Preparation of a conductive nanocarbon sphere and its calibration application in scanning electron microscope
Conductive carbon nanospheres were prepared by forming a dense polydopamine layer on the surface of spherical nano-silica and then heat-treating it. This solved the problem of high prices for commercially available calibration standards and enabled low-cost, easy-to-store, and efficient scanning electron microscope calibration.
Patent Information
- Application Number
- CN202310192306.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-02
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-03-02
AI Technical Summary
Commercially available calibration standards for scanning electron microscopes are expensive and difficult to preserve, making it difficult to produce them on a large scale at the laboratory level.
Conductive carbon nanospheres were prepared by using spherical nano-silica as a substrate, forming a dense polydopamine layer on its surface, and then subjecting it to heat treatment. These nanospheres were then used for the calibration of scanning electron microscopes.
It has low preparation cost, good repeatability and stability, and good conductivity of carbon nanospheres, making it suitable for calibration under different shooting conditions and providing clear imaging results and high resolution.
Smart Images

Figure CN116199208B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nanocomposite material preparation, and more particularly to a coated conductive nanosphere, and relates to the preparation of a conductive nanocarbon sphere and its calibration application in a scanning electron microscope. Background Art
[0002] Scanning electron microscopes have the advantages of continuously adjustable magnification, high shooting resolution and ultra-large depth of field, and are widely used in life sciences, materials sciences and microelectronics science. Since scanning electron microscopes use electron beams to scan line by line during shooting, problems such as image magnification and image distortion will occur over time. Only by maintaining a stable resolution and good imaging effect can the most accurate scientific images and measurement data be provided, which requires regular calibration of performance indicators such as resolution and imaging quality using standards. Currently, the main calibration standards on the market are gold nanometer standards, carbon fund standards, copper grid standards and carbon-based tin ball (SnO2) standards. Most of these standards are expensive and have harsh storage conditions. They are not easy or suitable for large-scale production in the laboratory. Therefore, it is particularly important to design and synthesize a nanometer standard with the same calibration effect at the laboratory level that is cheap, easy to obtain and easy to preserve. Summary of the invention
[0003] The present invention aims to solve the problem that the existing calibration standards for scanning electron microscopes on the market are expensive and difficult to preserve, and provides a method for preparing conductive nano-carbon spheres that can be realized at the laboratory level and the calibration application in scanning electron microscopes. The method has low preparation cost and good repetitive stability. The prepared nano-carbon spheres have good conductivity and uniform particle size distribution, and are suitable for calibration of scanning electron microscopes under different shooting conditions.
[0004] The present invention provides a technical solution: a method for preparing conductive nano-carbon spheres, the method comprising:
[0005] S1, providing a spherical nano-silica;
[0006] S2, forming a dense layer of polydopamine on the surface of the spherical silica;
[0007] S3, heat-treating the dense layer of polydopamine to obtain conductive nano-carbon spheres.
[0008] Preferably, in step S1, the specific preparation method is as follows: measure 1-4 ml of 25% ammonia water, 12-48 ml of 99.5% anhydrous ethanol and 80-100 ml of deionized water, stir vigorously for 20-40 min, add 1-3 ml of tetraethoxysilane dropwise, and continue to stir vigorously for 15-45 min.
[0009] Preferably, in step S2, the specific preparation method is as follows: 6-12 ml of 50 mg / ml dopamine hydrochloride is added to the spherical nano-silica solution prepared in S1 for self-polymerization for 12-36 hours to obtain a brown mixed solution, which is then washed with deionized water until neutral and filtered to obtain a brown-black solid, i.e., polydopamine-coated spherical nano-silica.
[0010] Preferably, in step S3, the conductive nano-carbon spheres need to be obtained by high temperature-cracking in an inert gas atmosphere, wherein the inert gas can be nitrogen, argon, or helium; the specific preparation method is as follows: the polydopamine-coated spherical nano-silicon dioxide obtained in S2 is dried in an oven at 80°C for 12 hours, and then carbonized in a programmable temperature-raising tubular furnace under the protection of a nitrogen atmosphere, with a heating rate of 5-10°C / min, a rising temperature of 700-900°C, and a holding time of 120-240min, and finally ground to obtain conductive nano-carbon spheres.
[0011] Another technical solution provided by the present invention is to apply any of the above-mentioned conductive nano-carbon spheres to the calibration of a scanning electron microscope.
[0012] The beneficial effects of the present invention are:
[0013] (1) The synthetic idea of the conductive carbon-coated silica nanospheres provided is relatively novel. Polydopamine (PDA) has properties similar to those of mussel and barnacle adhesion proteins and can adhere to the surface of almost all materials. The oxidation-self-polymerization of dopamine is used to form a PDA layer on the silica surface, and then the nanospheres are prepared through subsequent treatment. The steps are relatively simple, the preparation cost is low, the repetitive stability is good, and large-scale preparation can be achieved at the laboratory level.
[0014] (2) The prepared carbon-coated silica nanospheres have good electrical conductivity and uniform spherical particle size distribution. They can be used for routine calibration of (environmental) scanning electron microscopes without gold spraying and can be recycled and reused.
[0015] (3) Under high vacuum and strong electron beam bombardment, the carbon-coated silica nanosphere calibration standard can still maintain a high resolution and good secondary electron yield, and can be used for calibration at different magnifications (low, medium, and high) and different acceleration voltages (low, medium, and high). BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 The scanning electron microscope and particle size statistics of the conductive nano-carbon spheres in Example 1;
[0017] Figure 2 is a transmission electron microscope image of the conductive nano-carbon spheres in Example 1;
[0018] Figure 3 This is the EDS spectrum of the conductive nanocarbon spheres in Application Example 1;
[0019] Figure 4 The calibration pictures of the conductive nano-carbon spheres under different conditions for the scanning electron microscope in Application Example 1 (accelerating voltage 25 kV, magnification 20000 times);
[0020] Figure 5 The calibration pictures of the conductive nano-carbon spheres under different conditions for the scanning electron microscope in Application Example 2 (accelerating voltage 25 kV, magnification 8000 times);
[0021] Figure 6 These are the calibration images of the conductive nano-carbon spheres under different conditions for a scanning electron microscope in Application Example 3 (accelerating voltage 25 kV, magnification 15,000 times). DETAILED DESCRIPTION
[0022] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the contents of the present invention still fall within the scope of protection of the present invention.
[0023] Embodiment 1:
[0024] This embodiment provides a method for preparing conductive nano-carbon spheres, comprising the following steps:
[0025] S1, providing a spherical nano-silica;
[0026] S2, forming a dense layer of polydopamine on the surface of the spherical silica;
[0027] S3, heat-treating the dense layer of polydopamine to obtain conductive nano-carbon spheres;
[0028] In step S1, the silicon dioxide is prepared by hydrolysis-condensation of tetraethoxysilane under alkaline conditions. The preparation method is as follows: 1 ml of 25% ammonia water, 12 ml of 99.5% anhydrous ethanol and 80 ml of deionized water are measured, and vigorously stirred for 20 minutes, and 1 ml of tetraethoxysilane is added dropwise, and the vigorously stirring is continued for 15 minutes.
[0029] In step S2, the dense polydopamine layer needs to be formed in the alkaline environment of step S1 by oxidation-polymerization of dopamine itself. The preparation method is as follows: 6 ml of 50 mg / ml dopamine hydrochloride is added to the spherical nano-silica solution prepared in S1 for self-polymerization for 12 hours to obtain a brown mixed solution, which is then washed with deionized water until neutral and filtered to obtain a brown-black solid, i.e., polydopamine-coated spherical nano-silica.
[0030] In step S3, the conductive nano-carbon spheres need to be obtained by high temperature-cracking in an inert gas atmosphere. The preparation method is as follows: the polydopamine-coated spherical nano-silicon dioxide obtained in S2 is dried in an oven at 80°C for 12 hours, and then carbonized in a programmable temperature-raising tubular furnace under the protection of a nitrogen atmosphere, wherein the heating rate is 5°C / min, the rising temperature is 700°C, the holding time is 120 minutes, and finally ground to obtain conductive nano-carbon spheres. Figure 1 Scanning electron microscopy shows that the prepared conductive nanocarbon spheres have good sphericity, smooth surface and relatively uniform dispersion; Figure 2 Transmission electron microscopy shows that the outer surface of silicon dioxide is evenly covered with a dense carbon layer.
[0031] Embodiment 2:
[0032] This embodiment provides a method for preparing conductive nano-carbon spheres, comprising the following steps:
[0033] S1, providing a spherical nano-silica;
[0034] S2, forming a dense layer of polydopamine on the surface of the spherical silica;
[0035] S3, heat-treating the dense layer of polydopamine to obtain conductive nano-carbon spheres;
[0036] In step S1, the silicon dioxide is prepared by hydrolysis-condensation of tetraethoxysilane under alkaline conditions. The preparation method is as follows: 2 ml of 25% ammonia water, 36 ml of 99.5% anhydrous ethanol and 90 ml of deionized water are measured, and vigorously stirred for 30 minutes, and 2 ml of tetraethoxysilane is added dropwise, and the vigorously stirring is continued for 30 minutes.
[0037] In step S2, the dense polydopamine layer needs to be formed in the alkaline environment of step S1 by oxidation-polymerization of dopamine itself. The preparation method is as follows: 10 ml of 50 mg / ml dopamine hydrochloride is added to the spherical nano-silica solution prepared in S1 for self-polymerization for 24 hours to obtain a brown mixed solution, which is then washed with deionized water until neutral and filtered to obtain a brown-black solid, i.e., polydopamine-coated spherical nano-silica.
[0038] In step S3, the conductive nano-carbon spheres need to be obtained by high temperature-cracking in an inert gas atmosphere. The preparation method is as follows: the polydopamine-coated spherical nano-silicon dioxide obtained in S2 is dried in an oven at 80°C for 12 hours, and then carbonized in a programmable temperature-raising tubular furnace under the protection of a nitrogen atmosphere, wherein the heating rate is 8°C / min, the rising temperature is 800°C, the holding time is 180 minutes, and finally ground to obtain conductive nano-carbon spheres.
[0039] Embodiment 3:
[0040] This embodiment provides a method for preparing conductive nano-carbon spheres, comprising the following steps:
[0041] S1, providing a spherical nano-silica;
[0042] S2, forming a dense layer of polydopamine on the surface of the spherical silica;
[0043] S3, heat-treating the dense layer of polydopamine to obtain conductive nano-carbon spheres;
[0044] In step S1, the silicon dioxide is prepared by hydrolysis-condensation of tetraethoxysilane under alkaline conditions. The preparation method is as follows: 4 ml of 25% ammonia water, 48 ml of 99.5% anhydrous ethanol and 100 ml of deionized water are measured, and vigorously stirred for 40 minutes, and 3 ml of tetraethoxysilane is added dropwise, and the vigorously stirring is continued for 45 minutes.
[0045] In step S2, the dense polydopamine layer needs to be formed in the alkaline environment of step S1 by oxidation-polymerization of dopamine itself. The preparation method is as follows: 12 ml of 50 mg / ml dopamine hydrochloride is added to the spherical nano-silica solution prepared in S1 for self-polymerization for 36 hours to obtain a brown mixed solution, which is then washed with deionized water until neutral and filtered to obtain a brown-black solid, i.e., polydopamine-coated spherical nano-silica.
[0046] In step S3, the conductive nano-carbon spheres need to be obtained by high temperature-cracking in an inert gas atmosphere. The preparation method is as follows: the polydopamine-coated spherical nano-silicon dioxide obtained in S2 is dried in an oven at 80°C for 12 hours, and then carbonized in a programmable temperature-raising tubular furnace under the protection of a nitrogen atmosphere, wherein the heating rate is 10°C / min, the rising temperature is 900°C, the holding time is 240min, and finally ground to obtain conductive nano-carbon spheres.
[0047] Application Example 1:
[0048] The conductive carbon-coated silica nanospheres prepared in Example 1 are fixed on the sample loading sample stage of the (environmental) scanning electron microscope, and no gold spraying is required, and scanning and shooting imaging calibration is directly performed. Shooting is performed under the conditions of accelerating voltage 25kV and magnification 20000 times (scale size 1μm), and by focusing, adjusting the contrast, brightness and destigmatization steps, the same area is selected for shooting at different time periods, and 4 images are taken in each area. The explanation of the imaging effect of the calibration standard sample is as follows: ①, whether the image is clearly visible, ②, whether the sphere is offset and distorted, ③, whether the image brightness and contrast are moderate, and the particle size statistics of the same nanosphere are performed.
[0049] Figure 3 The EDS spectrum shows that the conductive carbon-coated silica nanosphere calibration standard is composed of three elements: C, O, and Si. There is no characteristic peak of the Au element remaining after gold spraying, which is sufficient to prove that the prepared calibration standard has not been gold-sprayed. Figure 4 The scanning images show that under the above high acceleration voltage and magnification, the obtained images have good clarity, moderate contrast, moderate brightness, no distortion and no lateral stripes due to poor conductivity. At the same time, the statistical error range of the particle size of the same nanospheres photographed at different time periods is small, proving that the prepared conductive carbon-coated silica nanospheres have a good calibration imaging level.
[0050] Application Example 2:
[0051] The conductive carbon-coated silica nanospheres prepared in Example 1 are fixed on the sample loading sample stage of the (environmental) scanning electron microscope, and no gold spraying is required, and the scanning and imaging calibration is directly performed. The images are taken under the conditions of an accelerating voltage of 25kV and a magnification of 8000 times (scale size 2μm), and the same area is selected for shooting at different time periods by focusing, adjusting the contrast, brightness, and stigmation steps, and 4 images are taken in each area. The description of the imaging effect of the calibration standard sample is as follows: 1. Whether the image is clearly visible, 2. Whether the sphere is offset and distorted, 3. Whether the image brightness and contrast are moderate, and the particle size statistics of the same nanosphere are performed.
[0052] Figure 5 The scanning images show that under the above high acceleration voltage and magnification, the obtained images have good clarity, moderate contrast, moderate brightness, no distortion and no lateral stripes due to poor conductivity. At the same time, the statistical error range of the particle size of the same nanospheres photographed at different time periods is small, proving that the prepared conductive carbon-coated silica nanospheres have a good calibration imaging level.
[0053] Application Example 3:
[0054] The conductive carbon-coated silica nanospheres prepared in Example 1 are fixed on the sample loading sample stage of the (environmental) scanning electron microscope, and no gold spraying is required, and scanning and shooting imaging calibration is directly performed. Shooting is performed under the conditions of accelerating voltage 25kV and magnification 15000 times (scale size 1μm), and by focusing, adjusting the contrast, brightness and destigmatization steps, the same area is selected for shooting at different time periods, and 4 images are taken in each area. The description of the imaging effect of the calibration standard sample is as follows: ①, whether the image is clearly visible, ②, whether the sphere is offset and distorted, ③, whether the image brightness and contrast are moderate, and the particle size statistics of the same nanosphere are performed.
[0055] Figure 6 The scanning images show that under the above high acceleration voltage and magnification, the obtained images have good clarity, moderate contrast, moderate brightness, no distortion and no lateral stripes due to poor conductivity. At the same time, the statistical error range of the particle size of the same nanospheres photographed at different time periods is small, proving that the prepared conductive carbon-coated silica nanospheres have a good calibration imaging level.
[0056] The above embodiments are intended to illustrate the essential content of the present invention, but are not intended to limit the protection scope of the present invention. A person skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and protection scope of the technical solution of the present invention.
Claims
1. An application of conductive nano-carbon spheres in scanning electron microscope calibration, characterized in that: The preparation method of the conductive nano-carbon spheres comprises: S1, providing a spherical nano-silica; S2, forming a dense layer of polydopamine on the surface of the spherical nano-silicon dioxide; S3, heat-treating the dense layer of polydopamine to obtain conductive nano-carbon spheres, Applying the conductive nano-carbon spheres to calibrate a scanning electron microscope; In step S1, the specific preparation method is as follows: 1-4 ml of 25% ammonia water, 12-48 ml of 99.5% anhydrous ethanol and 80-100 ml of deionized water are measured, and vigorously stirred for 20-40 min, 1-3 ml of tetraethoxysilane is added dropwise, and the vigorously stirring is continued for 15-45 min; In step S2, the specific preparation method is as follows: 6-12 ml of 50 mg / ml dopamine hydrochloride is added to the spherical nano-silica solution prepared in S1 for self-polymerization for 12-36 h to obtain a brown mixed solution, which is then washed with deionized water until neutral and filtered to obtain a brown-black solid, i.e., polydopamine-coated spherical nano-silica; In step S3, the conductive nano-carbon spheres need to be obtained by high temperature-cracking in an inert gas atmosphere, wherein the inert atmosphere is selected from nitrogen, argon, and helium; the specific preparation method is as follows: the polydopamine-coated spherical nano-silicon dioxide obtained in S2 is dried in an oven at 80°C for 12 h, and then carbonized in a programmable temperature-raising tubular furnace under the protection of a nitrogen atmosphere, with a heating rate of 5-10°C / min, a rising temperature of 700-900°C, and a holding time of 120-240 min. Finally, the conductive nano-carbon spheres are obtained by grinding.