A method for preparing fiber membrane dry electrode by spinning directly on skin
By spinning the fiber membrane dry electrode on the skin, combining the fiber structure and conductive materials, the problems of complex preparation and poor fit of existing dry electrodes are solved, and efficient preparation of fiber membrane dry electrodes is achieved, which improves the pulling of the electrodes Extensibility and breathability.
Patent Information
- Application Number
- CN202110388798.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-04-12
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-04-12
AI Technical Summary
The existing dry electrodes are complex in the preparation process and have poor fit with the skin, lack breathability and permeability, and cannot achieve long-term wear and continuous monitoring.
The method of preparing fiber membrane dry electrodes is adopted to spin directly on the skin. By mixing the spinning polymer and conductive materials in proportion to form a spinning liquid, it is used to form a fiber membrane on the skin by using solution airflow, electrostatic or high-speed rotary centrifugal spinning technology. Dry electrodes, combining fiber structures and conductive materials, improve fit and breathability.
A one-step forming fiber membrane dry electrode is realized, which improves the tensile and fit of the electrode, improves breathable and permeable properties, and avoids preprocessing steps and toxic solvent residues.
Smart Images

Figure CN113100773B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of novel flexible electrodes, and in particular relates to a method for preparing a fiber membrane dry electrode by spinning directly on the skin. Background Art
[0002] With the continuous development of flexible wearable devices, dry electrodes for physiological signals, which play an important role in signal transmission in human body sensing and machine interface, are gaining more and more attention. Dry electrodes are a commonly used electrode with a stable structure, which is most likely to achieve the purpose of long-term wear and continuous monitoring. However, dry electrodes often have some problems such as poor skin adhesion, complex preparation, and poor stretchability.
[0003] There are many dry electrode products reported in the literature and commercialized, but they can be roughly divided into the following categories: (1) hard materials, such as metal sheets; (2) flexible materials, such as conductive polymer films, graphene, carbon nanotubes, and polymer composites based on them; (3) structured materials, such as fabric electrodes, structured metal films, metal wires, conductive polymers, etc.
[0004] The above dry electrodes have some problems in terms of preparation and performance. For example, the metal sheet electrodes have poor stretchability and flexibility and cannot fit tightly to the skin. When using flexible or structured materials, either the electrodes are thicker and have poor fit to the skin, or the electrodes need to be ultra-thin, which makes processing more complicated. The electrodes are not breathable or have poor breathability. Summary of the invention
[0005] In response to the existing technical problems raised in the background technology, the present invention proposes a method for preparing fiber membrane dry electrodes by spinning directly on the skin, which can detect physiological electrical signals and solve the problems of complex preparation process of commonly used dry electrodes, poor skin adhesion, and air and sweat impermeability.
[0006] To achieve the above object, the present invention adopts the following technical solution: a method for preparing a fiber membrane dry electrode by spinning directly on the skin, the method comprising the following steps:
[0007] (1) mixing a spinning polymer, a conductive material and a solvent in proportion to form a uniform spinning solution. The spinning polymer and the conductive material can be separately added with a solvent to form a solution and then mixed to obtain the final spinning solution, or can be directly mixed and then the solvent is added to obtain the final spinning solution;
[0008] (2) The above spinning solution is directly used as a substrate for spinning on the skin to prepare a fiber membrane dry electrode.
[0009] In the technical solution of the present invention, the mass ratio of the spinning polymer and the conductive material in the spinning solution is (1:3)-(5:1), and the total mass concentration of the spinning polymer and the conductive material in the spinning solution is 1-30%.
[0010] In the technical solution of the present invention, the spinning polymer is selected from one or more of polyvinyl alcohol (PVA, molecular weight of 10,000-200,000), polyethylene oxide (PEO, molecular weight of 100,000-8 million), polyvinyl pyrrolidone (PVP, molecular weight of 20,000-1.5 million), and polyvinyl butyral (PVB, molecular weight of 10,000-300,000).
[0011] In the technical solution of the present invention, the conductive material is selected from one or more of metal particles, conductive carbon materials, and conductive polymers.
[0012] In the technical solution of the present invention, the metal particles include metal nanowires, metal nanoparticles, and metal nanosheets.
[0013] In the technical solution of the present invention, the conductive carbon material includes carbon nanotubes (CNT), graphene, carbon black, acetylene black, and carbon fiber.
[0014] In the technical solution of the present invention, the conductive polymer includes poly(3,4-ethylenedioxythiophene)-poly(styrene sulfonic acid) (PEDOT:PSS), polypyrrole, polyaniline, and polyacetylene.
[0015] In the technical solution of the present invention, the solvent is water or ethanol, or a mixture of the two.
[0016] In the technical solution of the present invention, the spinning method is selected from one or a combination of solution airflow spinning, electrostatic spinning, and high-speed rotary centrifugal spinning.
[0017] In the technical solution of the present invention, the spinning equipment used for spinning has a solution flow rate of 0.01-10 ml / h, a spinning distance of 2-30 cm, and a spinning time of more than 1 min. The specific time needs to be determined based on the material and the spinning area.
[0018] In the technical solution of the present invention, for solution airflow spinning, in addition to the above conditions, the spinning airflow temperature is set not to exceed 70°C; for electrospinning, in addition to the above conditions, the spinning needle and ground voltage are set to 1-20kV; for high-speed rotary centrifugal spinning, in addition to the above conditions, the rotation speed of the spinning plate is set to 100-5000rpm.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] 1. Using the skin as the substrate, the fiber membrane dry electrode is prepared by spinning directly on the skin, which is formed in one step and avoids various pre-processing and transfer steps.
[0021] 2. The fiber mesh structure formed on the skin combines the fiber structure and the conductive material into one, which effectively improves the stretchability and fit of the electrode to the skin and improves the breathability and sweat permeability of the electrode.
[0022] 3. Use water or ethanol, or a mixture of the two as the solvent to avoid the stimulation of organic solvents during the preparation process and the final toxic solvent residue. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a physical picture of the fiber membrane dry electrode prepared by spinning directly on the skin in Example 1.
[0024] Figure 2 This is the SEM image of the fiber membrane dry electrode prepared by spinning directly on the skin in Example 1.
[0025] Figure 3 This is the SEM image of the fiber membrane dry electrode prepared by spinning directly on the skin in Example 2.
[0026] Figure 4 This is the SEM image of the fiber membrane dry electrode prepared by spinning directly on the skin in Example 3. DETAILED DESCRIPTION
[0027] The present invention will be further described in detail below in conjunction with the examples, but the embodiments of the present invention are not limited thereto.
[0028] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the protection scope of the present invention.
[0029] Example 1
[0030] The 6 million molecular weight PEO polymer was dissolved into a 2% water dispersion, and then mixed with the PEDOT:PSS aqueous solution (mass concentration 1%) at a mass ratio of 1:1 to form a uniform spinning solution. The final spinning solution had a polymer and conductive material mass ratio of 2:1 and a total mass concentration of 1.5%. The spinning solution was then placed in the spray gun of the solution air spinning equipment (nozzle diameter 0.2mm), the flow rate of the solution air spinning equipment was 0.4ml / h, the pressure was 100psi, the spinning air temperature was 60℃, the receiving distance was 10cm, the spinning time was 10min, and the fiber membrane dry electrode was formed directly on the skin by spinning. The actual picture of the electrode prepared by spinning on the skin is shown in the attached figure. Figure 1 As shown in the figure, it can be seen that the electrode has good adhesion to the skin, can be deformed with the skin compression, and the skin texture is clearly visible. The obtained fiber membrane dry electrode is peeled off from the skin, and the SEM photo obtained by scanning electron microscopy is shown in Figure 2 ,from Figure 2 It can be seen that the fiber membrane dry electrode prepared in Example 1 presents a porous structure, which is conducive to air permeability.
[0031] Example 2
[0032] The 4 million molecular weight PEO polymer was dissolved and prepared into a 3% aqueous dispersion, and then mixed with the PEDOT:PSS aqueous solution (mass concentration of 1%) at a mass ratio of 1:1 to form a uniform spinning solution. The final mass ratio of polymer to conductive material in the spinning solution was 3:1, and the total mass concentration was 2%. The spinning solution was then placed in the spray gun of the solution air spinning equipment (nozzle diameter 0.2mm). The flow rate of the solution air spinning equipment was 0.6ml / h, the spinning air pressure was 80psi, the spinning air temperature was 55°C, the receiving distance was 10cm, the spinning time was 15min, and the fiber membrane dry electrode was directly sprayed on the skin. The obtained fiber membrane dry electrode was peeled off from the skin, and the SEM photo obtained by scanning electron microscopy was shown in FIG. Figure 3 ,from Figure 3 It can be seen that the fiber membrane dry electrode prepared in Example 2 has a fluffy fiber arrangement.
[0033] Example 3
[0034] The polyvinyl butyral polymer was dissolved in a mixture of ethanol and water (mass ratio 9:1) to prepare a 12% solution, and then the hydroxylated carbon nanotubes were dispersed in ethanol to form a 3% dispersion. The two were then mixed and stirred at a mass ratio of 1:0.8 to form a uniform spinning solution. The final mass ratio of polymer to conductive material in the spinning solution was 5:1, and the total mass concentration was 8%. Finally, the spinning solution was placed in the spray gun of the solution airflow spinning equipment (nozzle diameter 0.2mm), with a pressure of 100psi, a flow rate of 0.8ml / h in the spinning equipment, a spinning airflow temperature of 22°C, a receiving distance of 15cm, and a spinning time of 8min, and the fiber membrane dry electrode was directly sprayed on the skin. The obtained fiber membrane dry electrode was peeled off from the skin, and the SEM photo obtained by scanning electron microscopy was shown in FIG. Figure 4 ,from Figure 4 It can be seen that the fiber membrane prepared in Example 3 has a thin dry fiber diameter and is porous and breathable.
[0035] In summary, from Figure 1-4 It can be explained that the method for preparing fiber membrane dry electrodes by spinning directly on the skin provided by the present invention forms a fiber mesh structure on the skin, which combines the fiber structure and the conductive material into one, effectively improving the stretchability of the electrode and its conformity to the skin while retaining the porous air permeability of the fiber electrode.
[0036] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A method for preparing a fiber membrane dry electrode by spinning directly on the skin, characterized in that: The method comprises the following steps: (1) mixing a spinning polymer, a conductive material and a solvent in proportion to form a uniform spinning solution; (2) Spinning the above spinning solution directly on the skin as a substrate to prepare a fiber membrane dry electrode; The conductive material is selected from one or more of metal particles, conductive carbon materials, and conductive polymers; The mass ratio of the spinning polymer to the conductive material in the spinning solution is (2:1)-(5:1), and the total mass concentration of the spinning polymer and the conductive material in the spinning solution is 1-8%; The spinning polymer is selected from one or more of polyvinyl alcohol, polyethylene oxide, polyvinyl pyrrolidone and polyvinyl butyral.
2. The method for preparing a fiber membrane dry electrode by spinning directly on the skin according to claim 1, characterized in that: The metal particles include metal nanowires, metal nanoparticles or metal nanosheets.
3. The method for preparing a fiber membrane dry electrode by spinning directly on the skin according to claim 1, characterized in that: The conductive carbon material includes carbon nanotube, graphene, carbon black, acetylene black or carbon fiber.
4. The method for preparing a fiber membrane dry electrode by spinning directly on the skin according to claim 1, characterized in that: Conductive polymers include poly(3,4-ethylenedioxythiophene)-poly(styrene sulfonic acid), polypyrrole, polyaniline or polyacetylene.
5. The method for preparing a fiber membrane dry electrode by spinning directly on the skin according to claim 1, characterized in that: The solvent is water or ethanol, or a mixture of the two.
6. The method for preparing a fiber membrane dry electrode by spinning directly on the skin according to claim 1, characterized in that: The spinning method is selected from one or a combination of solution air spinning, electrostatic spinning, and high-speed rotary centrifugal spinning.
7. The method for preparing a fiber membrane dry electrode by spinning directly on the skin according to claim 6, characterized in that: The solution flow rate of spinning is 0.01-10mL / h, the spinning distance is 2-30cm, and the spinning time is greater than 1min.