A kind of printed brushed worsted wool fabric and preparation method thereof
A technology for printing and brushing worsted and wool, applied in the field of textiles, can solve problems such as difficulty in achieving printing effects, and achieve the effect of good color fastness
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
preparation example Construction
[0022] A method for preparing a printed napped worsted wool fabric, comprising:
[0023] S1. Step of sizing: sizing the woolen fabric after shrinking, and the sizing is alkaline sizing.
[0024] Specifically, before the sizing step, the woolen fabric is shrunk, so that the warp and weft directions of the woolen fabric are shrunk to a certain extent, and the increased surface strength can avoid the deformation of the woolen fabric in subsequent processes and improve the elasticity of the fabric. Warmth, and get a better feel.
[0025] Shrinking finishing includes shrinking, washing, boiling and drying in sequence. The specific parameters of each operation process are: the necking width of the shrinking process is 80-120mm, the roller pressure is 2-3bar, the shrinking box pressure is 1-2bar, the vehicle speed is 170-190m / min, the time is 60-90min, and the temperature is 35 ~ 45 ℃, the amount of shrinking agent is 3 ~ 5% of the cloth weight, in the embodiment of the present inv...
Embodiment 1
[0040] This embodiment provides a method for preparing a printed napped worsted wool fabric, and a printed napped worsted wool fabric prepared by the method.
[0041] The 100% wool used in this embodiment; the fabric specifications are: plain weave, width 150cm, meter weight 230g / m, warp density 440 threads / 10cm, and weft density 390 threads / 10cm.
[0042] A method for preparing a printed napped worsted wool fabric, comprising:
[0043] The wool fabric is subjected to shrinking finishing, and the shrinking finishing process includes shrinking, washing, boiling and drying in sequence. During the shrinking process, the necking width is 80mm, the roller pressure is 2bar, the shrinking box pressure is 1bar, the vehicle speed is 170m / min, the time is 60min, the temperature is 35°C, the amount of shrinking agent is 3% of the cloth weight, pH The value is 6.5; the temperature of the washing process is 35°C, the speed is 80 / min, the pressure is 1.5bar, the time is 8min, and the amoun...
Embodiment 2
[0050] The 100% wool used in this embodiment has a fabric specification of: weave 2 / 2 oblique to the right, a width of 150 cm, a meter weight of 450 g / m, a warp density of 630 threads / 10cm, and a weft density of 420 threads / 10cm.
[0051] A method for preparing a printed napped worsted wool fabric, comprising:
[0052] The wool fabric is subjected to shrinking finishing, and the shrinking finishing process includes shrinking, washing, boiling and drying in sequence. During the shrinking process, the necking width is 120mm, the roller pressure is 3bar, the shrinking box pressure is 2bar, the vehicle speed is 190m / min, the time is 90min, the temperature is 45°C, the amount of shrinking agent is 5% of the cloth weight, pH The value is 7.5; the temperature of the washing process is 45°C, the speed is 120 / min, the pressure is 2bar, the time is 10min, and the amount of soaping agent NF208 is 2% of the cloth weight; the temperature of the washing process is 90°C, and the speed is 40m...