A method for controlling Mg content in a nickel-based high-temperature alloy smelting process

By using aluminum particles to form films and nickel-magnesium alloys during the smelting process of nickel-based high-temperature alloys, and reasonably adding MgO during the electroslag remelting process, the problem of low magnesium element collection rate is solved and efficient magnesium control is achieved , improves the strength and oxidation resistance of the alloy.

CN116516190BActive Publication Date: 2024-11-15HEBEI IRON AND STEEL
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310051868.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-02
Publication Date
2024-11-15
Estimated Expiration
2043-02-02

AI Technical Summary

Technical Problem

During the vacuum + electroslag smelting process of nickel-based high-temperature alloy, the yield of magnesium is low and unstable, making it difficult to accurately control, affecting the strength, oxidation and corrosion resistance of the alloy.

Method used

By adding aluminum particles to the liquid steel during vacuum smelting, and increasing the magnesium content using nickel-magnesium alloy, the MgO allocation amount is determined according to the components in the consumable electrode and the fixed slag system during electroslag remelting. , controls the volatility and oxidation loss of magnesium elements.

Benefits of technology

The yield of magnesium elements is improved, and the stable control is between 65% and 75% and 80% and 90% is controlled, which improves the quality of the alloy and the reproducibility of the process, which is simple to operate, safe and reliable.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

A method for controlling the Mg content in a nickel-based high-temperature alloy smelting process includes two processes, vacuum smelting and electroslag remelting. The vacuum smelting process has the following operating steps: step 1: filling argon into a vacuum melting chamber; step 2: lowering the temperature of the molten steel to 20°C to 30°C above the liquidus, and then adding aluminum particles to the molten steel to form a thin film on the surface of the molten steel; step 3: adding a nickel-magnesium alloy to the molten steel from a secondary feeding bin; step 4: rapidly heating and stirring the molten steel, and when the temperature of the molten steel reaches the tapping temperature, tapping and pouring. The present invention reduces the volatilization of the Mg element when the nickel-magnesium alloy is added, and the Mg yield is improved and can be stably controlled at 65% to 75%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metallurgy, and specifically belongs to the technical field of controlling volatile metal elements in the special material smelting process. Background Art

[0002] In order to reduce the gas and inclusion content in nickel-based high-temperature alloys and obtain high-quality high-temperature alloys with high strength and good oxidation and corrosion resistance, the smelting process often uses "vacuum + electroslag" double smelting. In order to improve the hot processing plasticity and high-temperature strength of the alloy, a certain amount of magnesium is often added during the smelting process. However, due to the low melting point, low density, high vapor pressure, and active chemical properties of magnesium, it is difficult to accurately control the Mg content in both the vacuum smelting process and the electroslag remelting process.

[0003] In the vacuum smelting process, the conventional means of controlling the Mg content is to control the Mg alloy particle size, the temperature of the molten steel and the retention time of the molten steel in the furnace after adding Mg under a certain protective atmosphere pressure. However, although the above means reduce the volatilization of the Mg content to a certain extent, the recovery rate is still less than 40%, and the Mg recovery rate is unstable and the process reproducibility is low.

[0004] The method of controlling Mg in the electroslag remelting stage is to add a certain proportion of MgO into the slag to reduce the loss of Mg content in the remelting process. However, the addition ratio is unclear and no standardized operating procedures have been formed. If the MgO addition ratio is too low, the Mg content loss will not be significantly reduced. If the addition ratio is too high, it may not only increase the Mg content of the electroslag ingot, but also seriously affect the surface quality of the electroslag ingot.

[0005] Therefore, it is of great significance to conduct in-depth research on the key process factors affecting the Mg yield in the “vacuum + electroslag” smelting process of nickel-based high-temperature alloys and develop appropriate control processes for the precise control of the magnesium content in such materials. Summary of the invention

[0006] The technical problem solved by the present invention is to provide a method for controlling the Mg content in the nickel-based high-temperature alloy smelting process, which solves the problem of low and unstable Mg element yield in vacuum smelting and electroslag remelting smelting processes, and the operation method is simple and has a high safety factor.

[0007] In order to solve the above technical problems, the technical solution of the present invention is: a method for controlling the Mg content in a nickel-based high-temperature alloy smelting process, comprising two processes of vacuum smelting and electroslag remelting. The vacuum smelting process has the following operating steps:

[0008] Step 1: Filling the vacuum melting chamber with argon gas;

[0009] Step 2: Lower the temperature of the molten steel to 20°C to 30°C above the liquidus, then add aluminum particles into the molten steel to form a thin film on the surface of the molten steel;

[0010] Step 3: Adding nickel-magnesium alloy into the molten steel from the secondary feeding bin;

[0011] Step 4: Rapidly heat up and stir the molten steel, and when the temperature of the molten steel reaches the tapping temperature, pour the steel.

[0012] In step 2, the temperature of the molten steel is controlled to be 20°C to 30°C above the liquidus. The purpose is: the temperature is near the liquidus of the steel grade, and no solidified crust is formed on the surface of the molten steel. Under this condition, aluminum particles are added because they have a small density and will melt on the surface of the molten steel and float on the surface of the molten steel. When added under low temperature conditions, metallic aluminum aggregates to form a thin film, and the diffusion rate of the aluminum element into the molten steel will also slow down.

[0013] The purpose of heating and stirring the molten steel in step 4 is to quickly homogenize the composition of the molten steel, to reach the temperature of the steel-making conditions, to reduce the time under vacuum conditions, and to reduce the volatilization of magnesium.

[0014] The magnesium alloy is added to the molten steel in the present invention to increase the magnesium content in the molten steel. The nickel-magnesium alloy is used in the vacuum smelting process to reduce the volatilization of pure magnesium during the addition process and to increase the density of the magnesium alloy. After being added to the molten steel, the contact time with the molten steel can be increased to improve the yield. Generally, the magnesium alloy is selected to be greater than 7g / cm 3 As long as the above requirements are met during the production of metal alloys, other forms of magnesium alloys, such as manganese-magnesium alloys, iron-nickel-magnesium alloys, etc., can be added.

[0015] Furthermore, in the electroslag remelting process, the Al2O3 content in the fixed slag system is 25% to 30%, and the amount of MgO added is determined according to the Mg content in the consumable electrode and the Al2O3 content in the fixed slag system. The specific relationship is: [MgO]%=[(100a+1.12)×(b 1 / 3 +0.41)]%, in the above formula 0.004≤a≤0.012, 25≤b≤30, where [MgO]% is the amount of MgO added to the slag, the mass percentage of Mg in the consumable electrode is a%, and the mass percentage of Al2O3 in the fixed slag system is b%.

[0016] The fixed slag system refers to the slag before MgO is added, and the fixed slag system does not contain MgO. The [MgO]% refers to the mass percentage of MgO in the slag after MgO is added.

[0017] In the electroslag remelting process of the present invention, the fixed slag system does not contain MgO. In actual production, a fixed slag system containing MgO can also be used. In this case, first, according to the formula of the present invention, [MgO]%=[(100a+1.12)×(b 1 / 3+0.41)]% to calculate the total amount of MgO required, and then deduct the MgO contained in the original fixed slag system to obtain the amount of MgO to be added.

[0018] In addition, when producing steel with a specific composition, according to the formula of the present invention, [MgO]%=[(100a+1.12)×(b 1 / 3 +0.41)]% to calculate the MgO content in the slag, and directly add the MgO content calculated according to the formula in the production process of the fixed slag system instead of adding MgO in the remelting process. This is the same concept as the present invention and is an embodiment of the present invention.

[0019] Furthermore, in the vacuum smelting process, before step 1, except for the two elements Mg and Al, the other chemical components of the molten steel meet the control target requirements.

[0020] Furthermore, in the electroslag remelting process, the entire electroslag smelting process is carried out under argon protection conditions to ensure that the oxygen in the atmosphere during the entire smelting process is ≤50ppm.

[0021] Furthermore, in step 1 of the vacuum smelting process, the argon filling pressure in the smelting chamber is 45000Pa to 65000Pa.

[0022] Furthermore, in step 2 of the vacuum smelting process, the amount of aluminum particles added is at least 0.04% of the mass of the molten steel.

[0023] The experiment found that when the amount of aluminum particles added in step 2 is 0.04%-0.08% of the mass of the molten steel, it can ensure that at least half of the surface of the molten steel in the crucible is covered by a film. If the target Al content of the steel produced is high, the amount of aluminum particles added can be controlled to be above 0.08% of the mass of the molten steel while ensuring the composition requirements of the steel.

[0024] Furthermore, in step 3 of the vacuum smelting process, the Mg content in the nickel-magnesium alloy is 5% to 10%, and the alloy particle size is 15 mm to 20 mm.

[0025] Furthermore, in step 4 of the vacuum smelting process, the time from increasing the power supply to steel pouring is 3 minutes to 5 minutes.

[0026] The components of the molten steel, alloy, electrode, slag, etc. described in the present invention are all expressed in percentage by mass.

[0027] The purpose of using argon in the two processes of vacuum smelting and electroslag remelting in the present invention is to reduce the oxygen content in the atmosphere, and the purity of the argon is preferably ≥99.99%.

[0028] The beneficial effects of adopting the above technical solution are:

[0029] When adding Mg in vacuum smelting, a certain amount of argon is filled into the melting chamber to reduce the temperature of the molten steel, and aluminum particles are added. After a thin film is formed on the surface of the molten steel, the nickel-magnesium alloy is added. This method uses the film formed by Al to reduce the volatilization of the Mg element when the nickel-magnesium alloy is added, and the Mg yield is improved and can be stably controlled at 65% to 75%; in the electroslag remelting process, a certain proportion of MgO is added to the fixed slag system to inhibit the reaction process of Mg and Al2O3 in the slag during the remelting process, reduce the oxidation loss, and the MgO addition amount forms an empirical formula, which is highly operational and can stably control the Mg yield in the electroslag remelting stage at 80% to 90%. The above process operation method is simple and has a high safety factor, which is conducive to large-scale promotion. Implementation

[0030] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0031] Examples 1-4

[0032] The equipment uses a 500Kg vacuum induction furnace (the ultimate vacuum degree is 6.67×10 -2 Pa, rated power of power supply is 350KW) and 1t protective atmosphere electroslag furnace (AC power supply, ingot drawing type), smelting alloy type is GH4169.

[0033] (1) Vacuum induction furnace smelting

[0034] Ingredients: The smelting weight is 500kg. The vacuum smelting materials are calculated by mass percentage according to the composition of GH4169 alloy. Industrial pure materials are used as the main raw materials. Electrolytic nickel plates, metallic chromium, pure iron, industrial silicon, electrolytic manganese, aluminum, sponge titanium and other high-cleanliness alloy materials are selected. All elements in the metal materials are considered to accurately calculate the ingredients;

[0035] Preparation: Put nickel plates, pure iron, metal chromium, molybdenum bars, niobium bars and other non-oxidizable volatile alloys into the crucible of the vacuum induction furnace, put carbon powder, electrolytic manganese, industrial silicon, aluminum, sponge titanium and other easily oxidizable volatile alloys into the sub-bin, dry the ingot mold and place it in the corresponding position;

[0036] Melting: Evacuate the chamber to a vacuum degree of ≤5Pa, and apply power for heating until the steel in the crucible is completely melted.

[0037] Refining: After the molten steel is completely melted, the vacuum degree is controlled to be ≤5Pa and the molten steel is refined;

[0038] Alloying: turn off the vacuum pump, fill with argon, turn off the power to cool down, add industrial silicon, aluminum particles, electrolytic manganese, sponge titanium and other volatile alloys into the molten steel after the molten steel forms a film, raise the temperature of the molten steel, make the molten steel composition uniform, take samples for testing, and proceed to the next step when all elements in the molten steel except Mg and Al meet the control target requirements. The amount of Al added is the amount of Al added in the subsequent Mg addition process of the molten steel;

[0039] Adding Mg to molten steel: Continue to fill the vacuum melting chamber with argon gas to 45000Pa~65000Pa, reduce the temperature of the molten steel to 20℃~30℃ above the liquidus, add at least 0.04% aluminum particles, and form a thin film on the surface of the molten steel; then add a nickel-magnesium alloy with a Mg content of 5%~10% and a particle size of 15mm~20mm from the secondary feeding bin. The amount of Mg added should take into account the burning loss in the electroslag remelting stage;

[0040] Steel pouring: After adding nickel-magnesium alloy, quickly increase the power supply to strengthen stirring, increase the temperature of the molten steel to the steel-pouring temperature, the time is 3min to 5min, and the steel is poured. The ingot mold size is Φ220mm×1600mm.

[0041] (2) Electroslag remelting

[0042] Pre-melted slag preparation: 30kg of slag is needed for remelting and smelting. The amount of MgO in the slag is determined according to the Al2O3 content in the slag system and the Mg content of the smelted vacuum ingot. After stirring and mixing, put it into the heating furnace for baking;

[0043] Preparation of consumable electrode: pre-treat the vacuum ingot cast by vacuum smelting to ensure that there is no oxide layer on the surface of the ingot and no shrinkage cavity at the end of the ingot, and then weld it to the auxiliary electrode;

[0044] Furnace loading: Place a dummy plate of the same material on the electroslag bottom water tank, place arc starting chips of the same material in the center of the dummy plate, install a Φ300×1300mm crystallizer, protective smoke hood, and consumable electrode;

[0045] Melting: Turn on the power to start the arc, slowly add slag after the arc light is stable, adjust the melting speed to the target melting speed after the slag is melted, and feed the consumable electrode when a certain weight remains. After the feeding is completed, turn off the melting power supply and demould after 30 minutes;

[0046] Argon protection: Argon is continuously introduced as a protective gas during the entire smelting process. The purity of argon is ≥99.99%, ensuring that the oxygen content in the atmosphere during the entire smelting process is ≤50ppm;

[0047] Example 1-4 The control parameters of the Mg addition process in the vacuum smelting process are shown in Table 1, where TL represents the liquidus temperature of the molten steel. The data on the amount of aluminum particles added in Table 1 are the percentage of the amount of aluminum particles added to the mass of the molten steel.

[0048] Table 1

[0049]

[0050] The calculation of the amount of MgO added to the electroslag system is shown in Table 2, where [Mg]% is the mass percentage of Mg in the consumable electrode, [Mg]%=a%; and [Al2O3]% is the mass percentage of Al2O3 in the fixed slag system, [Al2O3]%=b%.

[0051] Table 2

[0052]

[0053] The test results of Mg content in ingots after vacuum and electroslag are shown in Table 3. The Mg recovery rate in the vacuum smelting stage is stably controlled at 65% to 75%, and the Mg recovery rate in the electroslag remelting process is 80% to 90%.

[0054] Table 3

[0055]

[0056] Embodiment 5-8

[0057] The equipment uses a 50Kg vacuum induction furnace (the ultimate vacuum degree is 4.28×10 -2 Pa, rated power of power supply is 100KW) and 1t protective atmosphere electroslag furnace (AC power supply, ingot drawing type), the smelting alloy type is GH80A.

[0058] (1) Vacuum induction furnace smelting

[0059] Ingredients: The smelting weight is 45kg. The vacuum smelting materials are calculated by mass percentage according to the GH80A alloy components. Industrial pure materials are used as the main raw materials. Electrolytic nickel plates, metallic chromium, pure iron, industrial silicon, electrolytic manganese, aluminum, sponge titanium and other high-cleanliness alloy materials are selected. All elements in the metal materials are considered to accurately calculate the ingredients;

[0060] Preparation: Put nickel plate, metal chromium and other non-oxidizable volatile alloys into the crucible of the vacuum induction furnace, put carbon powder, electrolytic manganese, industrial silicon, aluminum, sponge titanium and other easily oxidizable volatile alloys into the sub-bin, dry the ingot mold and place it in the corresponding position;

[0061] Melting: Evacuate the chamber to a vacuum degree of ≤5Pa, and apply power for heating until the steel in the crucible is completely melted.

[0062] Refining: After the molten steel is completely melted, the vacuum degree is controlled to be ≤5Pa and the molten steel is refined;

[0063] Alloying: turn off the vacuum pump, fill with argon, turn off the power to cool down, add industrial silicon, aluminum particles, electrolytic manganese, sponge titanium and other volatile alloys into the molten steel after the molten steel forms a film, raise the temperature of the molten steel, make the molten steel composition uniform, take samples for testing, and proceed to the next step when all elements in the molten steel except Mg and Al meet the control target requirements. The amount of Al added is the amount of Al added in the subsequent Mg addition process of the molten steel;

[0064] Adding Mg to molten steel: Continue to fill the vacuum melting chamber with argon gas to 45000Pa~65000Pa, reduce the temperature of the molten steel to 20℃~30℃ above the liquidus, add at least 0.04% aluminum particles, and form a thin film on the surface of the molten steel; then add a nickel-magnesium alloy with a Mg content of 5%~10% and a particle size of 15mm~20mm from the secondary feeding bin. The amount of Mg added should take into account the burning loss in the electroslag remelting stage;

[0065] Steel pouring: After adding nickel-magnesium alloy, quickly increase the power supply to strengthen stirring, increase the temperature of the molten steel to the steel-pouring temperature, the time is 3min to 5min, steel pouring, the ingot mold size is Φ90mm×850mm.

[0066] (2) Electroslag remelting

[0067] Pre-melted slag preparation: 5kg of slag is required for remelting and smelting. The amount of MgO in the slag is determined according to the Al2O3 content in the slag system and the Mg content of the smelted vacuum ingot. After stirring and mixing, put it into the heating furnace for baking;

[0068] Preparation of consumable electrode: pre-treat the vacuum ingot cast by vacuum smelting to ensure that there is no oxide layer on the surface of the ingot and no shrinkage cavity at the end of the ingot, and then weld it to the auxiliary electrode;

[0069] Furnace loading: Place a dummy plate of the same material on the electroslag bottom water tank, place arc starting chips of the same material in the center of the dummy plate, install a Φ150×1000mm crystallizer, protective smoke hood, and consumable electrode;

[0070] Melting: Turn on the power to start the arc, slowly add slag after the arc light is stable, adjust the melting speed to the target melting speed after the slag is melted, and feed the consumable electrode when a certain weight remains. After the feeding is completed, turn off the melting power supply and demould after 30 minutes;

[0071] Argon protection: Argon is continuously introduced as a protective gas during the entire smelting process. The purity of argon is ≥99.99%, ensuring that the oxygen content in the atmosphere during the entire smelting process is ≤50ppm;

[0072] Example 5-8 The control parameters of the Mg addition process in the vacuum smelting process are shown in Table 4, where TL represents the liquidus temperature of the molten steel. The data on the amount of aluminum particles added in Table 4 are the percentage of the amount of aluminum particles added to the mass of the molten steel.

[0073] The calculation of the amount of MgO added to the electroslag system is shown in Table 5, where [Mg]% is the mass percentage of Mg in the consumable electrode, [Mg]%=a%; and [Al2O3]% is the mass percentage of Al2O3 in the fixed slag system, [Al2O3]%=b%.

[0074] The test results of Mg content in ingot after vacuum and electroslag are shown in Table 6.

[0075] Table 4

[0076]

[0077] Table 5

[0078]

[0079] Table 6

[0080]

[0081] The above embodiments are only used to illustrate rather than limit the technical solutions of the present invention. Although the present invention is described in detail with reference to the above embodiments, those skilled in the art should understand that the present invention can still be modified or replaced by equivalents. Any modification or partial replacement that does not depart from the spirit and scope of the present invention should be included in the scope of the claims of the present invention.

Claims

1. A method for controlling the Mg content in a nickel-based high-temperature alloy smelting process, characterized in that: The method comprises two processes: vacuum smelting and electroslag remelting. In the vacuum smelting process, before step 1, the chemical components of the molten steel, except for the two elements Mg and Al, meet the control target requirements. The operation steps are as follows: Step 1: Filling the vacuum melting chamber with argon gas; Step 2: Lower the temperature of the molten steel to 20°C to 30°C above the liquidus, then add aluminum particles into the molten steel to form a thin film on the surface of the molten steel; Step 3: Adding nickel-magnesium alloy into the molten steel from the secondary feeding bin; Step 4: Rapidly heat and stir the molten steel until the temperature of the molten steel reaches the tapping temperature, and then perform electroslag remelting after the steel is tapped; In the electroslag remelting process, the Al2O3 content in the fixed slag system is 25% to 30%, and the amount of MgO added is determined according to the Mg content in the consumable electrode and the Al2O3 content in the fixed slag system. The specific relationship is: [MgO]%=[(100a+1.12)×(b 1 / 3 +0.41)]%, in the above formula 0.004≤a≤0.012, 25≤b≤30, where [MgO]% is the amount of MgO added to the slag, the mass percentage of Mg in the consumable electrode is a%, and the mass percentage of Al2O3 in the fixed slag system is b%.

2. The method for controlling Mg content in a nickel-based high-temperature alloy smelting process according to claim 1, characterized in that: The electroslag remelting process and the entire electroslag smelting process are carried out under argon protection conditions to ensure that the oxygen in the atmosphere during the entire smelting process is ≤50ppm.

3. The method for controlling Mg content in a nickel-based high-temperature alloy smelting process according to claim 1, characterized in that: In step 1 of the vacuum smelting process, the argon filling pressure in the smelting chamber is 45000Pa to 65000Pa.

4. The method for controlling Mg content in a nickel-based high-temperature alloy smelting process according to claim 1, characterized in that: In step 2 of the vacuum smelting process, the amount of aluminum particles added is at least 0.04% of the mass of the molten steel.

5. The method for controlling Mg content in a nickel-based high-temperature alloy smelting process according to claim 1, characterized in that: In step 3 of the vacuum smelting process, the Mg content in the nickel-magnesium alloy is 5% to 10%, and the alloy particle size is 15 mm to 20 mm.

6. The method for controlling Mg content in a nickel-based high-temperature alloy smelting process according to claim 1, characterized in that: In step 4 of the vacuum smelting process, the time from increasing the power supply to steel pouring is 3 minutes to 5 minutes.

Citation Information

Cited By

  • A nickel-based alloy containing low melting point elements melting device and method

    CN122835123A