Conductive film, dispersion, method for making the same, and device containing the conductive film

By using semiconductor nanoparticle separation and arrangement technology in the conductive film, the problems of high manufacturing cost and substrate limitation are solved, high conductive film formation on various substrates are achieved, and excellent fold resistance is demonstrated and transparency.

CN114651312BActive Publication Date: 2024-11-26OSAKA UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080072032.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-10-15
Filing Date
2020-10-15
Publication Date
2024-11-26
Estimated Expiration
2040-10-15

AI Technical Summary

Technical Problem

The existing conductive films have high manufacturing costs and are difficult to achieve high conductivity on a wide range of substrates, especially the use of precious metal elemental materials and special carbon materials limits their industrial applications.

Method used

Semiconductor nanoparticles are used as conductive elements to achieve high conductivity through their separation from each other in the film. Conductive films are formed on various substrates using non-vacuum film formation techniques such as coating methods and coordinated by specific compounds. and structural design improves conductivity and transparency.

Benefits of technology

It is realized that high-conductive conductive films are obtained without using precious metals and special carbon materials, which reduces manufacturing costs, and achieves high-efficiency film formation on a variety of substrates, with excellent fold resistance and transparency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114651312B_ABST
    Figure CN114651312B_ABST
Patent Text Reader

Abstract

The present invention provides a conductive film that can be formed without using a vacuum film forming method and includes a material that is not a noble metal and a special carbon material as a conductive element for expressing conductivity. The conductive film provided includes an arrangement portion of semiconductor nanoparticles, and when a cross section including the arrangement portion is observed, in the arrangement portion, the semiconductor nanoparticles are arranged in a row in a state of being separated from each other, and the conductivity C1 measured in at least one direction is 7 S / cm or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a conductive film, in particular a light-transmitting conductive film, a method for producing a conductive film, a dispersion for producing a conductive film, and a method for producing the dispersion, and also to a device comprising the conductive film. Background Art

[0002] Conductive films, especially highly light-transmitting transparent conductive films, are used in various devices as electrodes, antistatic films, etc. Industrial mass production of conductive films is often carried out by vacuum film forming methods represented by sputtering.

[0003] In the vacuum film forming method, since a reduced pressure atmosphere is required, large-scale equipment is required, and there is a problem that the substrate that can be used is limited. In view of this situation, a conductive film containing silver nanowires (for example, Patent Document 1 and Non-Patent Document 1) and a conductive film containing carbon nanotubes (for example, Patent Document 2) have been proposed. These conductive films can be formed by a printing method, a coating method, etc. that do not require a reduced pressure atmosphere.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2017-92036

[0007] Patent Document 2: International Publication No. 2015 / 115102

[0008] Non-patent literature

[0009] Non-patent document 1: Nakazawa Eri et al., "Development of Silver Nanowire Ink for Transparent Conductive Films", Journal of the Intelligent Processing Society, Intelligent Processing Society, Vol. 4, No. 4, 2015, pp. 202-206 Summary of the invention

[0010] Problems to be solved by the invention

[0011] However, it is not easy to reduce the manufacturing cost of single noble metal materials such as silver nanowires and carbon nanotubes or special carbon materials. An object of the present invention is to provide a conductive film that can be formed without using a vacuum film forming method and includes a material that is not equivalent to a noble metal or a special carbon material as a conductive element for exhibiting conductivity. Another object of the present invention is to provide a method and a dispersion for manufacturing such a conductive film, a method for manufacturing the dispersion, and a device including such a conductive film.

[0012] Methods used to solve problems

[0013] The presence of a conductive path formed by conductive elements contacting each other in a film is considered essential for the practical expression of conductivity. However, according to the research of the present inventors, a film containing semiconductor nanoparticles separated from each other can also express unexpectedly high conductivity.

[0014] That is, the present invention provides a conductive film comprising an arrangement portion of semiconductor nanoparticles. When observing a cross-section comprising the arrangement portion, in the arrangement portion, the semiconductor nanoparticles are arranged in a row in a state of being separated from each other, and the conductivity C1 measured along at least one direction is greater than 7 S / cm.

[0015] The conductivity required for the conductive film is sometimes sufficient in practice as long as it is achieved in a specific direction. From this point of view, the conductive film does not necessarily need to show high conductivity in all directions. Based on this concept, a conductive film with high utilization value containing semiconductor nanoparticles as conductive elements can be obtained.

[0016] That is, from another aspect, the present invention provides a conductive film containing semiconductor nanoparticles as conductive elements, and utilizing the above-mentioned conductive elements to exhibit anisotropic conductivity, with a conductivity C1 measured along a first direction being greater than 7S / cm and a conductivity C2 measured along a second direction being less than 10% of the above-mentioned conductivity C1, and any one of the above-mentioned first direction and the above-mentioned second direction being a film surface direction, and the other being a film thickness direction.

[0017] Furthermore, the present invention provides a dispersion suitable for producing the above-mentioned conductive film.

[0018] That is, from another aspect, the present invention provides a dispersion comprising a dispersion medium, semiconductor nanoparticles dispersed in the dispersion medium, and a first compound.

[0019] The first compound exists in the form of an attached compound attached to the semiconductor nanoparticle and a free compound released from the semiconductor nanoparticle.

[0020] The dispersion satisfies at least one of i) to iv):

[0021] i) the ratio of the amount of the first compound present in the form of the free compound to the amount of the first compound present in the form of the attached compound is 1 or more;

[0022] ii) the ratio of the amount of the first compound to the total amount of the semiconductor nanoparticles and the first compound is 10% or more on a mass basis;

[0023] iii) the semiconductor nanoparticles comprise at least one selected from oxides, sulfides, selenides and tellurides;

[0024] iv) The semiconductor nanoparticles are columnar and / or polyhedral.

[0025] In addition, the present invention provides a method for producing the dispersion of the present invention. The method is the following method, which comprises:

[0026] Mixing a stock solution containing a dispersion medium, semiconductor nanoparticles dispersed in the dispersion medium, a first compound, and impurities with a solvent to obtain a mixed solution;

[0027] Applying centrifugal operation to the mixed solution at a rotation speed of less than 5000 rpm; and

[0028] After the centrifugation operation, the solvent is removed from the mixed solution together with at least a portion of the impurities.

[0029] In addition, from another aspect, the present invention provides an ink set, which comprises:

[0030] A first ink is a dispersion containing a dispersion medium, semiconductor nanoparticles and a first compound dispersed in the dispersion medium, wherein the first compound exists in the form of an attached compound attached to the semiconductor nanoparticles and a free compound freed from the semiconductor nanoparticles; and

[0031] The second ink includes a second compound having a molecular weight smaller than that of the first compound, capable of replacing the first compound and adhering to the semiconductor nanoparticles.

[0032] Furthermore, from another aspect, the present invention provides a device comprising the conductive film of the present invention as at least one functional film selected from an electrode film, an antistatic film, a heat generating film, and an electromagnetic shielding film.

[0033] From another aspect, the present invention provides a device comprising a conductive film containing semiconductor nanoparticles and at least one electrode in contact with the conductive film.

[0034] The above conductive film satisfies the following a) and / or b):

[0035] a) comprising an arrangement portion of the semiconductor nanoparticles,

[0036] When observing a cross section including the arrangement portion, in the arrangement portion, the semiconductor nanoparticles are arranged in a row in a state of being separated from each other.

[0037] The electrical conductivity C1 measured along at least one direction is greater than 7 S / cm;

[0038] b) containing the above-mentioned semiconductor nanoparticles as conductive elements,

[0039] The conductive element exhibits anisotropic conductivity, wherein the conductivity C1 measured along the first direction is 7 S / cm or more and the conductivity C2 measured along the second direction is less than 10% of the conductivity C1.

[0040] Either one of the first direction and the second direction is a film surface direction, and the other is a film thickness direction.

[0041] From another aspect, the present invention provides a method for manufacturing the conductive film of the present invention. The manufacturing method is the following method for manufacturing the conductive film, which comprises:

[0042] In a first step, a first ink is applied onto a surface of a substrate to form a coating film, wherein the first ink is a dispersion comprising a dispersion medium, semiconductor nanoparticles and a first compound dispersed in the dispersion medium, and the first compound exists in the form of an attached compound attached to the semiconductor nanoparticles and a free compound freed from the semiconductor nanoparticles; and

[0043] In the second step, a second ink containing a second compound having a molecular weight smaller than that of the first compound and capable of replacing the first compound and adhering to the semiconductor nanoparticles is brought into contact with the coating film, thereby replacing at least a portion of the first compound in the coating film with the second compound.

[0044] Effects of the Invention

[0045] The conductive film of the present invention can be formed by a coating method, for example, in addition to the vacuum film forming method, and semiconductor nanoparticles are used as the conductive element for exhibiting conductivity. Therefore, it can be formed on a wide range of substrates, and from the perspective of reducing manufacturing costs, it is more advantageous than a film using a noble metal single substance material or a special carbon single substance material as the conductive element. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1 is a cross-sectional view showing an example of a conductive film.

[0047] Figure 2 This is a diagram showing an example of the shape and arrangement of semiconductor nanoparticles included in a conductive film.

[0048] Figure 3 This is a diagram showing another example of the shape and arrangement of semiconductor nanoparticles included in the conductive film.

[0049] Figure 4 This is a diagram showing still another example of the shape and arrangement of semiconductor nanoparticles included in the conductive film.

[0050] Figure 5 It is a cross-sectional view showing an example of a device including a conductive film.

[0051] Figure 6 It is a cross-sectional view showing another example of a device including a conductive film.

[0052] Figure 7 This is a diagram showing an example of light transmittance.

[0053] Figure 8 This is an example of an image obtained by observing a conductive film using a transmission electron microscope (TEM).

[0054] Fig. 9 This is another example of an image obtained by observing a conductive film using a TEM.

[0055] Fig.10 This is a diagram for explaining a bending test.

[0056] Fig.11 This is a diagram showing an example of a change in resistivity of a conductive film caused by a bending test. DETAILED DESCRIPTION

[0057] Hereinafter, the embodiments of the present invention will be described with reference to the accompanying drawings as appropriate, but the following description is not intended to limit the present invention to a specific embodiment. In this specification, the term "semiconductor" is used to include not only ordinary semiconductors but also semimetals. Semimetals are materials having a band structure in which the lower part of the conduction band and the upper part of the valence band overlap slightly across the Fermi level due to strain of the crystal structure or the interaction between the layers of the crystal. The term "nanoparticle" refers to a particle whose minimum diameter is less than 1 μm, for example, a particle in the range of 0.1 nm or more and less than 1 μm. Nanoparticles typically refer to particles whose maximum size is less than 5 μm, and further in the range of 3 nm to 2 μm. It should be noted that the "minimum diameter" is determined by the minimum size passing through the center of gravity of the particle, and the "maximum size" is determined by the longest line segment that can be set in the particle. In addition, the term "substantially parallel" is used to limit the difference in direction between each other to less than 10°, especially less than 5°. The term "arrange autonomously" or "autonomous arrangement" refers to the self-organized arrangement of semiconductor nanoparticles with the interaction between particles as the driving force. In addition, the term "functional group" is used as a term also including a halogen atom.

[0058] <Conductive Film>

[0059] The conductive film of this embodiment contains semiconductor nanoparticles as conductive elements. The conductive film includes an arrangement portion of semiconductor nanoparticles. When observing a cross section including the arrangement portion, in the arrangement portion, the semiconductor nanoparticles are arranged in a state of being separated from each other. The semiconductor nanoparticles may be arranged in a row in the arrangement portion. The conductive film may include a plurality of arrangement portions extending substantially parallel to each other, or may include a plurality of arrangement portions that intersect each other or are connected to each other at the ends. The conductive film may also have an arrangement portion in which semiconductor nanoparticles are arranged in a row in a state of being separated from each other in at least one cross section thereof.

[0060] The conductivity C1 of the conductive film measured along at least one direction is greater than 7S / cm. When the direction for measuring the conductivity C1 is set as the first direction, the conductivity C2 measured along the second direction different from the first direction can be, for example, less than 10% of the conductivity C1, especially less than 1% (i.e., C2 / C1<0.1, especially C2 / C1<0.01). The first direction and the second direction can also be orthogonal to each other. One of the characteristics of the conductive film of this embodiment is the anisotropy of conductivity. Here, with respect to the first direction and the second direction, for example, one is a direction parallel to the film surface, i.e., the film surface direction, and the other is a direction perpendicular to the film surface, i.e., the film thickness direction. The lower limit of the conductivity C2 is not particularly limited, for example, 2×10 -5 S / cm or more.

[0061] In the cross section where the arrangement of semiconductor nanoparticles is observed, the average spacing between adjacent semiconductor nanoparticles is preferably less than 10 nm. Regarding the "average spacing" of semiconductor nanoparticles, in the arrangement of semiconductor nanoparticles appearing in the film cross section, the shortest distance between two particles that are separated and adjacent to each other is measured respectively, and determined by the arithmetic average thereof. As an example, the average distance can be determined by measuring the shortest distance between two particles that are separated and adjacent to each other at 10 locations along the relative portions of the two particles and using the arithmetic average thereof (the so-called 10-point average). Adjacent semiconductor nanoparticles in the arrangement portion in the above-mentioned cross section are preferably separated in a manner that the sides that are substantially parallel to each other. In the conductive film, the first direction for obtaining a conductivity C1 of more than 7S / cm may also be parallel to the cross section where the above-mentioned arrangement portion appears. The arrangement portion may also be formed by the semiconductor nanoparticles being autonomously arranged during the formation of the conductive film.

[0062] The conductive film may include a compound attached to the semiconductor nanoparticles, i.e., an attached compound. The attached compound is a compound different from the semiconductor constituting the semiconductor nanoparticles, typically an organic or inorganic compound that is not equivalent to a semiconductor, and preferably a compound different from the attached substance that is used to protect the semiconductor nanoparticles contained in the conductive ink as a dispersion of semiconductor nanoparticles from agglomeration. The molecular weight of the attached compound is preferably less than 300, less than 200, or less than 150, further preferably less than 110, and particularly preferably less than 60. The attached compound may also have a functional group suitable for binding to semiconductor nanoparticles, such as a ligand that can bind to a metal atom through coordination. The functional group may be contained as an ion constituting a salt. However, in this case, the molecular weight of the compound is calculated by removing the counter ion of the salt. Therefore, for example, the molecular weight of KSCN containing SCN that can be attached to semiconductor nanoparticles is calculated by removing K and is 58.1.

[0063] The three-dimensional shape of semiconductor nanoparticles can be a column and / or a polyhedron. The bottom surface of the column is not particularly limited, for example, a circle, an ellipse, or a polygon. The column is typically a column with two identical and parallel bottom surfaces, but is not limited thereto, for example, a vertical cross section obtained by cutting along the surface passing through the two bottom surfaces is a quadrilateral or can be regarded as a three-dimensional body of a quadrilateral. The polyhedron can be a regular polyhedron such as a regular hexahedron, but is not limited thereto. One of the preferred three-dimensional shapes is a rod-shaped column (hereinafter, this shape is referred to as "rod-shaped") with a height of more than 2 times, further more than 3 times, and particularly more than 4 times the diameter of a circle when the bottom surface is regarded as a circle of the same area. But not limited thereto, the column can also be a disc-shaped column (hereinafter, this shape is referred to as "disc-shaped") with a height of less than 1 / 2 times, further less than 1 / 3 times, and particularly less than 1 / 4 times the diameter of a circle when the bottom surface is regarded as a circle of the same area. The three-dimensional shape of semiconductor nanoparticles can be a rod and / or a disc.

[0064] The semiconductor nanoparticles may include at least one selected from oxides, sulfides, selenides and tellurides, or may include at least one selected from sulfides, selenides and tellurides, or may be sulfides and / or selenides. However, for applications requiring durability such as heat resistance, semiconductor nanoparticles generally comprising oxides are suitable.

[0065] Figure 1 An example of a conductive film is shown in . A conductive film 1 is formed on a surface 7 a of a substrate 7 . Figure 1 This is a film cross section when the conductive film 1 is cut in a direction perpendicular to the surface 7a. Figure 2 Schematic diagram of the semiconductor nanoparticles 11 and 12 included in the conductive film 1 is shown in FIG. Figure 2The shape and arrangement of the semiconductor nanoparticles 11 and 12 shown can be observed using TEM, for example. The minimum diameter of the semiconductor nanoparticles 11 and 12 is less than 1 μm, for example, less than 500 nm, preferably less than 100 nm. In this embodiment, an insulating material is present in the matrix 40 where the semiconductor nanoparticles 11 and 12 are not present.

[0066] exist Figure 2 Semiconductor nanoparticles 11 and 12 appear in the film cross section of the conductive film 1 shown. The semiconductor nanoparticle 11 in the film cross section is substantially a polygon with more than 5 vertices, specifically a pentagon or a hexagon. The semiconductor nanoparticle 12 in the film cross section is substantially a quadrilateral. More specifically, the semiconductor nanoparticle 12 in the film cross section is a rectangle, more specifically, a rectangle whose long side corresponding to the bottom is more than twice the short side corresponding to the height. The semiconductor nanoparticles 11 and 12 observed in this way are, for example, disc-shaped. However, the shape of the semiconductor nanoparticles in the film cross section is not limited to the above shapes, and may also be a circle, an ellipse, a triangle, or a quadrilateral other than a rectangle, such as a square.

[0067] When the semiconductor nanoparticle 12 that appears in the film cross section is rectangular, the length of the long side of the rectangle is, for example, 3 to 2000 nm, further 5 to 900 nm, further 10 to 50 nm. The length of the short side of the semiconductor nanoparticle 12 is, for example, 2 to 100 nm, further 3 to 20 nm. The ratio of the length of the long side to the short side of the semiconductor nanoparticle 12 may be, for example, 2 or more.

[0068] The conductive film 1 includes arrangement parts 21, 22, 23 and 24 in which semiconductor nanoparticles 11 and 12 are arranged. In the arrangement parts 21 to 24, the semiconductor nanoparticles are arranged in a row without contacting adjacent particles. In the arrangement parts 21 and 22, semiconductor nanoparticles 11 that are substantially pentagonal or hexagonal are arranged, and in the arrangement parts 23 and 24, semiconductor nanoparticles 12 that are substantially rectangular are arranged. The number of semiconductor nanoparticles arranged in the arrangement part is not particularly limited, and 3 or more, 7 or more, 10 or more, or 20 or more semiconductor nanoparticles may be arranged.

[0069] In the arrangement sections 21 to 24, a straight line can be drawn through the semiconductor nanoparticles contained in each arrangement section. In other words, each arrangement section is arranged along the arrangement direction as a straight line. Figure 2 Only the arrangement directions 33 and 34 of the arrangement parts 23 and 24 are shown, and other arrangement directions are omitted. Figure 2 In the film cross section, there are also arranged portions of semiconductor nanoparticles other than those shown in the figure, but they are omitted for simplicity.

[0070] In the arrangement portions 23 and 24, adjacent semiconductor nanoparticles 12 are separated in a manner that the sides opposite to each other are substantially parallel. In such an arrangement portion, the average spacing between adjacent semiconductor nanoparticles 12 is easily kept small. The gaps between semiconductor nanoparticles are usually insulating, so the arrangement of semiconductor nanoparticles with small spacing is conducive to achieving high conductivity. In addition, in the arrangement portions 23 and 24, the opposite sides of adjacent semiconductor nanoparticles 12 are the long sides of a rectangle. In an arrangement structure with relatively long opposite sides, even if there is a local disorder in the arrangement of the semiconductor nanoparticles 12, it is easy to keep the parts close to the semiconductor nanoparticles 12, and it is easy to maintain the arrangement over a long distance. This feature is also conducive to achieving high conductivity.

[0071] The average spacing of semiconductor nanoparticles is, for example, 10 nm or less, further 7 nm or less, and in some cases 5 nm or less, preferably 3 nm or less, further preferably 2 nm or less, and particularly preferably 1.8 nm or less. The average spacing may be, for example, 0.3 nm or more, further 0.5 nm or more.

[0072] Figure 3 and 4 2 shows another example of a cross section of a conductive film. In the cross section of the conductive film 2, only semiconductor nanoparticles 13 that are substantially pentagonal or hexagonal appear. In the cross section of the conductive film 3, only semiconductor nanoparticles 14 that are substantially rectangular appear. Figure 4 In the arrangement parts 25, 26, 27, 28 and 29 extending along the arrangement directions 35, 36, 37, 38 and 39 which are substantially parallel to each other, the semiconductor nanoparticles 14 of rectangular shape are arranged. In addition, in the arrangement parts 61, 62, 63 and 64 extending along the arrangement directions 71, 72, 73 and 74 which are substantially non-parallel to the arrangement directions 35 to 39 and substantially parallel to each other, the semiconductor nanoparticles 14 of substantially rectangular shape are also arranged. Figure 4 In the film cross section, there are a plurality of substantially rectangular arrangement portions of semiconductor nanoparticles. In these arrangement portions, the semiconductor nanoparticles 14 are separated and adjacent in a manner that the opposite sides are substantially parallel to each other, and are arranged in a row over a long distance. Such a film cross section is advantageous in that the conductivity in the in-plane direction is sufficiently improved.

[0073] However, it should be noted that no rectangular semiconductor nanoparticles were observed in the film cross section ( Figure 3 ) of the conductive film 2 in different film cross sections, for example Figure 3In the direction perpendicular to the paper surface, rectangular arrangement of semiconductor nanoparticles can also be observed. For example, a film in which the three-dimensional shape of semiconductor nanoparticles 13 is disk-shaped and adjacent particles in the height direction are separated from each other and arranged with their bottom surfaces facing each other can have the following shapes depending on the cutting direction: Figure 4 Membrane cross section shown.

[0074] It should be noted that Figures 2 to 4 , all semiconductor nanoparticles 11 to 14 are separated from each other, but in this embodiment, as long as the arrangement portion in which the semiconductor nanoparticles are separated from each other is included, a part of the semiconductor nanoparticles may be in contact with each other in other parts. It should be noted that even if they are actually separated, the semiconductor nanoparticles may be observed in contact or overlapped depending on the direction of observation, the resolution of the instrument used in the observation, etc.

[0075] Figure 8 and Fig. 9 The example shows the ratio Figures 2 to 4 The arrangement state of semiconductor nanoparticles in a wider area. As shown in these figures, the arrangement parts of semiconductor nanoparticles do not need to extend in the same direction. The path composed of multiple arrangement parts can be bent, curved, intersected or partially overlapped. The path composed of multiple arrangement parts forms a conductive path.

[0076] The conductive films 1 to 3 contain a matrix 40 in which the semiconductor nanoparticles 11 to 14 are not present. The matrix 40 includes a binder and other materials described later. The binder and other materials are also sandwiched between the semiconductor nanoparticles adjacent to each other in the arrangement portion. It should be noted that the materials constituting the matrix 40 may be entirely insulating, or at least partially conductive.

[0077] The matrix 40 constitutes an element that allows the autonomous arrangement of the semiconductor nanoparticles 11 to 14. The proper arrangement of the semiconductor nanoparticles 11 to 14 makes the conductivity of the conductive films 1 to 3 anisotropic, and at least in a specific direction, the conductivity can be improved to a practical level. The matrix 40 can also be an element that helps to improve the light transmittance of the conductive films 1 to 3. The matrix 40 can also be an element that suppresses the decrease in the conductivity of the conductive films 1 to 3 caused by bending. In the cross-section of the arrangement portion formed by the arrangement of semiconductor nanoparticles, the matrix 40 without semiconductor nanoparticles can account for more than 20%, more than 30%, and further more than 40% of the whole, and can also be less than 90%, and further less than 80%.

[0078] The conductive films 1 to 3 preferably contain a compound attached to the semiconductor nanoparticles 11 to 14. The compound may also be sandwiched between the semiconductor nanoparticles adjacent to each other in the arrangement portion. In order to keep the interval between the semiconductor nanoparticles narrow, the molecular weight of the compound is preferably small. However, the compound attached to the semiconductor nanoparticles can be removed or reduced after film formation, for example, by heating. In particular, compounds with a small molecular weight, such as hydrazine, tend to disappear from the conductive film over time by so-called volatilization, even if they are not intentionally heated.

[0079] The conductivity C1 of the conductive film is 7S / cm or more, further 10S / cm or more, preferably 20S / cm or more, more preferably 50S / cm or more, further preferably 100S / cm or more, particularly preferably 150S / cm or more, and depending on the circumstances, 180S / cm or more. The conductivity C1 can be measured along at least one direction. The direction can be the film surface direction parallel to the surface of the film, or the film thickness direction perpendicular to the surface of the film. The high conductivity of the conductive film is mostly required in a specific direction in practice. For example, in an extremely thin conductive film, the length in the film surface direction is particularly large compared to the film thickness. Therefore, in most cases, if the conductivity in the film surface direction is increased, practical problems can be substantially solved.

[0080] From the above, it can be understood that the conductivity of the conductive films 1 to 3 may have anisotropy caused by the arrangement state of the semiconductor nanoparticles. The conductive film of this embodiment may be a film having a conductivity C1 measured along a first direction and a conductivity C2 lower than the conductivity C1 measured along a second direction. When the first direction is the film surface direction, the second direction may be the film thickness direction. When the first direction is the film thickness direction, the second direction may be the film surface direction.

[0081] The conductivity C2 may be, for example, less than 10% of the conductivity C1, less than 1%, further less than 0.1%, particularly less than 0.001%, or less than 0.0001% in some cases. However, by properly arranging the semiconductor nanoparticles or by narrowing the intervals between the semiconductor nanoparticles, not only the conductivity C1 but also the conductivity C2 may be increased. The conductivity C2 may be, for example, 2×10 -5 S / cm or more, and can be further 1×10 -4 S / cm or more, especially 1×10 -3 S / cm or more, depending on the situation, it can be 1×10 -2 S / cm or more, and can be further 1×10 -1 S / cm or more, and in particular, 1 S / cm or more. However, the conductive film of this embodiment does not necessarily have significant anisotropy of conductivity.

[0082] The disordered arrangement of semiconductor nanoparticles will hinder the realization of the above-mentioned conductivity. In order to prevent the disordered arrangement, for example, it is preferable that a compound that can adhere to semiconductor nanoparticles is sufficiently contained in the dispersion used as the conductive ink for forming the conductive film. In the film with disordered arrangement of semiconductor nanoparticles, not only the conductivity C1 but also the conductivity C2 tends to decrease.

[0083] The directional dependence of the conductivity of the conductive film is at least affected by the affinity of the semiconductor nanoparticles to the surface of the substrate and the three-dimensional shape of the semiconductor nanoparticles. For example, the semiconductor nanoparticles with a disc-like three-dimensional shape are arranged on the surface of the substrate with low affinity for the semiconductor nanoparticles in a manner that the disc surface is roughly perpendicular to the surface of the substrate. The semiconductor nanoparticles are arranged on the surface of the substrate with high affinity for the semiconductor nanoparticles in a manner that the disc surface is roughly parallel to the surface of the substrate. In addition, for example, the semiconductor nanoparticles with a rod-like three-dimensional shape are arranged on the surface of the substrate with low affinity for the semiconductor nanoparticles in a manner that the axial direction of the rod (long axis direction) is roughly perpendicular to the surface of the substrate, in other words, arranged in a manner that the rod is upright relative to the surface. The semiconductor nanoparticles are arranged on the surface of the substrate with high affinity for the semiconductor nanoparticles in a manner that the axial direction of the rod is roughly parallel to the surface of the substrate, in other words, arranged in a manner that the rod is laid flat.

[0084] In order to control the directional dependence of the conductivity of the conductive film by the arrangement of semiconductor nanoparticles, the substrate used can be appropriately selected or the affinity of the surface of the substrate can be adjusted. For example, in order to arrange rod-shaped semiconductor nanoparticles on the surface of a substrate with low affinity for semiconductor nanoparticles in a manner such that the long axis direction of the rods is roughly parallel to the surface, a material with high affinity for semiconductor nanoparticles can be pre-coated on the surface of the substrate. This arrangement is suitable for the formation of a conductive film with a relatively high conductivity C1 in the film thickness direction.

[0085] The light transmittance of the conductive film at a wavelength of 650nm is, for example, 80% or more, further 85% or more, preferably 90% or more, and more preferably 92% or more. A conductive film having a light transmittance as high as this is sometimes referred to as a transparent conductive film. However, the light transmittance of the conductive film at the same wavelength can be about 50% to about 80%, and sometimes 60% or more is sufficient depending on the application. In addition, the light transmittance of the conductive film in the visible light region (the region of wavelengths 400 to 800nm) is preferably, for example, 50% or more as a whole. Thus, a substantially transparent conductive film can be obtained.

[0086] Similarly, the light transmittance of the conductive film at a wavelength of 550 nm is, for example, 80% or more, further 85% or more, preferably 90% or more, and more preferably 92% or more. The light transmittance of the conductive film at the same wavelength may be about 50% to about 80%, and sometimes 60% or more is sufficient depending on the application.

[0087] The thickness of the conductive film is not particularly limited and can be appropriately set depending on the intended use. For example, it is 5 to 5000 nm, 5 to 2000 nm, further 10 to 1000 nm, and particularly 100 to 800 nm.

[0088] The conductivity of the conductive film of this embodiment can have excellent folding resistance. In the conventional conductive film in which conductive elements are in contact with each other to form a conductive path, the conductivity is easily reduced by bending. For example, as described in Non-Patent Document 1 Figure 7 As disclosed in , the conductivity of the conductive film containing silver nanowires as conductive elements that are in contact with each other is mostly greatly reduced after being bent about 300 to about 400 times. In contrast, in the conductive film of this embodiment, the semiconductor nanoparticles as conductive elements form a conductive path while being separated from each other, so the conductivity is not easily reduced even if it is repeatedly bent. As described later, according to an example of the conductive film of this embodiment, the result that the conductivity does not greatly reduce even if it is repeatedly bent more than hundreds of times, and further 1000 times (refer to Fig.11 In order to prevent the conductivity of the conductive film containing silver nanowires from decreasing to this extent, it is necessary to melt and integrate the silver nanowires by photonic curing. Figure 7 As shown, even if photon sintering is performed, the conductivity of the silver nanowires decreases sharply when the silver nanowires are folded about 900 times or more. The conductive film of this embodiment has excellent folding resistance and is suitable for use in flexible devices.

[0089] When the conductive film of this embodiment is subjected to the following bending test, the resistance change rate calculated by (|R2-R1| / R1)×100 based on the resistivity R1 before the test and the resistivity R2 after the test can be less than 30%, further less than 20%, and particularly less than 10%.

[0090] The bending test is a test as follows: the test piece formed with the above-mentioned conductive film is bent at a bending angle of 180° and a curvature radius of the bending portion of less than 5 cm, and further bent to the opposite side in the same manner, which is counted as one time and repeated 500 times, and repeated 800 times if necessary, and further repeated 1000 times. The curvature radius can usually be set to 5 cm. However, if a smaller bend can be performed, as a more stringent bending test, the curvature radius can be set to less than 5 cm, for example, 1 cm, and can be set to 5 mm depending on the situation.

[0091] It should be noted that the resistivity R1 used in the measurement is preferably 7 S / cm or more when converted into electrical conductivity.

[0092] like Fig.10 As shown, each time the bending test is performed, the test piece 100 is bent once to both sides. The curvature radius r of the bending portion 101 is determined by the deepest portion 102 of the bending portion 101. In the bent state, the ends 103 of the test piece 100 are kept parallel to each other at a bending angle of 180°.

[0093] The conductive film of this embodiment can have excellent weather resistance. For example, in a conductive film containing silver nanowires as conductive elements, if the conductive film is not covered with an outer coating, it will be oxidized and migrated in a high temperature and humid environment, thereby sharply reducing the conductivity. In contrast, the conductive film of this embodiment uses semiconductor nanoparticles as conductive elements, so even when the surface of the film is exposed to a high temperature and humid atmosphere, its conductivity is not easily affected.

[0094] <Composition of Conductive Film>

[0095] (Semiconductor Nanoparticles)

[0096] The semiconductor nanoparticles preferably contain a compound semiconductor, specifically at least one selected from oxides, sulfides, selenides and tellurides. The semiconductor nanoparticles may also be composed of a semiconductor equivalent to a metal compound. In addition, trace components, particularly components called dopants for improving conductivity, may be added to the semiconductor nanoparticles.

[0097] Preferred oxides include indium oxide, zinc oxide, tungsten oxide, molybdenum oxide, cadmium oxide, copper oxide, vanadium oxide, and gallium copper oxide. Preferred sulfides include copper sulfide and copper indium sulfide. Preferred selenides include copper selenide. Preferred tellurides include copper telluride.

[0098] Semiconductor nanoparticles may be crystalline or amorphous. When containing crystals, their crystal structure sometimes affects their conductivity. In addition, the type of crystal also affects the three-dimensional shape of semiconductor nanoparticles. Depending on the type of semiconductor nanoparticles, the preferred crystal structure is different. For example, copper sulfide preferably contains at least one selected from the group consisting of covellite, anilite, roxybite, digenite and djuleite, and particularly preferably contains covellite and / or digenite. Nanoparticles containing copper sulfide may contain only at least one crystal selected from the above.

[0099] The semiconductor nanoparticles preferably have a three-dimensional shape of a local ordered structure brought about by autonomous arrangement. Specifically, the three-dimensional shape is a shape having a cross section with substantially parallel opposite sides, typically a columnar body and / or a polyhedron. An example of a three-dimensional shape is a columnar body whose bottom surface is a circle, an ellipse or a polygon or can be approximated to any of them. The shape can be the above-mentioned rod-like shape or a disk-like shape.

[0100] The content of the semiconductor nanoparticles in the conductive film is not particularly limited, and is, in terms of mass %, for example, 5 to 98%, further 10 to 50%, and preferably 20 to 40%.

[0101] (Adhesive)

[0102] The conductive film may also contain a binder while containing semiconductor nanoparticles. The binder is a preferred constituent element sandwiched between semiconductor nanoparticles and capable of imparting flexibility to the conductive film. The binder may also contribute to improving the film-forming properties of the conductive film, the proper arrangement of nanoparticles, and the like.

[0103] The adhesive preferably comprises an attachment compound attached to the semiconductor nanoparticles. The attachment compound may comprise a functional group that can be combined with the semiconductor nanoparticles, for example, selected from at least one of fluoride (F), chloride (Cl), bromide (Br), iodide (I), cyanide (CN), thiocyanide (SCN), isothiocyanate (NCS), hydroxide (OH), sulfhydryl (SH), carbonyl (CO), amino (NR3), nitroso (NO), nitroso (NO2), phosphine (PR3), carbene (R2C) and pyridine (NC5H5). Here, R is independently an organic residue or a hydrogen atom. It can be understood from the above examples that the functional group that can be combined with the semiconductor nanoparticles can be other functional groups that can act as a ligand of a metal atom or an anion.

[0104] The attachment compound may be an inorganic compound or an organic compound. In addition, the attachment compound may be a salt containing the functional groups exemplified above or composed of ions composed of functional groups and their counterions. The attachment compound may be a compound having multiple of the above functional groups, represented by hydrazine (H2NNH2), ethylenediamine (H2NCH2CH2NH2), ethanedithiol (HSCH2CH2SH), mercaptopropionic acid (HSCH2CH2COOH), acetylacetone (H3CCOCHCOCH3), aminobenzonitrile (NH2C6H4CN), etc.

[0105] The molecular weight of the attachment compound is, for example, 300 or less, preferably 200 or less, more preferably 100 or less, further preferably 80 or less, and in some cases less than 60. The lower limit of the molecular weight is not particularly limited, and is, for example, 20 or more, further 30 or more. The use of an attachment compound with a molecular weight that is not too large is suitable for controlling the interval between semiconductor nanoparticles to be narrow.

[0106] The content of the attached compound in the conductive film can be appropriately adjusted according to its type, and is expressed as the ratio of the mass of the attached compound to the total amount of the semiconductor nanoparticles and the attached compound, for example, it can be 1% or more, further can be 2% or more, especially can be 3% or more, depending on the situation can be 5% or more, preferably 8% or more. The upper limit of the content is not particularly limited, but is 30% or less, and further 20% or less.

[0107] As the binder, materials other than the above-mentioned adhesion compounds can be used. Examples of such compounds include various resins, specifically polyvinyl alcohol, polyvinyl acetal, polyvinyl pyrrolidone, carboxymethyl cellulose, acrylic resins, polyvinyl acetate, polyethylene terephthalate, polystyrene, polyethylene, etc. In addition, pH adjusters, colorants, thickeners, surfactants, etc. can also be used depending on the necessity and purpose of the conductive film.

[0108] <Device>

[0109] The conductive film of the present invention is suitable for use in various devices, especially devices using a conductive film having light transmittance. Examples of such devices include photovoltaic devices represented by solar cells, image display devices represented by liquid crystal displays and organic EL displays, heating devices represented by heated windshields, and electromagnetic shielding devices represented by electromagnetic shielding windows and heat shielding windows. In these devices, the conductive film is used as an electrode film, an antistatic film, a heating film, an electromagnetic shielding film, and the like. By using a highly transparent conductive film for the above-mentioned purposes, advantages such as not hindering the design of the product, not hindering information communication, and being able to achieve invisibility can be obtained.

[0110] In the above device, at least one electrode is sometimes arranged in contact with the conductive film for the purpose of conducting electricity or releasing electric charge. Figure 5 and Figure 6 In. Figure 5 In the example shown, a pair of electrodes 51 and 52 are arranged in a manner separated in the film surface direction of the conductive film 4. By applying a potential difference to the electrodes 51 and 52, a current flows in the film surface direction of the conductive film 4. The conductive film can function as a heating film, for example. The electrodes 51 and 52 do not need to be formed on the surface 7a of the substrate 7, and can be formed on the surface 4a of the conductive film 4. It should be noted that if it is not for heat generation but for releasing charge from the conductive film to prevent static electricity, only one electrode is sufficient.

[0111] exist Figure 6 In the example shown, the conductive film 4 in contact with the electrode 53 is used as a light-transmitting electrode. For example, when light 9 transmitted from the conductive film 4 is incident on the functional film 8, a potential difference is generated between the electrodes 53 and 54 by the photoelectric conversion function of the functional film 8. In another device, when a potential difference is applied between the conductive film 4 and the electrode 54, the functional film 8 is subjected to a voltage drop in the film thickness direction ( Figure 6 When a voltage is applied to the functional film 8, the functional film 8 emits light in the direction opposite to the incident light 9. Figure 6 In the example, a transparent substrate such as a glass plate or a transparent resin plate can be used as the substrate 7, and a metal film such as aluminum can be used as the electrode 54. However, the examples of the substrate 7 and the electrode 54 are not limited thereto. For example, the substrate 7 may also be a substrate having a thin film on the surface.

[0112] exist Figure 6 In the manner shown, the electrode 53 is arranged in a direction perpendicular to the paper surface ( Figure 6 In this case, in order to reduce the difference in potential within the conductive film 4 caused by the distance from the electrode 53, the conductive film 4 preferably has a high conductivity C1 at least in the film surface direction (x direction) perpendicular to the direction in which the electrode extends.

[0113] exist Figure 6 In the illustrated embodiment, when viewed from the z direction perpendicular to the film surface of the conductive film 4, the area S1 of the region where the electrode 53 overlaps with the conductive film 4 is less than 1 / 2, that is, less than 50%, of the area S2 of the conductive film 4. The ratio of the area S1 to the area S2 may be, for example, 30% or less, further 20% or less, and may be 10% or less depending on the circumstances.

[0114] However, the shape and configuration of the electrodes in the device are not limited to Figure 5 and Figure 6 .

[0115] In order to utilize the excellent folding resistance of the conductive film, the present embodiment also provides a flexible device. The flexible device, for example, also has a substrate supporting the conductive film, and can be bent without damage at a bending angle of 180° and a curvature radius of the bending portion of less than 5 cm, for example, 1 Gm, and 5 mm depending on the situation. In such a device, soft substrates such as fabrics, non-woven fabrics, paper, and films are suitable. In the device of the present embodiment, the resistance change rate of the conductive film measured by the above-mentioned bending test can be less than 30%, further can be less than 20%, and in particular can be less than 10%. However, the device of the present embodiment may also be a rigid device that lacks flexibility.

[0116] As described above, in this embodiment mode, the conductive film can have excellent durability. In order to utilize this characteristic, in the device of this embodiment mode, at least a portion of the conductive film can be exposed.

[0117] <Dispersion>

[0118] The dispersion used in the formation of the conductive film is sometimes referred to as conductive ink. According to this convention, in this specification, the dispersion is sometimes also described as conductive ink below. From the above, it can be understood that the conductive ink itself does not need to have conductivity. The dispersion as a conductive ink contains a dispersion medium, semiconductor nanoparticles dispersed in the dispersion medium, and a first compound, the first compound exists in the form of an attached compound attached to the above-mentioned semiconductor nanoparticles and a free compound free from the above-mentioned semiconductor nanoparticles, and satisfies at least one of the following i) to iv). The dispersion preferably satisfies at least i). The dispersion may also satisfy all of i) to iv).

[0119] i) The ratio of the amount of the first compound existing in the form of a free compound to the amount of the first compound existing in the form of an attached compound is 1 or more.

[0120] ii) The ratio of the amount of the first compound to the total amount of the semiconductor nanoparticles and the first compound is 10% or more on a mass basis.

[0121] iii) The semiconductor nanoparticles include at least one selected from oxides, sulfides, selenides, and tellurides.

[0122] iv) The semiconductor nanoparticles are columnar and / or polyhedral.

[0123] The conductive ink contains a dispersion medium, semiconductor nanoparticles dispersed in the dispersion medium, and a first compound. A portion of the first compound is contained in the conductive ink in the form of an attached compound attached to the semiconductor nanoparticles, and the remainder of the first compound is contained in the conductive ink in the form of a free compound freed from the semiconductor nanoparticles. The first compound may be the same as the second compound that should be attached to the semiconductor nanoparticles in the conductive film, but is preferably a different compound. This is because the preferred compound for improving the conductivity in the conductive film is not necessarily the same as the preferred compound for forming a conductive film in which semiconductor nanoparticles are properly arranged by the conductive ink. As the first compound, a compound suitable for stably dispersing semiconductor nanoparticles in the ink and for autonomously arranging semiconductor nanoparticles during the formation of the conductive film can be used. The second compound can be introduced into the conductive film by replacing the first compound after film formation.

[0124] The autonomous arrangement of semiconductor nanoparticles can be achieved by using the interaction between semiconductor nanoparticles, specifically electrostatic force, van der Waals force, dipole force, dispersion force, etc. as a driving force. By using these as a driving force, as the dispersion medium is removed from the applied ink, the semiconductor nanoparticles can be arranged in a self-controlled manner in a state sandwiched between the first compound.

[0125] The first compound may be an inorganic or organic compound, particularly an organic compound, containing at least one, or more than one, of the functional groups exemplified above, as well as the second compound already described as an attachment compound. However, it is preferred that the molecular weight of the first compound is greater than that of the second compound. The molecular weight of the first compound is preferably 2000 or less, more preferably 1000 or less, and further preferably 500 or less, for example 60 to 300. When the first compound is a salt, the molecular weight of the first compound is also calculated based on the above method.

[0126] The content of the first compound in the conductive ink can be appropriately adjusted according to its type, but expressed as the ratio of the mass of the first compound to the total mass of the semiconductor nanoparticles and the first compound, it is preferably 10% or more, 15% or more, 16% or more, 17% or more, particularly preferably 18% or more, and depending on the circumstances, it can be 20% or more, 25% or more, 28% or more, and particularly 30% or more. The upper limit of this ratio is not particularly limited, for example, it can be 90% or less, or 86% or less, or 75% or less depending on the circumstances. In order to arrange the semiconductor nanoparticles autonomously and appropriately in the film after film formation, it is preferred to add more of the first compound than when only the semiconductor nanoparticles are stably dispersed in the ink. For a conductive film formed by a conductive ink with insufficient first compound, its conductivity is mostly insufficient.

[0127] In order to properly arrange the semiconductor nanoparticles, it is preferred that the conductive ink contains an appropriate amount of the first compound in the form of a free compound. It is believed that when the amount of the free compound is lower than the appropriate range, even if the semiconductor nanoparticles can be ensured to be dispersed in the conductive ink, sometimes a very small part of the agglomeration will occur. This agglomeration may be the cause of hindering the proper arrangement of the semiconductor nanoparticles in the conductive film. The state attached to the semiconductor nanoparticles is generally relatively stable compared to the free state, so the range of the amount of the appropriate free compound can be expressed by the ratio relative to the attached compound, specifically the mass ratio or the molar ratio. The ratio of the amount of the first compound contained in the form of a free compound to the amount of the first compound contained in the form of an attached compound is preferably 1 or more, 2 or more, 3 or more, 4 or more, 5 or more, 6 or more, 7 or more, particularly preferably 8 or more, and can be 10 or more depending on the circumstances. The upper limit of the ratio is not particularly limited, for example, it is less than 100, it can be less than 50, and it can be further less than 30, and it can be less than 28 depending on the circumstances, and it can be further less than 27.

[0128] The dispersion of semiconductor nanoparticles sometimes contains impurities from the raw materials used to synthesize semiconductor nanoparticles, additives added for synthesis, etc. Impurities are typically unreacted raw materials. In order to remove these impurities, a solvent can be added and the impurities can be removed together with the solvent. As such a solvent, a polar solvent, particularly a polar organic solvent, can be used. It should be noted that, as described later, a non-polar organic solvent or a low polarity polar organic solvent is usually used as a dispersion medium. The removal of impurities can be implemented, for example, by a method comprising the following steps.

[0129] Addition of solvent: A step of mixing a stock solution containing a dispersion medium, semiconductor nanoparticles dispersed in the dispersion medium, the first compound, and impurities with a solvent to obtain a mixed solution.

[0130] Application of centrifugal operation: The process of applying centrifugal operation to the mixed liquid at a specified rotation speed.

[0131] Removal of solvent: a step of removing the solvent together with at least a part of the impurities from the mixed liquid after the centrifugation operation.

[0132] When the rotation speed of the centrifugal operation is too high, the amount of the first compound removed together with the solvent increases. Therefore, the rotation speed of the centrifugal operation is preferably less than 5000rpm, and particularly preferably in the range of 500 to 4000rpm. For the same reason, the centrifugal operation is preferably carried out under the condition that the temperature of the mixed solution is near room temperature, specifically in the range of 10 to 30°C. It should be noted that for polar solvents, poor solvents for semiconductor nanoparticles are suitable, and when the dispersion medium is a polar solvent, a polar solvent with a higher polarity than the dispersion medium is suitable. As a polar solvent, specifically, a low boiling point solvent, such as water or a polar organic solvent such as alcohol having 1 to 4 carbon atoms, acetone, etc. is suitable. In addition, there is no particular restriction on the number of applications of the centrifugal operation, and it is preferably about 2 to 3 times.

[0133] Separately from the above-mentioned conductive ink (when it is set with the second ink described later, it is sometimes referred to as "first ink"), it is preferable to prepare an ink containing a second compound to replace the first compound (hereinafter sometimes referred to as "second ink"). The ink set including the first ink and the second ink facilitates the formation of a conductive film. The ink set includes, for example, a first ink, a first container for storing the first ink, a second ink, and a second container for storing the second ink. As described above, the first compound and the second compound are a combination of compounds in which the molecular weight of the latter is smaller than the molecular weight of the former.

[0134] The conductive ink (first ink) and the second ink may contain a pH adjuster, a cosolvent, and other components. The other components may be the above-mentioned components that may be contained in the conductive film, or may be volatile components that do not remain in the conductive film.

[0135] The preferred forms of the shapes, crystals, etc. of the semiconductor nanoparticles are as described above. The content of the semiconductor nanoparticles in the conductive ink (first ink) is not particularly limited, and is expressed in mass %, for example, 1 to 70%, further 5 to 50%, and preferably 10 to 20%. The dispersion medium in the conductive ink (first ink) is not particularly limited as long as it can disperse the semiconductor nanoparticles, and is preferably an organic solvent such as toluene, hexane, octane, chloroform, etc. The solvent of the second ink is not particularly limited as long as it can dissolve the second compound, and a solvent corresponding to the type of the second compound can be used.

[0136] <Method for producing conductive film>

[0137] The method for manufacturing a conductive film of this embodiment includes the following first step and second step in sequence. After the second step is performed, the following third step and fourth step may be performed. If the desired film thickness is not achieved, the third step and fourth step may be performed repeatedly two or more times. When the above-mentioned ink set is used, the first ink is used as the conductive ink, and the second ink is used as the solution containing the second compound.

[0138] (First step)

[0139] In the first step, a conductive ink containing semiconductor nanoparticles and a first compound is applied onto the surface of a substrate to form a coating film.

[0140] (Second step)

[0141] In the second step, a solution containing the second compound is brought into contact with the coating film formed in the first step to replace at least a portion of the first compound with the second compound, thereby obtaining a conductive film.

[0142] (Third step)

[0143] In the third step, a conductive ink is applied onto the surface of the formed conductive film, thereby forming an additional coating film.

[0144] (Step 4)

[0145] In the fourth step, a solution containing the second compound is brought into contact with the formed additional coating film to replace at least a portion of the first compound contained in the additional coating film formed in the third step with the second compound, thereby obtaining a thicker conductive film.

[0146] The coating of the conductive ink or solution in each step can be carried out by a known coating method such as spin coating, roll coating, flow coating, dip coating, etc.

[0147] Hereinafter, the present invention will be further described by way of examples, but the following description is not intended to limit the present invention to specific examples.

[0148] (Example A1)

[0149] ·Production of conductive ink

[0150] 1.891 g of copper acetate, 1.13 g of 1,3-dibutyl-2-thiourea and 10 ml of oleylamine were added to a three-necked flask, and nitrogen substitution was performed while stirring. Next, the liquid temperature was raised to 80° C. using a heating jacket and maintained for 1 hour. Then, when the liquid temperature dropped to 40° C., 40 ml of chloroform was slowly added to the three-necked flask to dissolve the solid components.

[0151] The contents of the three-necked flask were transferred to a centrifuge tube, and after confirming that the solid components in the centrifuge tube were fully dissolved, 40 ml of ethanol was added. The centrifuge was further performed at 2000 rpm (revolutions / minute) for 10 minutes, and the supernatant was directly discarded. Next, the precipitate was dissolved in 5 ml of octane, and then 30 ml of ethanol was added again, and the centrifuge was performed again at a speed of 2000 rpm for 5 minutes to collect the precipitate. The mass of the precipitate was measured, and based on this, octane was added in a manner to become 200 mg / ml to disperse the copper sulfide nanoparticles, thereby obtaining a conductive ink.

[0152] The conductive ink contains oleylamine as a compound capable of coordinating with the copper sulfide nanoparticles together with the copper sulfide nanoparticles. When the precipitate is analyzed by thermogravimetric analysis (TGA), the ratio of the mass of oleylamine to the total mass of the copper sulfide nanoparticles and oleylamine is 10%. It should be noted that this ratio is also the same in the following examples.

[0153] ·Conductive film formation

[0154] On a glass plate on which comb-shaped electrodes were preformed, 50 μl of conductive ink (first ink) was applied using a spin coater to obtain a coating film. It should be noted that during the coating, the concentration of the conductive ink was adjusted to 50 mg / ml. The glass plate on which the comb-shaped electrodes were formed used a commercial product (manufactured by Drop Sens, G-IDEU5) with an electrode width and electrode spacing of 5 μm or 10 μm, a pair number of electrodes of 250 (when the electrode width is 5 μm) or 125 (when the electrode width is 10 μm), and a column length of 6760 μm.

[0155] A 200 μl solution (second ink) containing KSCN as an adhesion compound was applied to the coating film using a spin coater to obtain a conductive film. The solvent of the solution was octane, and the concentration of KSCN was 10% by mass. By contacting with the second ink, at least a portion of the compound coordinated with the copper sulfide nanoparticles was replaced from oleylamine (first compound) to KSCN (second compound).

[0156] An additional coating film is formed on the conductive film by the same film formation as the above film formation using the first ink, and then the compound is replaced in the same manner as above using the second ink. Thus, a conductive film with increased film thickness is obtained.

[0157] (Examples A2 to A4)

[0158] A conductive film was produced in the same manner as in Example A1 except that the second compound in the second ink to be the adhesion compound was set to the compound shown in Table 1. At this time, the number of repetitions n (n=2 in Example A1) of coating for thickening the film was also set to the number shown in Table 1.

[0159] (Examples A5 to A8)

[0160] ·Production of conductive ink

[0161] 0.246 g of copper acetate and 20 ml of oleylamine are added to three-necked flask A, and the mixture is evacuated while being stirred. Next, flask A is heated using an oil bath to raise the liquid temperature to 160°C, and maintained in this state for 1 hour. The heating rate is set to 8°C / min. On the other hand, 0.096 g of sulfur and 30 ml of 1-octadecene are added to another three-necked flask B, and the mixture is repeatedly evacuated and replaced with a nitrogen atmosphere while being stirred, and then nitrogen is flowed in and maintained in a nitrogen atmosphere. Next, flask B is heated using an oil bath to raise the liquid temperature to 160°C, and sulfur is dissolved. The heating rate is set to 5°C / min. Flask B is left for 1 hour, and then nitrogen is flowed in and maintained in a nitrogen atmosphere.

[0162] Transfer the contents of flask A to a centrifuge tube, add the contents of flask B to the centrifuge tube using a syringe, and keep for 10 minutes. Then turn off the heater, and after the liquid temperature drops to 40°C, add about 30 ml of hexane to the centrifuge tube. Next, after visually confirming that the generated solid component has dissolved, add 30 ml of ethanol, centrifuge at 2000 rpm for 5 minutes, and collect the precipitate. Next, dissolve the precipitate in 5 ml of octane, then add 30 ml of ethanol again, centrifuge at 2000 rpm for 5 minutes again, and collect the precipitate. The mass of the precipitate is measured, and based on this, octane is added in a manner to become 200 mg / ml to disperse the copper sulfide nanoparticles, thereby obtaining a conductive ink.

[0163] ·Conductive film formation

[0164] A conductive film was produced in the same manner as in Example A1 except that the second compound in the second ink serving as the adhesion compound was set to the compound shown in Table 1. At this time, the number of repetitions n of coating for thickening the film was also set to the number shown in Table 1.

[0165] (Example A9)

[0166] 50.5 mg of copper chloride (CuCl2), 271.8 mg of copper nitrate (Cu(NO3)2 / 3H2O), 2.46 ml of oleylamine, 15 ml of 1-octadecene, and 6 ml of dodecanethiol were added to a three-necked flask, and vacuuming and replacement with nitrogen were repeated while stirring, and finally vacuuming was performed. Next, the three-necked flask was heated using a heating mantle to raise the liquid temperature to 100°C, and maintained in this state for 30 minutes. Next, while the liquid temperature was raised to 180°C, 10 ml of tert-dodecyl mercaptan was injected from a syringe, and the temperature was maintained at 180°C for 5 minutes, and then rapidly cooled with tap water.

[0167] Transfer the contents of the three-necked flask to a centrifuge tube, and add about 30 ml of hexane to the centrifuge tube. Next, visually confirm that the generated solid component has dissolved, add 15 ml of isopropanol and 15 ml of acetone, centrifuge at 2000 rpm for 5 minutes, and collect the precipitate. Next, dissolve the precipitate in 5 ml of octane, then add 30 ml of ethanol again, centrifuge at 2000 rpm for 5 minutes again, and collect the precipitate. Measure the mass of the precipitate, and based on this, add octane in a manner to become 200 mg / ml to disperse the copper sulfide nanoparticles, thereby obtaining a conductive ink. After the liquid temperature drops to 40°C, add about 30 ml of hexane to the centrifuge tube. Next, visually confirm that the generated solid component has dissolved, add 30 ml of ethanol, centrifuge at 2000 rpm for 5 minutes, and collect the precipitate. Next, the precipitate was dissolved in 5 ml of octane, and then 30 ml of ethanol was added again, and centrifugation was performed again at 2000 rpm for 5 minutes to collect the precipitate. The mass of the precipitate was measured, and based on the mass, octane was added to make it 200 mg / ml to disperse the copper sulfide nanoparticles, thereby obtaining a conductive ink.

[0168] ·Conductive film formation

[0169] A conductive film was produced in the same manner as in Example A1 except that the second compound in the second ink serving as the adhesion compound was set to the compound shown in Table 1. At this time, the number of repetitions n of coating for thickening the film was also set to the number shown in Table 1.

[0170] The conductivity and film thickness of the obtained conductive film were measured, and the crystal system of copper sulfide contained in the copper sulfide nanoparticles was measured by X-ray diffraction. In addition, the light transmittance of Examples A1 to A3 was also measured. The results are shown in Tables 1 and Figure 7 It should be noted that the light transmittance in Table 1 is the value at a wavelength of 650 nm.

[0171] [Table 1]

[0172]

[0173] ·R: pentathite, C: covellite; ·d: disk-shaped, r: rod-shaped

[0174] ·KSCN: Potassium thiocyanate (molecular weight is only SCN), MPA: Mercaptopropionic acid, BT: Benzenethiol, EDT: Ethylene dithiol, EDA: Ethylenediamine, ABN: Aminobenzonitrile

[0175] A conductive film was prepared on the surface of a glass plate with an ITO film in the same manner as in Example A5, and a gold electrode was locally deposited on the surface of the conductive film. The conductivity of the conductive film in the film thickness direction was measured and the result was 9×10 -5 S / cm. For the conductive films obtained from other embodiments, it can also be confirmed that the conductivity in the film thickness direction is lower than the conductivity in the film surface direction measured using the comb electrode, which is much lower than 1%. Regarding other embodiments, from the arrangement of nanoparticles, it is believed that the conductivity in the film thickness direction is also much lower than the conductivity in the film surface direction, which does not exceed 10%.

[0176] It should be noted that, when observed using TEM, it can be confirmed that the nanoparticles prepared in Example A9 have a rod-like shape and are arranged in a manner such that the long axis direction is facing a direction perpendicular to the surface of the substrate. On the other hand, it is confirmed that the nanoparticles prepared in Examples A1 to A8 have a disc-like shape and are arranged in a manner such that the disc surface is facing a direction perpendicular to the surface of the substrate. These grains are arranged close to each other in a manner such that the cross-section is substantially rectangular and the relative long sides are substantially parallel to each other. In addition, it can also be confirmed that the arrangement direction of the arrangement extends along the film surface direction. In addition, in any embodiment, the average spacing of the copper sulfide nanoparticles is less than 10nm. For example, when a conductive film is prepared in the same manner as in Example A5 on the surface of a glass plate having a comb-shaped electrode, the average spacing of the copper sulfide nanoparticles after replacement with EDT is 1.1nm.

[0177] The results of observing the conductive film formed from the conductive ink obtained in the same manner as above using TEM are shown in FIG. Figure 8 and Fig. 9 middle. Figure 8 and Fig. 9 This is an image obtained by observing the film surface of the conductive film.

[0178] As can be seen from Table 1, pentathite is a preferred crystal that can stably provide relatively high conductivity. As far as the inventors know, this is a view that was not known before. In addition, covellite is a crystal that can provide significantly improved conductivity when combined with a compound with a particularly small molecular weight. In other words, the conductivity obtained from covellite is easily affected by the attached compound.

[0179] (Example A10)

[0180] ·Conductive film formation

[0181] A conductive film is prepared on a borosilicate glass substrate in the same manner as in Example A1, except that the second compound in the second ink that will become the attached compound is set to hydrazine. At this time, the number of repetitions of the coating for thickening is 15 times. Then, it is cut into a size of 10 mm × 10 mm to prepare a measurement sample. Then, Au electrodes with a thickness of 100 to 200 nm are respectively set at the four corners of the surface of the measurement sample by vapor deposition. Then, the four terminals are respectively contacted with the Au electrodes formed at the four corners, and the sheet resistance of the measurement sample is measured by the Van Der Pauw method using a sheet resistance measuring device Resi Test8400 (manufactured by Toyo Technica). As a result of the measurement, the sheet resistance as the resistance in the film surface direction is 100Ω / □. That is, in a conductive film of a certain size close to practical application, performance almost the same as that of ITO (indium tin oxide) is obtained. Unlike ITO, which needs to be formed by vapor deposition, this conductive film can be formed by coating, so it is easier to manufacture and its superiority can be confirmed.

[0182] (Example B1)

[0183] A conductive ink was obtained in the same manner as in Example A5 except that octadecene was used instead of octane as the organic solvent added last to obtain the conductive ink. In the conductive ink, oleylamine was contained in the form of an attached compound attached to the copper sulfide nanoparticles and a free compound released from the copper sulfide nanoparticles. The ratio of the free compound to the attached compound in the conductive ink was determined as follows.

[0184] First, add 5 ml of conductive ink to a centrifugal tube, then add 45 ml of ethanol, and centrifuge at 2000 rpm for 10 minutes. Next, vacuum the resulting precipitate to remove the residual solvent, perform thermogravimetric analysis (TGA) on the resulting dried solid, and measure the amount of copper sulfide nanoparticles constituting the precipitate and the amount of oleylamine (attached compound) attached to the copper sulfide nanoparticles, respectively. It should be noted that the ratio of the amount of oleylamine (attached compound) to the total amount of copper sulfide nanoparticles and oleylamine (attached compound) is 10% by mass. On the other hand, an evaporator is used to remove only ethanol from the supernatant obtained by centrifugation, and the amount of oleylamine (free compound) freed from the copper sulfide nanoparticles is calculated based on the amount of liquid after the ethanol is removed and the ratio of the amount of oleylamine to the amount of octadecene added. When the ratio of the amount of free compound to the amount of attached compound is calculated based on the above, it is 21.4.

[0185] A conductive film was obtained in the same manner as in Example A5 except that the conductive ink of Example B1 was used. However, the film was formed so that the film thickness became 135 nm. The measured conductivity is shown in Table 2.

[0186] (Example B2)

[0187] The conductive ink prepared in Example A1 was subjected to a total of 2 impurity removal steps using centrifugal operation. However, from the viewpoint of removing impurities such as unreacted compounds, it is preferred to further repeat the centrifugal operation. In view of this, in Example B2, after applying two centrifugal operations under the same conditions as Example B1, a third centrifugal operation was performed under the same conditions as the second centrifugal operation. In addition, a conductive ink was obtained in the same manner as Example B1, and the ratio of free compounds to attached compounds was calculated using the obtained conductive ink in the same manner as Example B1, a conductive film was formed, and the conductivity was measured. The results are shown in Table 2.

[0188] (Comparative Example B3)

[0189] The conductive ink prepared in Example A1 is subjected to an impurity removal process using a centrifugal operation at a rotation speed of 2000 rpm. However, from the viewpoint of removing impurities, it is preferred to also apply a centrifugal operation with a higher rotation speed. Taking this into account, in Comparative Example B3, the conditions of the centrifugal operation were changed to 8000 rpm and 2 minutes, and a total of 3 centrifugal operations were performed. It should be noted that the second and third washings were performed by adding a mixed solution containing chloroform and ethanol at a ratio of 1:20. In addition, a conductive ink was obtained in the same manner as in Example B1, and the obtained conductive ink was used to determine the ratio of free compounds to attached compounds in the same manner as in Example B1, to form a conductive film and measure the conductivity. The results are shown in Table 2.

[0190] [Table 2]

[0191]

[0192] ·B3 is a comparative example; ·All compounds except particles: free compounds + attached compounds

[0193] In each conductive film obtained from Examples B1, B2 and Comparative Example B3, the conductivity in the film surface direction is also higher than the conductivity in the film thickness direction. In Comparative Example B3, it is believed that since the semiconductor nanoparticles are partially condensed in the conductive ink, when the conductive film as a whole is observed, the arrangement of the semiconductor nanoparticles partially disappears or becomes different. In such a film, sufficient conductivity cannot be obtained even in the direction where the conductivity is relatively high (the film surface direction in the above examples).

[0194] (Example C1)

[0195] A conductive film was obtained in the same manner as in Example A6 except that a PET plate with comb-shaped electrodes was used instead of a glass plate with comb-shaped electrodes and the number of coatings was set to 5. It should be noted that a commercially available product (DRIP-P-IDEAU100 manufactured by Drop Sens) was used as the PET plate with comb-shaped electrodes. Fig.10 As shown in FIG. 1 , a PET plate having a conductive film formed thereon was bent 1000 times so that the curvature radius of the bent portion was about 5 mm. The number of bendings was calculated by continuously performing bending with the conductive film on the inside and bending with the conductive film on the outside, and this combination was counted as one time. In addition, the resistivity of the conductive film was measured using a comb-shaped electrode every 50 bendings. Fig.11 The change in resistivity of the conductive film due to bending is shown in FIG. The change rate of resistivity is less than 10%.

[0196] (Example D1)

[0197] A conductive film was obtained in the same manner as in Example A6 except that anisidine (molecular weight 123.2) was used as the second compound in the second ink to be the adhesion compound. The resistance value was measured at the time of production and after one and a half years (13140 hours) or more had passed since the production, with the conductive film exposed. As a result, no increase in the resistivity of the conductive film was observed.

[0198] (Example D2)

[0199] The conductive film of Example A6 was exposed, and the resistance was measured at the time of manufacture and after one and a half years from the time of manufacture. The result was 44Ω at the time of manufacture, but it was 78Ω after one and a half years. Although the resistance value increased, it is considered that the increase in resistance value can be significantly suppressed compared with the silver nanowire without an outer coating.

Claims

1. A conductive film comprising an arrangement of semiconductor nanoparticles, When observing a cross section including the arrangement portion, in the arrangement portion, the semiconductor nanoparticles are arranged in a row in a state of being separated from each other. The electrical conductivity C1 measured in at least one direction is 7 S / cm or more, The average interval between the semiconductor nanoparticles is greater than or equal to 0.3 nm and less than or equal to 10 nm.

2. The conductive film according to claim 1, wherein In the cross section, the adjacent semiconductor nanoparticles in the array portion are separated such that sides facing each other are substantially parallel.

3. A conductive film containing semiconductor nanoparticles as conductive elements, The conductive element exhibits anisotropic conductivity, wherein the conductivity C1 measured along the first direction is 7 S / cm or more and the conductivity C2 measured along the second direction is less than 10% of the conductivity C1. Either the first direction or the second direction is a film surface direction, and the other is a film thickness direction. The average interval between the semiconductor nanoparticles is greater than or equal to 0.3 nm and less than or equal to 10 nm.

4. The conductive film according to claim 3, wherein The conductivity C2 is 2×10 -5 S / cm or more.

5. The conductive film according to claim 1 or 3, wherein: When the bending test is performed, the resistance change rate calculated by (|R2-R1| / R1)×100 based on the resistivity R1 before the test and the resistivity R2 after the test is 30% or less. Among them, the bending test is a test in which the following operation is counted as 1 time and repeated 500 times. The operation is: bending the test piece formed with the conductive film at a bending angle of 180° and a curvature radius of the bending portion of less than 5 cm, and further bending it to the opposite side in the same manner.

6. The conductive film according to claim 1 or 3, wherein: The three-dimensional shape of the semiconductor nanoparticles is a column and / or a polyhedron.

7. The conductive film according to claim 1 or 3, wherein: The semiconductor nanoparticles include at least one selected from the group consisting of oxides, sulfides, selenides, and tellurides.

8. The conductive film according to claim 1 or 3, wherein: The semiconductor nanoparticles include copper sulfide.

9. The conductive film according to claim 8, wherein The copper sulfide comprises covellite and / or pentahedrite.

10. A dispersion for producing the conductive film according to any one of claims 1 to 9, the dispersion comprising a dispersion medium, semiconductor nanoparticles dispersed in the dispersion medium, and a first compound, The first compound exists in the form of an attached compound attached to the semiconductor nanoparticle and a free compound freed from the semiconductor nanoparticle, The first compound has a functional group capable of binding to the semiconductor nanoparticles, The dispersion satisfies at least one of i) to iv): i) the ratio of the amount of the first compound present in the form of the free compound to the amount of the first compound present in the form of the attached compound is 1 or more; ii) the ratio of the amount of the first compound to the total amount of the semiconductor nanoparticles and the first compound is 10% or more on a mass basis; iii) the semiconductor nanoparticles comprise at least one selected from oxides, sulfides, selenides and tellurides; iv) The semiconductor nanoparticles are columnar and / or polyhedral.

11. The dispersion according to claim 10, which satisfies at least i).

12. The dispersion according to claim 11, which satisfies all of i) to iv).

13. The dispersion of claim 10, wherein When the dispersion is applied onto a substrate to form a coating film, the semiconductor nanoparticles are autonomously arranged, thereby forming an arrangement portion in which the semiconductor nanoparticles are arranged separately from each other in a cross section of the coating film.

14. The dispersion of claim 10, wherein The semiconductor nanoparticles include copper sulfide.

15. The dispersion of claim 14, wherein The copper sulfide comprises covellite and / or pentahedrite.

16. A method for producing a dispersion, which is the method for producing a dispersion according to any one of claims 10 to 15, comprising: mixing a stock solution containing a dispersion medium, semiconductor nanoparticles dispersed in the dispersion medium, a first compound, and impurities with a solvent to obtain a mixed solution; Applying centrifugal operation to the mixed solution at a rotation speed of less than 5000 rpm; as well as After the centrifugation operation, the solvent is removed from the mixed liquid together with at least a portion of the impurities.

17. An ink kit comprising: A first ink is a dispersion containing a dispersion medium, semiconductor nanoparticles dispersed in the dispersion medium, and a first compound, wherein the first compound exists in the form of an attached compound attached to the semiconductor nanoparticles and a free compound freed from the semiconductor nanoparticles; and a second ink comprising a second compound having a smaller molecular weight than the first compound, capable of replacing the first compound and attaching to the semiconductor nanoparticles, The first ink is the dispersion according to any one of claims 10 to 15.

18. The ink set of claim 17, wherein: The molecular weight of the second compound is less than 60.

19. A device comprising the conductive film according to claim 1 or 3, The conductive film is provided as at least one functional film selected from an electrode film, an antistatic film, a heating film and an electromagnetic shielding film, The device is a photovoltaic device, an image display device, a heating device or an electromagnetic shielding device.

20. A device comprising a conductive film containing semiconductor nanoparticles and at least one electrode in contact with the conductive film, The conductive film satisfies the following a) and / or b): a) comprising an arrangement portion of the semiconductor nanoparticles, When observing a cross section including the arrangement portion, in the arrangement portion, the semiconductor nanoparticles are arranged in a row in a state of being separated from each other. The electrical conductivity C1 measured in at least one direction is 7 S / cm or more, The average spacing of the semiconductor nanoparticles is greater than 0.3 nm and less than 10 nm; b) containing the semiconductor nanoparticles as conductive elements, The conductive element exhibits anisotropic conductivity, wherein the conductivity C1 measured along the first direction is 7 S / cm or more and the conductivity C2 measured along the second direction is less than 10% of the conductivity C1. Either the first direction or the second direction is a film surface direction, and the other is a film thickness direction. The average spacing between the semiconductor nanoparticles is greater than or equal to 0.3 nm and less than or equal to 10 nm. The device is a photovoltaic device, an image display device, a heating device or an electromagnetic shielding device.

21. The device of claim 19, wherein further comprising a substrate supporting the conductive film, The substrate can be bent without being damaged so that the bending angle is 180° and the curvature radius of the bent portion is 5 cm or less.

22. The device of claim 20, wherein: further comprising a substrate supporting the conductive film, The substrate can be bent without being damaged so that the bending angle is 180° and the curvature radius of the bent portion is 5 cm or less.

23. A method for manufacturing a conductive film, wherein: The conductive film is the conductive film according to claim 1 or 3, The method for manufacturing the conductive film comprises: In a first step, a first ink is applied onto a surface of a substrate to form a coating film, wherein the first ink is a dispersion comprising a dispersion medium, semiconductor nanoparticles dispersed in the dispersion medium, and a first compound, wherein the first compound exists in the form of an attached compound attached to the semiconductor nanoparticles and a free compound freed from the semiconductor nanoparticles; as well as In the second step, a second ink containing a second compound having a molecular weight smaller than that of the first compound and capable of replacing the first compound and adhering to the semiconductor nanoparticles is brought into contact with the coating film to replace at least a portion of the first compound in the coating film with the second compound.