A cold rolling tension roller with a wear-resistant and roughness-reducing nano-coating

By spraying a nanocoat that is resistant to wear and roughness reduction on the tension roller and designing both ends of the widening roller body, the unstability and fatigue wear problems during high-speed operation of the tension roller are solved, and the service life is significantly extended. Improve product quality and operating rate.

CN111438201BActive Publication Date: 2024-11-22SHANGHAI INFOMAN NANOTECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010250505.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-04-01
Publication Date
2024-11-22
Estimated Expiration
2040-04-01

AI Technical Summary

Technical Problem

The existing tension rollers rotate unsteadily and have large vibrations when operating at high speed. The roller surface is fatigued and worn due to changes in temperature fields, and the service life is short, making it difficult to meet the requirements of high-speed operation and product quality.

Method used

Using a nanocoat that is resistant to wear and roughness, including nano-bottom layer, nano-transition layer and nano-ceramic surface layer, it is sprayed on the surface of the tension roller through supersonic nano-thermal spraying equipment to form a metal cermet composite coating to enhance the roller surface Its wear resistance and crack resistance are stable by widening the roller body design and designing both ends of the roller body.

Benefits of technology

It significantly improves the service life of the tension roller to more than 2 years, eliminates vibration during high-speed operation, increases the roller operation speed to 12,000 to 18,000 speeds per minute, extends the unit operating rate and product quality, and reduces maintenance costs. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111438201B_ABST
    Figure CN111438201B_ABST
Patent Text Reader

Abstract

The invention discloses a cold rolling tension roller with a wear-resistant and roughness-reducing nano coating, comprising a roller body and a shaft base arranged at both ends of the roller body, the surface of the roller body is coated with a nano protective layer, the roller body comprises an outer roller body, a hollow roller body middle part and hollow roller body ends located at both ends of the roller body middle part, the roller body middle part and the roller body ends are both arranged inside the outer roller body, and the diameter of the roller body ends is greater than the diameter of the roller body middle part. The invention has a wear-resistant and crack-resistant nano-ceramic composite coating, the nano-coating has both good physical and chemical properties, can improve the bonding ability of the coating and the substrate, and at the same time improves the wear resistance and roughness reduction resistance of the tension roller surface, has both mechanical load and high temperature resistance, and the service life is increased from the original 7 months to more than 2 years, which is much longer than the service life of the cold rolling tension roller in the prior art, effectively improves the unit operation rate and product quality, reduces maintenance costs, and provides reliable guarantee for customers to reduce costs and increase efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of tensioning roller equipment, in particular to a cold rolling tensioning roller with a wear-resistant and roughness-reducing nano coating. Background Art

[0002] At present, the tension roller has problems such as insufficient rotation stability, low vibration critical point, large vibration, and difficulty in high-speed operation of the tension roller. In the actual production process, due to the uneven temperature field in the working environment of the tension roller, stress is generated. As the roller rotates, the temperature field changes periodically, and the stress also changes accordingly. The roller surface temperature is high, and the fatigue strength decreases, which causes the roller surface to crack due to fatigue. At the same time, the tension roller is subjected to mechanical stress during the pickling of the plate and strip, and the roller surface is severely worn, which not only affects the quality of the plate and strip, but also seriously affects the service life of the tension roller. The service life of the original roller is 7 months. The current solution is to build up the wear-resistant material on the roller surface to improve the wear resistance of the roller surface, or to use micron material to spray the wear-resistant layer to increase the service life of the roller. Both methods cannot solve the problems of roller surface wear, cracking, and roughness reduction leading to plate and strip slipping. The welding layer and the sprayed micron coating are easy to peel off. Summary of the invention

[0003] The object of the present invention is to provide a cold rolling tensioning roller with a wear-resistant and roughness-reducing nano-coating to solve one or more of the above-mentioned prior art problems.

[0004] According to the present invention, a cold-rolled tensioning roller with a wear-resistant and roughness-reducing nano-coating comprises a roller body and an axis base arranged at both ends of the roller body, the surface of the roller body is coated with a nano-protective layer, the roller body comprises an outer roller body, a hollow roller body middle part and hollow roller body ends located at both ends of the roller body middle part, the roller body middle part and the roller body ends are both arranged inside the outer roller body, and the diameter of the roller body ends is greater than the diameter of the roller body middle part.

[0005] The present invention has a wear-resistant and crack-resistant metal-ceramic composite coating. This nano coating has both good physical and chemical properties, can improve the bonding ability between the coating and the substrate, and at the same time improves the wear resistance and roughness reduction resistance of the tensioning roller surface. It has both mechanical load and high temperature resistance, and the service life is increased from the original 7 months to more than 2 years, which is much longer than the service life of the cold-rolled tensioning roller in the prior art. It effectively improves the unit operation rate and product quality, reduces maintenance costs, and provides reliable guarantee for customers to reduce costs and increase efficiency.

[0006] In some embodiments, the diameter of the middle part of the roller body is 150-450 mm, the diameter of the end of the roller body is 10 mm larger than the diameter of the middle part of the roller body, the outer end surface of the end of the roller body is provided with a connecting cylinder, the connecting cylinder ring is provided with a mounting base, and the mounting base is provided with a plurality of mounting screw holes. By increasing the width of the two ends of the roller body, it is possible to ensure that the pressure roller can remain stable during high-speed operation and eliminate vibration, so as to achieve the purpose of making the critical point outside the process speed, and the operating speed of the pressure roller can be increased to 12,000-18,000 rpm.

[0007] In some embodiments, the outer roller body is provided with a ring body at intervals, and the diameter of the ring body is larger than the diameter of the outer roller body. Both ends of the roller body are widened, which can solve the defect of unstable pressure roller running at high speed.

[0008] In some embodiments, the central axes of the outer roller body, the middle portion of the roller body, the end portions of the roller body, and the shaft base are located on the same straight line.

[0009] In some embodiments, the nano protective layer is a metal ceramic composite coating, which includes a nano bottom layer, a nano transition layer and a nano ceramic surface layer, and the nano bottom layer, nano transition layer and nano ceramic surface layer are sprayed sequentially from inside to outside.

[0010] In some embodiments, the grade of the metal-ceramic composite coating is INF-8235.

[0011] In some embodiments, the metal-ceramic composite coating has a thickness of 150-200 μm.

[0012] In some embodiments, the thickness of the nano bottom layer is 30-50 μm, the thickness of the nano transition layer is 40-60 μm, and the thickness of the nano ceramic surface layer is 80-90 μm. The coating with this thickness can ensure that the outer layer of the tension roller is not affected by the coating thickness, and can also make the surface of the tension roller more wear-resistant.

[0013] In some embodiments, a supersonic nano thermal spraying device is used to spray the nano protective layer on the roller body, and the spraying speed is 1350-2000 m / s. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 A schematic structural diagram of a cold rolling tension roller with a wear-resistant and roughness-reducing nano-coating according to an embodiment of the present invention;

[0015] Figure 2 A schematic structural diagram of an outer roller body of a cold rolling tension roller with a wear-resistant and roughness-reducing nano-coating according to an embodiment of the present invention;

[0016] Figure 3 This is a schematic structural diagram of a shaft base of a cold-rolled tensioning roller with a wear-resistant and roughness-reducing nano-coating according to an embodiment of the present invention. DETAILED DESCRIPTION

[0017] The present invention will be further described in detail below in conjunction with the accompanying drawings.

[0018] like Figure 1 As shown in the figure, a cold rolling tensioning roller with a wear-resistant and roughness-reducing nano-coating includes a roller body 1 and an axis base 2 arranged at both ends of the roller body 1, the surface of the roller body 1 is coated with a nano protective layer, the roller body 1 includes an outer roller body 11, a hollow roller body middle part 12 and hollow roller body end parts 13 located at both ends of the roller body middle part 12, the roller body middle part 12 and the roller body end parts 13 are both arranged inside the outer roller body 11, and the diameter of the roller body end parts 13 is larger than the diameter of the roller body middle part 12.

[0019] The nano protective layer is a metal-ceramic composite coating, which includes a nano bottom layer, a nano transition layer and a nano ceramic surface layer, which are sprayed in sequence from inside to outside.

[0020] The grade of the metal-ceramic composite coating is INF-8235. The metal-ceramic composite coating of INF-8235 can make the wear resistance of the entire coating better.

[0021] The thickness of the nano protective layer is 150~200μm, among which the nano bottom layer is a nano NGr layer, the nano base layer is a nano NGrS2Mo layer, and the nano ceramic layer is a chromium oxide-based ceramic composite layer; the thickness of the nano bottom layer is 30~50μm, the thickness of the nano transition layer is 40~60μm, and the thickness of the nano ceramic surface layer is 80~90μm. At this thickness of the nano protective layer, the entire tensioning roller has the effects of wear resistance, roughness reduction resistance, and crack resistance.

[0022] A supersonic nano thermal spraying device is used to spray a nano protective layer on the roller body 1, and the spraying speed is 1350-2000 m / s.

[0023] The microhardness of the prepared nano coating reaches HV900-1100, the roller surface roughness is Ra5-6, the roller surface dynamic balance imbalance is less than 80 grams, and the service life is more than 700 days.

[0024] The present invention provides a cold-rolled tensioning roller with a wear-resistant and roughness-reducing nano-coating, which has a wear-resistant, roughness-reducing and crack-resistant nano-coating composite material. The composite material has both good physical and chemical properties, and can improve the bonding ability between the coating and the substrate, while improving the wear resistance and roughness-reduction resistance of the tensioning roller surface, and has both mechanical load and high temperature resistance. The service life is increased from the original 7 months to more than 2 years, which is much longer than the service life of the cold-rolled tensioning roller in the prior art, effectively improving the unit operation rate and product quality, reducing maintenance costs, and providing reliable guarantee for customers to reduce costs and increase efficiency.

[0025] A method for preparing a wear-resistant and roughness-reducing nano-coating:

[0026] The steps include:

[0027] (1) Cleaning and degreasing: the roller body 1 is immersed in a non-ionic surfactant solution with a mass concentration of 3% to 5% for cleaning, and then ultrasonically cleaned in acetone. After ventilation and drying, it is calcined at 280 to 360° C. for 1 to 3 hours and naturally cooled to room temperature;

[0028] (2) Preparation of nano-bottom layer: The cooled roller body 1 is placed in a vacuum furnace and evacuated to 3×10-1Pa~5×10-1Pa first, and then evacuated to 1.2×10 -2 Pa, heat the furnace body to 650°C, introduce argon gas into the furnace body to raise the pressure to 2.5Pa, turn on the NGr target, set the current to 2-3A, bias voltage to -75--95V, and deposit a metal Ti layer on the surface of the circular saw blade substrate for 8-14 minutes;

[0029] (3) Preparation of nano transition layer: nitrogen gas is introduced into the vacuum furnace to raise the pressure to 4 Pa, and a first NGrS2Mo layer is deposited on the surface of the metal Ti layer for 5 to 7 minutes at a Ti target current of 2 to 3 A and a bias voltage of -75 to -95 V. Then, nitrogen gas is introduced to raise the pressure to 4 Pa, and a second NGrS2Mo layer is deposited on the first NGrS2Mo layer for 6 to 8 minutes, thereby preparing a nano transition layer;

[0030] (4) Preparation of nano-ceramic surface layer: Turn on the chromium oxide-based alloy target and the ceramic target, and apply a current of 4 to 6A and a bias voltage of -86 to -110V, so that the chromium oxide-based alloy target and the ceramic target are alternately deposited to form a nano-ceramic surface layer, and the deposition time is 20 to 25 minutes;

[0031] In the above, by increasing the width at both ends of the roller body 1, it is possible to ensure that the roller can remain stable and eliminate vibration during high-speed operation, thereby achieving the purpose of making the critical point outside the process speed. The operating speed of the roller can be increased to 12,000 to 18,000 rpm.

[0032] Among them, Figure 3 As shown in , the roller body diameter is 150~450mm, the diameter of the roller body end 13 is 10mm larger than the diameter of the roller body middle part 12, the roller body coating thickness is 150-200um, the outer end surface of the roller body end 13 is provided with a connecting cylinder 14, the connecting cylinder 14 is surrounded by a mounting base 15, and the mounting base 15 is provided with a plurality of mounting screw holes. In this embodiment, both ends of the roller body 1 are widened, and the diameter of the roller body end 13 is 10mm larger than the diameter of the roller body middle part 12, which can solve the defect of the unsteady pressure roller in high-speed operation.

[0033] Screw holes are also provided at positions corresponding to the mounting screw holes of the shaft base 2, and the shaft base 2 and the roller end 13 are fixedly connected by screws. The screws are installed and fixed along the axis direction, with good fixing effect, stable and convenient installation.

[0034] like Figure 2 As shown in the figure, the outer roller body 11 is provided with a ring body 3 at intervals, and the diameter of the ring body 3 is slightly larger than the diameter of the outer roller body 11. The function of the ring body 3 is to make the silk thread easy to be formed on the pressure roller, so as to become a silk cake.

[0035] The central axis of the outer roller body 11, the roller body middle part 12, the roller body end 13 and the shaft base 2 are located on the same straight line. The purpose of this design is to ensure that the speed of the pressure roller is stable and steady under the same axis.

[0036] The cold rolling tension roller with wear-resistant and roughness-reducing nano coating provided by the present invention can eliminate the critical point and roller vibration during high-speed rotation of the roller by adjusting the width of the inner cavity at both ends of the sleeve, thereby achieving the purpose of smooth rotation.

[0037] The above is only a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several similar modifications and improvements without departing from the creative concept of the present invention, and these are also considered to be within the scope of invention protection.

Claims

1. A cold rolling tension roller with a wear-resistant and roughness-reducing nano-coating, characterized in that: The invention comprises a roller body (1) and shaft bases (2) arranged at both ends of the roller body (1); the surface of the roller body (1) is coated with a nano protective layer; the roller body (1) comprises an outer roller body (11), a hollow roller body middle part (12) and hollow roller body ends (13) located at both ends of the roller body middle part (12); the roller body middle part (12) and the roller body ends (13) are both arranged inside the outer roller body (11); and the diameter of the roller body ends (13) is greater than the diameter of the roller body middle part (12); The diameter of the middle part (12) of the roller body is 150-450 mm, the diameter of the end part (13) of the roller body is 10 mm larger than the diameter of the middle part (12) of the roller body, the outer end surface of the end part (13) of the roller body is provided with a connecting cylinder (14), the connecting cylinder (14) is provided with a mounting base (15) around it, and the mounting base (15) is provided with a plurality of mounting screw holes; screw holes are also provided at positions corresponding to the mounting screw holes of the shaft base (2), and the shaft base (2) and the end part (13) of the roller body are fixedly connected by screws, and the screws are installed and fixed along the axis direction; The nano protective layer is a metal-ceramic composite coating, which includes a nano bottom layer, a nano transition layer and a nano ceramic surface layer, and the nano bottom layer, the nano transition layer and the nano ceramic surface layer are sprayed in sequence from the inside to the outside; The thickness of the metal-ceramic composite coating is 150-200 μm; The thickness of the nano bottom layer is 30-50 μm, the thickness of the nano transition layer is 40-60 μm, and the thickness of the nano ceramic surface layer is 80-90 μm.

2. A cold rolling tension roller with a wear-resistant and roughness-reducing nano-coating according to claim 1, characterized in that: The outer roller body (11) is provided with a ring body (3) at intervals, and the diameter of the ring body (3) is greater than the diameter of the outer roller body (11).

3. The cold rolling tension roller with wear-resistant and roughness-reducing nano-coating according to claim 1, characterized in that: The central axes of the outer roller body (11), the roller body middle part (12), the roller body end part (13) and the shaft base (2) are located on the same straight line.