicon-germanium are alternately stacked, and silicon nitride is stacked thereon as a hard mask, by bringing the etching solution into contact with the device structure.

[0083] Furthermore, the etching process is not particularly limited as long as it can selectively etch silicon nitride with respect to at least one species selected from the group consisting of silicon and silicon oxide, and may be a process including a substrate holding process for holding a substrate in a horizontal position and a processing liquid supply process for supplying an etching liquid to a main surface of the substrate while rotating the substrate about a vertical axis of rotation passing through the center of the substrate, or a process including a substrate holding process for holding a plurality of substrates in an upright position and a process for immersing the substrates in an upright position in an etching liquid stored in a processing tank.

[0084] The conditions for the etching step are not particularly limited, and for example, the temperature of the etching solution in the etching step may be appropriately determined taking into consideration the desired etching rate, the shape and surface state of the silicon nitride after etching, productivity, the heat resistance temperature of the components of the etching device, etc. For example, the temperature may be 20 to 200°C, preferably in the range of 50 to 190°C, more preferably in the range of 100 to 190°C, even more preferably in the range of 120 to 185°C, and particularly preferably in the range of 165 to 185°C.

[0085] The etching process can also be performed while degassing under vacuum or reduced pressure or bubbling with an inert gas. Such operations can prevent or reduce the increase in dissolved oxygen during etching. Alternatively, the etching process can be performed without bubbling with an inert gas. By omitting bubbling with an inert gas, the dissolved oxygen in the etching solution increases. When the substrate contains silicon, the dissolved oxygen in the etching solution contributes to the oxidation of silicon, which can decrease the silicon etching rate, but can also increase it. Therefore, when the silicon etching rate increases due to the influence of dissolved oxygen, i.e., when the etching rate of silicon nitride relative to silicon may decrease, bubbling with an inert gas can be performed. However, when the silicon etching rate is maintained or decreased due to the influence of dissolved oxygen, bubbling with an inert gas can be omitted.

[0086] In the etching step, the substrate may be simply brought into contact with the etching solution by immersing the substrate in the etching solution, or an electrochemical etching method in which a constant potential is applied to the substrate may also be employed.

[0087] As described above, the etching target in the etching process is a substrate containing at least one selected from the group consisting of silicon and silicon oxide, and silicon nitride. Here, the at least one selected from the group consisting of silicon and silicon oxide is a non-etching target that is not the target of the etching process. The silicon, silicon oxide, and silicon nitride may be, for example, a silicon film, a silicon oxide film, or a silicon nitride film, or a silicon nitride single crystal film containing silicon as a substrate. The thickness of the silicon film or the like is not particularly limited and can be appropriately set depending on the application. The substrate may also contain various metal films or the like as non-etching targets. Examples include structures in which silicon and silicon-germanium are alternately stacked, silicon-germanium films, silicon oxide films, or silicon nitride films are formed on single crystal silicon, and silicon or polysilicon and silicon-germanium films are formed thereon, as well as structures patterned using these films.

[0088] 4. Substrate Processing Method A third embodiment of the present invention relates to a substrate processing method including an etching step of etching the silicon nitride using the etching solution of the first embodiment. Note that the third embodiment may include steps other than the etching step described above, as long as the effects of the present invention can be obtained.

[0089] Since the etching solution of the first embodiment can selectively etch silicon nitride relative to at least one selected from the group consisting of silicon and silicon oxide, the substrate processing method may be a substrate processing method containing at least one selected from the group consisting of silicon and silicon oxide and silicon nitride, comprising an etching step of selectively etching silicon nitride relative to at least one selected from the group consisting of silicon and silicon oxide using the etching solution of the first embodiment. In the following description, an example of each condition of the embodiment will be described, but the present invention is not limited to this condition.

[0090] The etching step of selectively etching silicon nitride over at least one selected from the group consisting of silicon and silicon oxide using an etching solution can be the etching step described in the section on the method for manufacturing a semiconductor device. The etching step can also be, for example, a step including a substrate holding process for holding a substrate in a horizontal position and a processing solution supply process for supplying an etching solution to a main surface of the substrate while rotating the substrate about a vertical axis of rotation passing through the center of the substrate, or a step including a substrate holding process for holding a plurality of substrates in an upright position and a process for immersing the substrates in an upright position in the etching solution of the first embodiment stored in a processing tank. Furthermore, the substrate can be any of the substrates described in the section on the method for manufacturing a semiconductor device.

[0091] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0092] <Ultrapure water> The ultrapure water used for diluting the etching solution in measuring the pH of the etching solution and for producing the etching solution was produced by purifying water using a Millipore pure water production system, Elix Essential UV5, and then further purifying it using a Millipore ultrapure water production system, Milli-Q Advantage. <Evaluation of etching solution> The etching solutions in the examples and comparative examples were evaluated as follows.

[0093] [Method for measuring pH of etching solution (10-fold diluted)] First, the etching solution was diluted 10 times by mass with ultrapure water. The pH of the diluted etching solution was measured at a temperature of 24°C using a Horiba, Ltd. benchtop pH meter F-73 and a Horiba, Ltd. pH electrode 9632-10D.

[0094] [Method of calculating the etching rate of SiN] 200 mL of etching solution heated to the predetermined temperature shown in Table 1 was prepared, and a 2 cm x 1 cm silicon substrate (silicon nitride film thickness 104 nm) on which a silicon nitride film had been epitaxially grown by low pressure CVD (LP-CVD) was immersed in the etching solution for 3 minutes. The etching solution was stirred at 1200 rpm during etching. The etching rate of the silicon nitride film (R SiN The thickness (nm / min) of each substrate was calculated by measuring the film thickness before and after etching with a spectroscopic ellipsometer (M-2000D manufactured by J.A. Woollam Co.), determining the amount of silicon nitride film etched from the difference in film thickness before and after treatment, and dividing the amount by the etching time (3 minutes).

[0095] [Si(100) and SiO 2 Etching selectivity ratio of SiN to SiN] The etching rate of silicon (R') was calculated in the same manner as in the calculation of the etching rate of SiN described above, except that a substrate (silicon (100) film, silicon (100) film thickness of 60 nm) in which silicon (Si) was epitaxially grown on a silicon-germanium (SiGe) substrate of 2 cm x 1 cm size was used, and the immersion time was set to 10 minutes. 100 The etching rate of silicon oxide (R , nm / min) was calculated in the same manner as in the calculation of the etching rate of SiN described above, except that a substrate (thickness of silicon oxide film: 105 nm) in which a silicon oxide film was epitaxially grown on a silicon substrate of 2 cm × 1 cm size was used and the immersion time was set to 10 minutes. SiO2 , nm / min) was calculated.

[0096] From these measurement results, it is clear that the silicon nitride film, silicon (100) and SiO 2 Etching selectivity (R SiN / R' 100、 R SiN / R SiO2 ) was sought.

[0097] The lower limit of the measurement of film thickness change using the spectroscopic ellipsometer used is 0.01 nm, so the lower limit of the etching rate of the silicon-germanium film that can be determined using the above method is 0.001 nm / min.

[0098] [Whether or Not the Etching Solution Discolored Before and After the Etching Step] The presence or absence of discoloration of the etching solution was visually confirmed and evaluated as an index of the stability of the etching solution.

[0099] <Production of Etching Solution> [Example 1] (Method of Preparing Etching Solution) Sulfuric acid (manufactured by Fujifilm Wako Pure Chemical Industries, electronics industry grade, 96% by mass aqueous solution, pKa at 25°C: -3.0) was diluted with ultrapure water and mixed to form a uniform chemical solution. Boric acid (manufactured by Fujifilm Wako Pure Chemical Industries, special grade reagent, powder) was then added as a boron compound not containing fluorine atoms to prepare an etching solution with a sulfuric acid concentration of 75% by mass and a fluorine-atom-free boron compound (boric acid) concentration of 0.8% by mass. The mixture was then heated at 195°C for 30 minutes, and the etching solution was then heated to 185°C (near the boiling point). The resulting etching solution was diluted 10 times by mass with water and measured at 24°C for a pH of 0.22. The results are shown in Table 1. The etching rates of silicon nitride, silicon oxide, and silicon were evaluated using the resulting etching solution. The evaluation results are shown in Table 2. In this experimental example, the etching rate (ER) of the silicon nitride film was 3.8 nm / min. SiN / R SiO2 ) is 41, and the etching selectivity (R SiN / R' 100 ) was 4.6, and the silicon nitride film could be selectively etched relative to the silicon oxide film and the silicon (100) film.

[0100] Examples 2 to 7 Etching solutions were prepared and evaluated in the same manner as in Example 1, except that the boric acid concentration was changed as shown in Table 1. The evaluation results are shown in Table 2.

[0101] Comparative Example 1 An etching solution was prepared and evaluated in the same manner as in Example 1, except that boric acid was not added. The evaluation results are shown in Table 2. In Comparative Example 1, the etching rate (also expressed as ER) of the silicon nitride film was lower than that in Example 1. In addition, the etching selectivity (R SiN / RSiO2 ), and the etching selectivity (R SiN / R' 100 ) are lower than those in Example 1, and in particular, the etching selectivity (R SiN / R' 100 ) was 2.5, which was lower than any of the Examples.

[0102] Comparative Examples 2 to 3 Etching solutions were prepared and evaluated in the same manner as in Example 1, except that the boric acid concentration was changed as shown in Table 1. The evaluation results are shown in Table 2. Comparative Examples 2 to 3 are experimental examples in which the concentration of added boric acid was less than 0.10 mass %. In Comparative Examples 2 and 3, the etching rate of the silicon nitride film was equal to or lower than that of Comparative Example 1, in which an etching solution without added boric acid was used, and in particular, the etching selectivity (R SiN / R' 100 ) were 3.0 and 2.8, respectively, which were lower than any of the Examples.

[0103] [Example 8] Etching solutions were prepared and evaluated in the same manner as in Example 1, except that the sulfuric acid concentration and boric acid concentration were changed as shown in Table 1 and further ammonia (manufactured by Hayashi Pure Chemical Industries, electronics industry grade, 28 mass % aqueous solution) was added as a basic compound in an amount of 0.25 molar equivalents relative to the sulfuric acid. The evaluation results are shown in Table 2.

[0104] Examples 9 to 16 Etching solutions were prepared and evaluated in the same manner as in Example 4, except that silicon or silicon oxide etching inhibitors were added as shown in Table 1. The evaluation results are shown in Table 2. In Examples 9 to 16, the silicon etching rate decreased and the etching selectivity (R SiN / R' 100) increased. In addition, in Examples 9 to 16, the etching rate of silicon oxide decreased, and the etching selectivity (R SiN / R SiO2 ) rose.

[0105] Examples 17 to 19 Etching solutions were prepared and evaluated in the same manner as in Example 1, except that methanesulfonic acid (manufactured by Tokyo Chemical Industry Co., Ltd., pKa at 25°C: -2.6) was used as the specific acid, the specific acid concentration and boric acid concentration were changed as shown in Table 1, and the etching temperature was set to 175°C. The evaluation results are shown in Table 2. In Examples 17 to 19, the etching rate of the silicon nitride film was lower than in Examples 1 to 7, which used sulfuric acid as the specific acid, but the etching rates of the silicon and silicon oxide films were relatively significantly lower, and the etching selectivity (R SiN / R SiO2 ) and the etching selectivity between the silicon nitride film and the silicon film (R SiN / R' 100 ) rose.

[0106] Example 20 An etching solution was prepared and evaluated in the same manner as in Example 1, except that sulfuric acid and methanesulfonic acid were used in combination as the specific acid, the concentrations of the specific acids were as shown in Table 1, and the etching temperature was 175°C. The evaluation results are shown in Table 2. In Example 20, the etching rate of the silicon nitride film was lower than in Example 4, which used sulfuric acid as the specific acid, but the etching rates of the silicon and silicon oxide films were relatively significantly lower, and the etching selectivity (R SiN / R SiO2 ) and the etching selectivity between the silicon nitride film and the silicon film (R SiN / R' 100 ) rose.

[0107] [Example 21] An etching solution was prepared and evaluated in the same manner as in Example 1, except that ammonium pentaborate octahydrate (manufactured by Toyama Pharmaceutical Co., Ltd.) was used as the boric acid compound and the etching solution was adjusted to have the concentration shown in Table 1. The evaluation results are shown in Table 2.

[0108] Comparative Example 4 An etching solution was prepared and evaluated in the same manner as in Example 1, except that fluorine-containing tetrafluoroboric acid (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., for chemical use, 42% by mass aqueous solution) was used as the boric acid compound, the etching solution was adjusted to the concentration shown in Table 1, and the etching temperature was set to 164°C. The evaluation results are shown in Table 2. In Comparative Example 4, the etching selectivity (R SiN / R SiO2 ) was 5.9, which was lower than any of the experimental examples in which boric acid, a boron compound that does not contain fluorine, was used as the boron compound.

[0109] It should be noted that while free hydrogen fluoride was produced in the etching solution of Comparative Example 4, free hydrogen fluoride was not produced in the other Examples and Comparative Examples.

[0110] Comparative Example 5 An etching solution was prepared and evaluated in the same manner as in Examples 17 to 19, except that boric acid was not added. The evaluation results are shown in Table 2. In Comparative Example 5, the etching rate (also expressed as ER) of the silicon nitride film was 0.2 nm / min, which was lower than in Examples 17 to 19 and also lower than in any of the Examples.

[0111] In Table 2, ER represents the etching rate of the silicon nitride film, and the etching selectivity represents the etching selectivity of the silicon nitride film relative to silicon or silicon oxide film.

[0112]

[0113]

[0114]

[0115] According to the present invention, it is possible to provide an etching solution that can efficiently etch silicon nitride and further suppress the generation of hydrogen fluoride, a substrate processing method, and a semiconductor device manufacturing method.

Claims

1. A silicon nitride etching solution comprising one or more acids selected from the group consisting of sulfuric acid and organic acids, a boron compound, and water, wherein the boron compound is a boron compound that does not contain fluorine atoms, the concentration of the boron compound is 0.10 mass% or more and 30.00 mass% or less, and the pH measured at 24°C after diluting 10 times by mass with water is 5.0 or less.

2. The silicon nitride etching solution according to claim 1, wherein the pKa of said acid at 25° C. is from −5 to 2.

3. The silicon nitride etching solution according to claim 1 or 2, wherein at least one of the boiling point and the decomposition temperature of the acid at 1 atmospheric pressure is 150° C. or higher and 400° C. or lower.

4. The silicon nitride etching solution according to any one of claims 1 to 3, wherein the organic acid is one or more organic acids selected from the group consisting of sulfonic acid compounds and carboxylic acid compounds.

5. The silicon nitride etching solution according to any one of claims 1 to 4, wherein the total concentration of the acid is 60 mass % or more and 90 mass % or less.

6. The silicon nitride etching solution according to any one of claims 1 to 5, wherein the boron compound is one or more boron compounds selected from the group consisting of boric acid, boric acid anhydride, and polymers of boric acid.

7. The silicon nitride etching solution according to any one of claims 1 to 6, further comprising one or more basic compounds selected from the group consisting of ammonia, amines, and tetraalkylammonium hydroxides.

8. The silicon nitride etching solution according to any one of claims 1 to 7, further comprising one or more silicon etching inhibitors selected from the group consisting of nonionic compounds, anionic compounds having a hydrophobic group, cationic compounds having a hydrophobic group, and amphoteric compounds having a hydrophobic group, wherein the concentrations of the compounds contained as the acids are all 10 mass% or more, and the concentrations of the compounds contained as the etching inhibitors are all less than 10 mass%.

9. The silicon nitride etching solution according to claim 8, wherein the etching inhibitor comprises one or more compounds selected from the group consisting of cationic compounds having a hydrophobic group and aromatic ring compounds having an electron-withdrawing group.

10. The silicon nitride etching solution according to claim 9, wherein the cationic compound is a cationic compound having two or more cationic sites in its structure.

11. The silicon nitride etching solution according to claim 9 or 10, wherein the aromatic ring compound having an electron-withdrawing group is an aromatic ring compound having one or more electron-withdrawing groups selected from the group consisting of a chloro group, a fluoro group, a trifluoromethyl group, a carboxyl group, and a nitro group.

12. The silicon nitride etching solution according to claim 11, wherein the aromatic ring compound having an electron-withdrawing group is an aromatic ring compound having two or more electron-withdrawing groups selected from the group consisting of a chloro group, a fluoro group, a trifluoromethyl group, a carboxyl group, and a nitro group.

13. A method for producing an etching solution for silicon nitride, comprising: a composition preparation step of preparing a composition containing one or more acids selected from the group consisting of sulfuric acid and organic acids, a boron compound not containing a fluorine atom, and water.

14. A method for treating a substrate containing silicon nitride, comprising an etching step of etching the silicon nitride using the silicon nitride etching solution according to any one of claims 1 to 12.

15. The method for treating a substrate according to claim 14, wherein the etching temperature in the etching step is 120 to 185°C.

16. The method for treating a substrate according to claim 14 or 15, wherein the substrate further contains at least one selected from the group consisting of silicon and silicon oxide, and the etching step is a step of selectively etching silicon nitride with respect to at least one selected from the group consisting of silicon and silicon oxide using the etching solution.

17. A method for manufacturing a semiconductor device using a substrate containing silicon nitride, comprising an etching step of etching the silicon nitride using the silicon nitride etching solution according to any one of claims 1 to 12.

18. The method for manufacturing a semiconductor device according to claim 17, wherein the etching temperature in the etching step is 120 to 185° C.

19. The method for manufacturing a semiconductor device according to claim 17 or 18, wherein the substrate further comprises at least one selected from the group consisting of silicon and silicon oxide, and the etching step is a step of selectively etching silicon nitride with respect to at least one selected from the group consisting of silicon and silicon oxide using the etching solution.

Citation Information

Patent Citations

  • Etchant for silicon nitride

    JP2012033561A

  • Composition

    JP2014082329A

  • Cleaning composition for removing etching residue

    JP2020170841A

  • Etching solution capable of suppressing particle appearance

    US20170321121A1

Cited By

  • Acidic silicon etching liquid capable of effectively regulating and controlling etching brightness

    CN122278481A

  • Silicon etching solution, method for processing silicon substrate, and method for manufacturing semiconductor device

    WO2026205413A1