Production method of battery shell for energy storage and battery shell for energy storage
By optimizing the composition and extrusion process of aluminum alloy, the battery case for energy storage with dense grains is solved, and the problems of complex production processes and large wall thickness in the existing technology are achieved, and the battery pack is lighter and energy density is improved.
Patent Information
- Application Number
- CN202311337553.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-16
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-10-16
AI Technical Summary
The existing battery housing for energy storage is complex, with high energy consumption and large wall thickness, making it difficult to achieve lightweight structure and increase energy density of the battery pack.
The Mn and Fe element contents are optimized and adjusted in aluminum alloy, and the battery shell for energy storage is produced by extrusion and molding in one go, controlling the grain structure to control the denseness of the grain and the wall thickness is less than or equal to 0.8mm.
Shorten production processes, reduce energy consumption, improve production efficiency, reduce costs, and achieve lightweight structure and increase energy density of the battery pack.
Smart Images

Figure CN117340030B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of energy storage technology, and more specifically, to a production method of a battery shell for energy storage and a battery shell for energy storage. Background Art
[0002] Energy storage refers to the process of storing energy through a medium or device and releasing it when needed. According to the energy storage method, energy storage can be divided into three categories: physical energy storage, chemical energy storage, and electromagnetic energy storage. Physical energy storage mainly includes pumped storage, compressed air energy storage, flywheel energy storage, etc. Chemical energy storage mainly includes lead-acid batteries, lithium-ion batteries, sodium-sulfur batteries, flow batteries, etc. Electromagnetic energy storage mainly includes supercapacitor energy storage and superconducting energy storage. Lithium-ion battery energy storage is currently the most popular energy storage method.
[0003] At this stage, higher requirements are put forward for the energy density of battery systems. There are two ways to improve the energy density of batteries: one is to increase the specific energy of single cells; the other is to make the battery pack structure lightweight. Increasing the specific energy of single cells is technically difficult, has a long research and development cycle, and requires a large capital investment. In contrast, making the battery pack structure lightweight is easier to achieve. In the prior art, the battery shell for energy storage is generally formed by stamping, using a punch press and a hydraulic press to punch out the aluminum plate, and then stretch it through multiple passes (usually 7-8 passes), and temper it to remove stress. The production process is complicated, the process is long, the energy consumption is high, the production efficiency is low, the manufacturing cost is high, the product wall thickness is large, and it is not conducive to achieving the lightweight structure of the battery pack.
[0004] Therefore, there is an urgent need to provide a method for producing a battery shell for energy storage that can shorten the production process and reduce the wall thickness, so as to achieve a lightweight structure of the battery pack. Summary of the invention
[0005] In view of this, the present invention provides a production method of a battery shell for energy storage and a battery shell for energy storage, which are used to shorten the production process, reduce the wall thickness, achieve lightweight structure of the battery pack, and improve the battery energy density.
[0006] In one aspect, the present invention provides a method for producing a battery casing for energy storage, comprising:
[0007] The steps of preparing aluminum melt include:
[0008] Providing a master alloy, controlling the mass percentage of each component in the master alloy: Si 0.06%-0.2%, Mg <0.05%, Fe 0.3%-0.45%, Cu 0.10%-0.18%, Mn 1.06%-1.20%, Cr <0.10%, Ti <0.05%, Zn <0.05%, and the balance is Al;
[0009] Providing furnace charge, the furnace charge includes 20%-80% of electrolytic aluminum liquid, less than or equal to 50% of complex aluminum liquid, less than or equal to 10% of complex ingot, and the furnace charge also includes waste generated in the process of manufacturing battery shell for energy storage;
[0010] The charge is placed in a smelting furnace for melting, and the smelting temperature is controlled between 720°C and 760°C. When the charge is melted to 730°C to 750°C, the intermediate alloy is added; and then the aluminum melt is obtained after refining and standing; the aluminum melt is processed and filtered online by SNIF to control the hydrogen content of the aluminum melt to be less than or equal to 0.16ml / 100g.Al, the Na content to be less than or equal to 2ppm, and the Ca content to be less than or equal to 3ppm;
[0011] A casting step, wherein the aluminum melt is cooled to form an aluminum rod;
[0012] Homogenizing step, the homogenizing temperature is 620℃+5℃ / 6h;
[0013] The step of extruding a battery shell for energy storage in one step comprises: extruding an aluminum rod through a die to produce the battery shell for energy storage;
[0014] The step of quenching and cooling;
[0015] The straightening step includes straightening and adjusting the energy storage battery casing.
[0016] Optionally, in the step of extruding a battery shell for energy storage, the temperature of the extrusion cylinder is 400℃±20℃, the mold temperature is 470℃±10℃, the aluminum rod heating temperature is 450℃-550℃, the extrusion adopts constant speed extrusion, the filling pressure is less than or equal to 110bar, the main cylinder limit pressure is less than or equal to 260bar, the breakthrough pressure slope is less than or equal to 5sec, the extrusion speed attenuation ratio is -15%--5%, the extrusion rod length is 500mm-1000mm, and the extrusion rod speed is 3.0mm / s-7.0mm / s.
[0017] Optionally, in the quenching and cooling step, the quenching method is wind cooling, and after cooling, the temperature of the energy storage battery shell is less than or equal to 250°C.
[0018] Optionally, the straightening requirement is within an error of 0.5%-1%.
[0019] Optionally, when the waste is Class 1 waste, the mass fraction is less than or equal to 80%, and when the waste is Class 2 waste, the mass fraction is less than or equal to 20%.
[0020] Optionally, the step of preparing the aluminum melt also includes smelting sampling, and the smelting sampling temperature is 725°C-745°C.
[0021] Optionally, in the step of preparing the aluminum melt, the refining temperature is 725-740° C., and the standing time is greater than or equal to 30 minutes.
[0022] Optionally, a mixed gas of argon and chlorine is used in the refining step, and the amount of chlorine is 2%-5%; the refining time is 40min-60min.
[0023] Optionally, in the casting step, the aluminum melt is injected into an ingot, and the aluminum melt is cooled through a crystallizer to form an aluminum rod. The starting casting temperature is 670°C-700°C, the starting casting speed is 135mm / min-175mm / min, the intermediate casting temperature is 680°C-710°C, the intermediate casting speed is 130mm / min-170mm / min, the inlet water temperature is 15°C-45°C, and the water flow rate is 590m3 / h±100m3 / h.
[0024] Optionally, the filtration is CFF bipolar plate filtration.
[0025] The present invention also provides a battery shell for energy storage manufactured by the above production method, wherein the wall thickness of the shell is less than or equal to 0.8 mm.
[0026] Optionally, the size of the grains in the shell is less than or equal to 100 μm.
[0027] Optionally, the shell is circular or rectangular.
[0028] Optionally, the thickness of the shell is not equal, and the thickness at the middle of the shell is greater than the thickness at the edge of the shell.
[0029] Compared with the prior art, the production method of the energy storage battery shell and the energy storage battery shell provided by the present invention achieve at least the following beneficial effects:
[0030] The production method of the energy storage battery shell provided by the present invention adopts a method of extruding an aluminum rod through a die to produce the energy storage battery shell in one step, thereby shortening the production process, shortening the flow, and being conducive to reducing energy consumption, improving production efficiency, and reducing production costs accordingly;
[0031] In the step of making aluminum melt, the mass percentage of each component in the master alloy is controlled as follows: Si 0.06%-0.2%, Mg <0.05%, Fe 0.3%-0.45%, Cu 0.10%-0.18%, Mn1.06%-1.20%, Cr<0.10%, Ti<0.05%, Zn<0.05%, and the balance is Al. The present invention optimizes and adjusts the content of Mn element in the alloy. Mn can increase the strength of the alloy. Controlling the Mn element content at 1.06%-1.20% can avoid forming a large amount of brittle compound MnAl6, which causes the alloy to crack easily during extrusion molding. The present invention controls the Fe element content in the alloy to 0.3%-0.45%, and the chain-like Fe phase is spheroidized after high-temperature homogenization, which can promote particle recrystallization. The present invention reduces the Si element content in the alloy. Since Si is an impurity, the impurity Si can increase the thermal cracking tendency of the alloy and reduce the casting performance, so the present invention reduces the Si element content and can improve the casting performance. The grain structure prepared by the present invention is dense.
[0032] The energy storage battery shell produced by the above method has a dense grain structure and a grain size of less than or equal to 100 μm, so the shell wall thickness is small after one extrusion molding, and the shell wall thickness is less than or equal to 0.8 mm, which can achieve a lightweight structure of the battery pack and improve the battery energy density.
[0033] Of course, any product implementing the present invention does not necessarily need to achieve all of the technical effects described above at the same time.
[0034] Further features and advantages of the present invention will become apparent from the following detailed description of exemplary embodiments of the present invention with reference to the attached drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] The accompanying drawings, which are incorporated in and constitute a part of the specification, illustrate embodiments of the invention and, together with the description, serve to explain the principles of the invention.
[0036] Figure 1 This is a flow chart of a method for producing a battery casing for energy storage provided by the present invention;
[0037] Figure 2 It is a structural schematic diagram of a battery housing for energy storage provided by the present invention;
[0038] Figure 3 It is a structural schematic diagram of a battery housing for energy storage provided by the present invention;
[0039] Figure 4 It is a structural schematic diagram of a battery housing for energy storage provided by the present invention;
[0040] Figure 5 This is a scanning electron microscope image of the grains in the shell. DETAILED DESCRIPTION
[0041] Various exemplary embodiments of the present invention will now be described in detail with reference to the accompanying drawings. It should be noted that the relative arrangement of components and steps, numerical expressions and numerical values set forth in these embodiments do not limit the scope of the present invention unless otherwise specifically stated.
[0042] The following description of at least one exemplary embodiment is merely illustrative in nature and is in no way intended to limit the invention, its application, or uses.
[0043] Technologies, methods, and equipment known to ordinary technicians in the relevant art may not be discussed in detail, but where appropriate, the technologies, methods, and equipment should be considered as part of the specification.
[0044] In all examples shown and discussed herein, any specific values should be interpreted as merely exemplary and not as limiting. Therefore, other examples of the exemplary embodiments may have different values.
[0045] It should be noted that like reference numerals and letters refer to similar items in the following figures, and therefore, once an item is defined in one figure, it need not be further discussed in subsequent figures.
[0046] Reference Figure 1 , Figure 1 This is a flow chart of a method for producing a battery casing for energy storage provided by the present invention. Figure 1 The production method comprises the following steps:
[0047] S1, a step of preparing an aluminum melt, comprising:
[0048] S11, providing a master alloy, controlling the mass percentage of each component in the master alloy: Si 0.06%-0.2%, Mg < 0.05%, Fe 0.3%-0.45%, Cu 0.10%-0.18%, Mn 1.06%-1.20%, Cr < 0.10%, Ti < 0.05%, Zn < 0.05%, and the balance is Al;
[0049] S12, providing a furnace charge, the furnace charge comprising 20%-80% of electrolytic aluminum liquid, less than or equal to 50% of complex aluminum liquid, less than or equal to 10% of complex ingots, and the furnace charge also includes waste generated in the process of manufacturing the battery shell for energy storage;
[0050] S13, placing the charge into a smelting furnace for melting, controlling the melting temperature between 720°C and 760°C, and adding the intermediate alloy when the charge melts to 730°C to 750°C; then refining and standing to obtain molten aluminum; the molten aluminum is processed and filtered online by SNIF to control the hydrogen content of the molten aluminum to be less than or equal to 0.16ml / 100g.Al, the Na content to be less than or equal to 2ppm, and the Ca content to be less than or equal to 3ppm;
[0051] S2, a casting step, wherein the aluminum melt is formed into an aluminum rod by cooling;
[0052] S3, homogenization step, the homogenization temperature is 620℃+5℃ / 6h;
[0053] S4, a step of extruding a battery shell for energy storage in one step, comprising: extruding an aluminum rod through a die to produce a battery shell for energy storage;
[0054] S5, a quenching and cooling step;
[0055] S6, a straightening step, includes straightening and adjusting the energy storage battery casing so that its size and straightness meet the requirements.
[0056] Specifically, step S1 is a step of preparing aluminum melt. Step S11 and step S12 in this step are not in particular order and can be performed simultaneously, or step S11 can be performed first and then S12, or step S12 can be performed first and then S11.
[0057] Optionally, the mass percentage of Si can be 0.06%, 0.07%, 0.08%, 0.09%, 0.1%, 0.11%, 0.12%, 0.13%, 0.14%, 0.15%, 0.16%, 0.17%, 0.18%, 0.19%, or 0.2%. Optionally, the mass percentage of Si is 0.06%-0.08%. The present invention reduces the content of Si element in the alloy. Since Si is an impurity, the impurity Si can increase the hot cracking tendency of the alloy and reduce the casting performance, so the present invention greatly reduces the mass percentage of Si element, thereby improving the casting performance. Optionally, the mass percentage of Mg can be 0.01%, 0.02%, 0.03%, 0.04% or 0.05%, and the mass percentage of Mn can be 1.06%, 1.07%, 1.08%, 1.09%, 1.1%, 1.11%, 1.12%, 1.13%, 1.14%, 1.15%, 1.16%, 1.17%, 1.18%, 1.19%, 1.20%. Preferably, the mass percentage of Mn is 1.11%-1.2%. It can be understood that Mg can increase the tensile strength of the alloy, and Mn can supplement the strengthening effect. For every 1% increase in Mg, the tensile strength increases by about 34MPa. Of course, if less than 1% of Mn is added, the strengthening effect may be supplemented. Therefore, the Mg content can be reduced after adding Mn, that is, the higher the Mn content, the lower the Mg content can be. Of course, Mn can reduce the tendency of thermal cracking. In addition, Mn can also make the Mg5Al8 compound precipitate evenly and improve the corrosion resistance. The present invention optimizes and adjusts the content of the Mn element in the alloy. Mn can increase the strength of the alloy. Controlling the Mn element content to 1.06%-1.20% can avoid the formation of a large amount of brittle compound MnAl6, which can cause the alloy to crack easily during the extrusion molding process. The present invention controls the Fe element content in the alloy to 0.3%-0.45%, and the chain-like Fe phase is spheroidized after high-temperature homogenization, which can promote particle recrystallization.
[0058] It should be noted that the composition of the master alloy (aluminum alloy) is controlled in the present invention, and the mass percentage of each component in the master alloy is controlled: Si 0.06%-0.2%, Mg<0.05%, Fe0.3%-0.45%, Cu 0.10%-0.18%, Mn1.06%-1.20%, Cr<0.10%, Ti<0.05%, Zn<0.05%, and the balance is Al. The shell made according to the above mass percentages has a dense grain structure and can improve the extrudability of the final aluminum rod.
[0059] The present invention optimizes the composition and grain structure of 3003 aluminum alloy through a melting and casting process, improves the extrudability of 3003 aluminum alloy, realizes one-time extrusion forming of thin-walled (≤0.8mm) battery shell, greatly simplifies the production process and reduces production costs.
[0060] In the above step S12, a charge is provided, the charge includes 20%-80% of electrolytic aluminum liquid, less than or equal to 50% of complex aluminum liquid, or less than or equal to 10% of complex ingots, and the charge also includes waste material, which is waste material generated in the process of manufacturing the battery shell for energy storage;
[0061] Specifically, when the charge includes electrolytic aluminum liquid, the solid material mass of the electrolytic aluminum liquid is between 20% and 80%, for example, the solid material mass of the electrolytic aluminum liquid is 20%, 25%, 30%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, when the charge includes complex aluminum liquid, the solid material mass of the complex aluminum liquid can be 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, when the charge includes complex ingots, the solid material mass in the complex ingot can be 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, the charge can also include waste, of course, the waste here is the waste generated in the process of manufacturing the battery shell for energy storage, which is conducive to reducing costs. The total amount of solid material used in the charge of the present invention needs to be above 20%.
[0062] In the above step S13, the purpose of smelting is to melt the solid charge and melt out an aluminum alloy melt with the required chemical composition. Specifically, the charge is placed in a smelting furnace for melting, and the smelting temperature is controlled between 720°C and 760°C. For example, the smelting temperature can be 720°C, 725°C, 730°C, 735°C, 740°C, 745°C, 750°C, 755°C, and 760°C. When the charge is melted to 730°C-750°C, for example, the charge is melted to 730°C, 735°C, 740°C, 745°C, and 750°C, an intermediate alloy is added; and then the aluminum melt is obtained after refining and standing; the aluminum melt is processed and filtered online by SNIF to control the hydrogen content of the aluminum melt to be less than or equal to 0.16ml / 100g.Al, the Na content is less than or equal to 2ppm, and the Ca content is less than or equal to 3ppm.
[0063] It is understandable that the casting step in the present invention can adopt the structure in the prior art, and no specific limitation is made here. The crystallizer can be specifically a hollow cylindrical hollow area, and the aluminum melt is injected into the hollow cylindrical hollow area. The crystallizer has an inner wall and an outer wall, and a coolant can be injected between the inner wall and the outer wall. The coolant can be water. When the aluminum melt is injected into the hollow cylindrical hollow area, it is cooled to form an aluminum rod.
[0064] In step S3, the purpose of homogenization is to make the unbalanced eutectic structure in the aluminum rod be evenly distributed in the matrix, and the supersaturated solid solution elements precipitate from the solid solution, thereby eliminating the stress of the aluminum rod and improving the structure and performance of the processed product.
[0065] Step S4 of the present invention is a step of obtaining an energy storage battery shell by extrusion forming in one step. Specifically, an aluminum rod is extruded through a die to produce a target energy storage battery shell, and the die here is determined according to the shape of the target energy storage battery shell.
[0066] In the prior art, the battery shell for energy storage is generally formed by stamping, using a punch press and a hydraulic press to punch out the aluminum plate, and then stretch it through multiple passes (usually 7-8 passes) and temper it to remove stress. The production process is complicated, the process is long, the energy consumption is high, the production efficiency is low, and the manufacturing cost is high. The present invention only needs to be extruded to form it at one time, thereby shortening the production process, shortening the process, helping to reduce energy consumption, improve production efficiency, and reduce the production cost accordingly.
[0067] Of course, the present invention also includes a quenching and cooling step S5 and a straightening step S6, so that the size and straightness of the energy storage battery shell produced meet the requirements, the product qualification rate is high, and the product qualification rate can reach more than 99%.
[0068] Compared with the prior art, the production method of the energy storage battery casing provided by the present invention achieves at least the following beneficial effects:
[0069] In the step of making aluminum melt, the mass percentage of each component in the master alloy is controlled as follows: Si 0.06%-0.2%, Mg <0.05%, Fe 0.3%-0.45%, Cu 0.10%-0.18%, Mn1.06%-1.20%, Cr<0.10%, Ti<0.05%, Zn<0.05%, and the balance is Al. The present invention optimizes and adjusts the content of Mn element in the alloy. Mn can increase the strength of the alloy. Controlling the Mn element content at 1.06%-1.20% can avoid forming a large amount of brittle compound MnAl6, which causes the alloy to crack easily during extrusion molding. The present invention controls the Fe element content in the alloy to 0.3%-0.45%, and the chain-like Fe phase is spheroidized after high-temperature homogenization, which can promote particle recrystallization. The present invention reduces the Si element content in the alloy. Since Si is an impurity, the impurity Si can increase the thermal cracking tendency of the alloy and reduce the casting performance, so the present invention reduces the Si element content and can improve the casting performance. The grain structure prepared by the present invention is dense.
[0070] The present invention produces the energy storage battery shell by extruding the aluminum rod through a die in one step, thereby shortening the production process, shortening the flow, and being conducive to reducing energy consumption, improving production efficiency, and reducing production costs accordingly.
[0071] In some optional embodiments, continue to refer to Figure 1In step S4 of extruding a battery shell for energy storage, the temperature of the extrusion cylinder is 400℃±20℃, the mold temperature is 470℃±10℃, the aluminum rod heating temperature is 450℃-550℃, the extrusion adopts constant speed extrusion, the filling pressure is less than or equal to 110bar, the main cylinder limit pressure is less than or equal to 260bar, the breakthrough pressure slope is less than or equal to 5sec, the extrusion speed attenuation ratio is -15%-5%, the extrusion rod length is 500mm-1000mm, and the extrusion rod speed is 3.0mm / s-7.0mm / s.
[0072] The temperature of the extrusion barrel can be any temperature value between 380°C and 420°C, for example, 380°C, 390°C, 400°C, 410°C, or 420°C.
[0073] The temperature of the extrusion barrel in this temperature range is conducive to extending the life of the equipment, and at the same time 380-420℃ can ensure that the temperature of the aluminum rod is not too low.
[0074] The mold temperature may be any temperature value between 460°C and 480°C, for example, 460°C, 470°C, or 480°C.
[0075] The mold temperature has good performance when set in this temperature range. When the temperature is lower than the standard (460℃), the extrusion difficulty increases, and when the temperature exceeds the standard (480℃), the surface quality of the mold working zone is poor.
[0076] The heating temperature of the aluminum rod can be any temperature value between 450°C and 550°C, for example, 450°C, 460°C, 470°C, 480°C, 490°C, 500°C, 510°C, 520°C, 530°C, 540°C, and 550°C. The heating temperature of the aluminum rod in this range can meet the performance requirements. If the aluminum rod temperature is lower than the standard (450°C), the extrusion is difficult. If it exceeds the standard (550°C), the product surface quality is poor.
[0077] The filling pressure is less than or equal to 110 bar. When the filling pressure is greater than 110 bar, for example, the filling pressure is 110-130 bar, the filling pressure is small and there is residual gas in the extrusion cylinder. The filling pressure is high and the equipment life is affected.
[0078] The master cylinder limit pressure is 260bar, which is an inherent parameter of the equipment.
[0079] The breakthrough pressure slope is 5 seconds. If it is lower than the standard, cracks will appear in the product. If it exceeds the standard, the extrusion capacity will be low.
[0080] The extrusion speed attenuation ratio is between -15% and -5%, for example, the extrusion speed attenuation ratio is -15%, -14%, -13%, -12%, -11%, -10%, -9%, -8%, -7%, -6%, -5%, -4%, -3%, -2%, -1%, 1%, 2%, 3%, 4%, 5%. If the extrusion speed attenuation is greater than -5%, the product is prone to cracks, and if the extrusion speed attenuation is less than -15%, the extrusion capacity is low.
[0081] The length of the extruded rod is 500mm-1000mm, for example, the extruded rod can be 500mm, 600mm, 700mm, 800mm, 900mm, 1000mm. If the length of the extruded rod is less than 500mm, the extrusion capacity is low. In addition, the maximum rod length allowed by the extrusion equipment is 1000mm.
[0082] The extrusion rod speed is between 3.0 mm / s and 7.0 mm / s, for example, the extrusion rod speed can be 3.0 mm / s, 4.0 mm / s, 5.0 mm / s, 6.0 mm / s, and 7.0 mm / s. If the extrusion rod speed is lower than 3.0 mm, the production capacity is low, and if it is higher than 7.mm / s, the product surface quality is poor and cracks are easily generated.
[0083] The present invention adopts reasonable process conditions and can produce the battery shell for energy storage through one-time extrusion molding, thereby simplifying the process flow and reducing the production cost.
[0084] In some optional embodiments, in the quenching and cooling step, the quenching method is wind cooling, and the temperature of the energy storage battery shell after cooling is less than or equal to 250°C.
[0085] Specifically, the quenching method here can be strong wind cooling. After strong wind cooling, the temperature of the energy storage battery shell is required to be reduced to below 250°C. For example, the temperature of the energy storage battery shell is between 200°C and 250°C, such as 200°C, 210°C, 220°C, 230°C, 240°C, 250°C, or any value between 200°C and 250°C. If the temperature of the energy storage battery shell after cooling is higher than 250°C, the product performance is unqualified and the extrusion efficiency is low. If the temperature of the energy storage battery shell after cooling is less than or equal to 250°C, the product character qualification rate is high and the extrusion efficiency is high.
[0086] In some optional embodiments, combined with Figure 1 The straightening requirement is that the error is within 0.5%-1%.
[0087] The straightening requirement can be 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, or 1%.
[0088] The required straightening error is less than 0.5%, otherwise the product cannot be straightened and the size is likely to be unqualified. The required straightening error is higher than 1%, and orange peel is likely to appear on the surface.
[0089] In some optional embodiments, when the waste is Class 1 waste, the mass fraction is less than or equal to 80%, and when the waste is Class 2 waste, the mass fraction is less than or equal to 20%.
[0090] The waste materials in the present invention are divided into first-class waste materials and second-class waste materials. The first-class waste materials have a mass fraction of less than or equal to 80%, such as casting stubs, runner waste, ingot cut heads, cut tails, scrapped ingots, extrusion residues, stubs with a length greater than 200 mm, mold samples, low-magnification samples, oxidation products, etc. The second-class waste materials have a mass fraction of less than or equal to 20%, such as metals in waste slag, machined aluminum chips, etc. Utilizing the waste materials in the workshop can realize waste utilization and reduce costs.
[0091] In some optional embodiments, the step of preparing the aluminum melt further includes smelting sampling, and the smelting sampling temperature is 725°C-745°C.
[0092] It is understandable that the purpose of smelting sampling is to detect whether the chemical composition meets the standard requirements.
[0093] Optionally, the smelting sampling temperature may be 725°C, 730°C, 735°C, 740°C, 745°C, or any value between 725°C and 745°C, which is not specifically limited here.
[0094] When the smelting sampling temperature is lower than 725°C, the smelting is incomplete. When the smelting sampling temperature is higher than 745°C, the fuel is wasted and the product is prone to hydrogen absorption.
[0095] In some optional embodiments, in the step of preparing the aluminum melt, the refining temperature is between 725° C. and 740° C., and the standing time is greater than or equal to 30 minutes.
[0096] It is understandable that the purpose of refining is to remove oxide inclusions and gases from the melt.
[0097] The refining temperature is between 725°C and 740°C. For example, the refining temperature may be 725°C, 730°C, 735°C, or 740°C.
[0098] If the refining temperature is lower than 725°C, the refining is incomplete; if the refining temperature is higher than 740°C, fuel is wasted and the product is prone to hydrogen absorption.
[0099] The standing time is greater than or equal to 30 minutes. The longer the standing time is, the more thorough the removal of oxide inclusions and gases in the melt. Of course, the standing time cannot be too long. Too long a standing time will reduce production efficiency and affect production rhythm.
[0100] In some optional embodiments, a mixed gas of argon and chlorine is used in the refining step, and the amount of chlorine is 2%-5%; the refining time is 40min-60min.
[0101] The amount of chlorine can be 2%, 3%, 4%, or 5%. The refining time can be 40 min, 45 min, 50 min, 55 min, or 60 min.
[0102] It is understandable that the purpose of refining is to remove oxide inclusions and gases in the melt. The refining time is 40min-60min, which can not only remove oxide inclusions and gases in the melt more thoroughly, but also will not reduce production efficiency due to too long a time.
[0103] Chlorine is a harmful gas. If it exceeds the standard, it is harmful to the human body and easily corrodes equipment. If it is below the standard, there is no refining effect. The chlorine amount is 2%-5%, which is not easy to corrode equipment and can achieve the refining effect.
[0104] In some optional embodiments, continue to refer to Figure 1 In the casting step, the aluminum melt is injected into the ingot, and the aluminum melt is cooled through the crystallizer to form an aluminum rod. The starting casting temperature is 670℃-700℃, the starting casting speed is 135mm / min-175mm / min, the intermediate casting temperature is 680℃-710℃, the intermediate casting speed is 130mm / min-170mm / min, the water inlet temperature is 15℃-45℃, and the water flow rate is 590m 3 / h±100m 3 / h.
[0105] The temperature for starting casting is between 670°C and 700°C, for example, the temperature for starting casting is 670°C, 680°C, 690°C, or 700°C.
[0106] If the starting temperature of casting is lower than 670°C, the casting will be insufficient. If the starting temperature of casting is higher than 700°C, the grains will tend to be coarse.
[0107] The starting casting speed is between 135 mm / min and 175 mm / min. For example, the starting casting speed can be 135 mm / min, 140 mm / min, 145 mm / min, 150 mm / min, 155 mm / min, 160 mm / min, 165 mm / min, 170 mm / min, or 175 mm / min.
[0108] The casting speed is slow and the efficiency is low. If the casting speed is too fast, the surface quality of the product is poor. In this embodiment, the starting casting speed is 135mm / min-175mm / min, which can ensure both the casting efficiency and the surface quality of the product.
[0109] The intermediate casting temperature is between 680°C and 710°C. For example, the intermediate casting temperature may be 680°C, 690°C, 700°C, or 710°C.
[0110] The intermediate casting speed is between 130 mm / min and 170 mm / min, for example, the intermediate casting speed can be 130 mm / min, 135 mm / min, 140 mm / min, 145 mm / min, 150 mm / min, 155 mm / min, 160 mm / min, 165 mm / min, and 170 mm / min. The casting speed is slow, the efficiency is low, the casting speed exceeds the standard, and the product surface quality is poor. In this embodiment, the intermediate casting speed is between 130 mm / min and 170 mm / min, which can ensure both the casting efficiency and the product surface quality.
[0111] The inlet water temperature is between 15°C and 45°C, for example, the inlet water temperature can be 15°C, 20°C, 25°C, 30°C, 35°C, 40°C, and 45°C. If the water temperature is lower than 15°C, the cost will increase, and if the water temperature exceeds 45°C, the cooling effect will be poor.
[0112] Water flow at 590m 3 / h±100m 3 / h, water flow rate can be 490m 3 / h to 590m 3 Any value between / h, for example, 490m 3 / h、500m 3 / h、500m 3 / h、520m 3 / h、530m 3 / h、540m 3 / h、550m 3 / h、560m 3 / h、570m 3 / h、580m 3 / h、590m 3 / h. If the water flow rate is lower than the standard, the cooling effect is poor; if the water flow rate exceeds the standard, cracks are likely to occur.
[0113] The invention can cast aluminum rods that meet the requirements through reasonable manufacturing process.
[0114] In some optional embodiments, continue to refer to Figure 1 , the filtration is CFF bipolar plate filtration.
[0115] The present invention adopts SNIF degassing online processing, and the filtration can adopt CFF bipolar plate filtration. CFF can adopt 30PPi+50PPi, which can remove impurities and hydrogen in the aluminum liquid and improve the purity of the melt.
[0116] Based on the same inventive concept, the present invention also provides a battery housing for energy storage, which is manufactured by the production method of any of the above embodiments, referring to Figures 2 to 5 , Figure 2 is a schematic structural diagram of a battery housing for energy storage provided by the present invention, Figure 2 is a schematic structural diagram of a battery housing for energy storage provided by the present invention, Figure 3 This is a schematic diagram of the structure of a battery housing for energy storage provided by the present invention. Figure 4 is a schematic structural diagram of a battery housing for energy storage provided by the present invention, Figure 5 This is a scanning electron microscope image of the grains in the shell, and the wall thickness of the shell is less than or equal to 0.8 mm.
[0117] It should be noted that Figure 2-Figure 4 The dimensions are for illustrative purposes only and are not intended to limit the actual product. Of course, the wall thickness of the shell produced by the present invention is relatively small, less than or equal to 0.8 mm, and the minimum can reach 0.45 mm. The wall thickness of the shell of the present invention is less than or equal to 0.8 mm, which can achieve a lightweight structure of the battery pack and improve the battery energy density.
[0118] Optionally, the size of the grains in the shell is less than or equal to 100 μm.
[0119] The energy storage battery shell produced by the above method has a grain size of less than or equal to 100 μm. Since the grain structure is dense and the grain size is less than or equal to 100 μm, the shell wall thickness is small after one extrusion molding, and the shell wall thickness is less than or equal to 0.8 mm. This can achieve a lightweight structure of the battery pack and improve the battery energy density.
[0120] In some optional embodiments, referring to Figures 2 to 4 , the shell is circular or rectangular.
[0121] Figure 2 and Figure 3 The middle shell is rectangular. Figure 4 The middle shell is circular.
[0122] The energy storage battery shell produced by the above method of the present invention has high strength and tensile properties due to its dense grain structure and grain size less than or equal to 100 μm. Therefore, the shell after one-time extrusion molding can be made into different shapes as needed, such as rectangular or circular, to achieve product diversification.
[0123] In some optional embodiments, continue to refer to Figure 2 , the thickness of the shell is not equal, and the thickness at the middle of the shell is greater than the thickness at the edge of the shell.
[0124] Figure 3The thickness of the middle shell is equal. Figure 2 The thickness of the middle shell is not uniform, and the thickness at the middle of the shell is greater than the thickness at the edge of the shell. Although the thickness at the edge of the shell is smaller, due to the dense grain structure in the present invention, the strength requirements of the shell can still be guaranteed. Of course, due to the smaller thickness at the edge of the shell, the structure of the battery pack can be further lightweight and the battery energy density can be improved.
[0125] Comparison table of battery casings for energy storage in the prior art and battery casings for energy storage in the present invention
[0126] Prior art The present invention Multiple stamping passes Extrusion molding Wall thickness 0.8mm or more Wall thickness 0.8mm or less Grain size: >160μm Grain size: ≤100μm
[0127] The technical effects of the present invention are described below in conjunction with Examples 1 to 3.
[0128] Embodiment 1:
[0129] Process path: melting-casting-homogenization-extrusion
[0130] 1. Melting and Casting:
[0131] 1.1 Casting is carried out according to the internal controlled chemical composition, the chemical composition is as follows:
[0132]
[0133] The measured results of the chemical composition of this embodiment are as follows:
[0134]
[0135] 1.2 Melting temperature: 725℃-745℃;
[0136] 1.3 When the charge melts to 730°C, add ingredient additives;
[0137] 1.4 The smelting sampling temperature is 730℃;
[0138] 1.5 Refining temperature: 735℃, standing time: 30min;
[0139] 1.6 Gas refining is used for smelting, the refining gas is argon, and the refining time is 30 minutes;
[0140] 1.7 Online treatment: SNIF degassing online treatment, CFF bipolar plate filtration (30PPi+50PPi);
[0141] 1.8 Metallurgical quality control
[0142] H content: 0.12ml / 100g.Al;
[0143] Na content: 1.5ppm;
[0144] Ca content: 2.2ppm;
[0145] 2. Casting:
[0146] 2.1 Ingot specification: ¢127mm;
[0147] 2.2 Starting casting temperature: 680℃;
[0148] 2.3 Intermediate casting temperature: 690℃;
[0149] 2.4 Starting casting speed: 145mm / min;
[0150] 2.5 Intermediate casting speed: 150mm / min;
[0151] 2.6 Inlet water temperature: T = 20℃;
[0152] 2.7 Water flow: 550m3 / h;
[0153] 3. Homogenization: 622℃, 6H, strong air cooling.
[0154] 4. Extrusion
[0155] 4.1 Extrusion equipment: 1100T;
[0156] 4.2 Extrusion barrel temperature setting: 400℃;
[0157] 4.3 Mold temperature setting: 470℃;
[0158] 4.4 Aluminum rod heating temperature: 460℃;
[0159] 4.5 Extrusion adopts constant speed extrusion, filling pressure is set to 110bar, main cylinder limit pressure is 260bar, breakthrough pressure slope setting: 5sec, extrusion speed attenuation ratio: -10%, extrusion rod length: 600mm, extrusion rod speed: 7.0mm / s;
[0160] 4.6 Quenching method: air cooling;
[0161] 4.7 Straightening: 0.7%;
[0162] 4.8 Grain size detection: 90μm.
[0163] Battery case for energy storage Figure 2 .
[0164] Embodiment 2:
[0165] Process path: melting - casting - homogenization - extrusion
[0166] Casting:
[0167] 1.1 Casting is carried out according to the internal controlled chemical composition, the chemical composition is as follows:
[0168]
[0169] The measured results of chemical composition are as follows:
[0170]
[0171] 1.2 Melting temperature: 740℃
[0172] 1.3 When the charge melts to 735℃, add the ingredient additives;
[0173] 1.4 The smelting sampling temperature is 735℃;
[0174] 1.5 Refining temperature: 735℃, standing time: 40min;
[0175] 1.6 Gas refining is used for smelting, the refining gas is argon, and the refining time is 35 minutes;
[0176] 1.7 Online treatment: SNIF degassing online treatment, CFF bipolar plate filtration (30PPi+50PPi);
[0177] 1.8 Metallurgical quality control
[0178] H content: 0.13ml / 100g.Al
[0179] Na content: 1.8ppm
[0180] Ca content: 2.5ppm;
[0181] 2. Casting:
[0182] 2.1 Ingot specification: ¢127mm;
[0183] 2.2 Starting casting temperature: 685℃;
[0184] 2.3 Intermediate casting temperature: 695℃;
[0185] 2.4 Starting casting speed: 155mm / min;
[0186] 2.5 Intermediate casting speed: 160mm / min;
[0187] 2.6 Inlet water temperature: T = 20℃;
[0188] 2.7 Water flow: 580m3 / h.
[0189] 3. Homogenization: 618℃, 6H, strong air cooling.
[0190] 4. Extrusion
[0191] 4.1 Extrusion barrel temperature setting: 400℃;
[0192] 4.2 Mold temperature setting: 475℃;
[0193] 4.3 Aluminum rod heating temperature: 470℃;
[0194] 4.4 Extrusion adopts constant speed extrusion, filling pressure is set to 110bar, main cylinder limit pressure is 260bar, breakthrough pressure slope setting: 5sec, extrusion speed attenuation ratio: -5%, extrusion rod length: 800mm, extrusion rod speed: 5.0mm / s;
[0195] 4.5 Quenching method: air cooling;
[0196] 4.6 Straightening: 0.7%;
[0197] 4.7 Grain size detection: 90μm.
[0198] Battery case for energy storage Figure 3 .
[0199] Embodiment 3:
[0200] Process path: melting - casting - homogenization - extrusion
[0201] Casting:
[0202] 1.1 Casting is carried out according to the internal controlled chemical composition, the chemical composition is as follows:
[0203]
[0204] The measured results of chemical composition are as follows:
[0205]
[0206] 1.2 Melting temperature: 745℃;
[0207] 1.3 When the charge melts to 740℃, add the ingredient additives;
[0208] 1.4 The smelting sampling temperature is 735℃;
[0209] 1.5 Refining temperature: 735℃, standing time: 35min;
[0210] 1.6 Gas refining is used for smelting, the refining gas is argon, and the refining time is 40 minutes;
[0211] 1.7 Online treatment: SNIF degassing online treatment, CFF bipolar plate filtration (30PPi+50PPi);
[0212] 1.8 Metallurgical quality control
[0213] H content: 0.11ml / 100g.Al;
[0214] Na content: 1.7ppm;
[0215] Ca content: 2.8ppm.
[0216] 2. Casting:
[0217] 2.1 Ingot specification: ¢127mm;
[0218] 2.2 Starting casting temperature: 695℃;
[0219] 2.3 Intermediate casting temperature: 700℃;
[0220] 2.4 Starting casting speed: 152mm / min;
[0221] 2.5 Intermediate casting speed: 160mm / min;
[0222] 2.6 Inlet water temperature: T = 20℃;
[0223] 2.7 Water flow: 600m3 / h
[0224] 3. Homogenization:
[0225] 620℃*6H, strong air cooling
[0226] 4. Extrusion
[0227] 4.1 Extrusion barrel temperature setting: 400℃;
[0228] 4.2 Mold temperature setting: 475℃;
[0229] 4.3 Aluminum rod heating temperature: 500℃;
[0230] 4.4 Extrusion adopts constant speed extrusion, filling pressure is set to 110bar, main cylinder limit pressure is 260bar, breakthrough pressure slope setting: 5sec, extrusion speed attenuation ratio: -5%, extrusion rod length: 750mm, extrusion rod speed: 5.5mm / s;
[0231] 4.5 Quenching method: air cooling;
[0232] 4.6 Straightening: 0.7%;
[0233] 4.7 Grain size detection: 88μm.
[0234] Battery case for energy storage Figure 4 .
[0235] It can be seen from the above embodiments that the production method of the energy storage battery housing and the energy storage battery housing provided by the present invention achieve at least the following beneficial effects:
[0236] The production method of the energy storage battery shell provided by the present invention adopts a method of extruding an aluminum rod through a die to produce the energy storage battery shell in one step, thereby shortening the production process, shortening the flow, and being conducive to reducing energy consumption, improving production efficiency, and reducing production costs accordingly;
[0237] In the step of making aluminum melt, the mass percentage of each component in the master alloy is controlled as follows: Si 0.06%-0.2%, Mg <0.05%, Fe 0.3%-0.45%, Cu 0.10%-0.18%, Mn1.06%-1.20%, Cr<0.10%, Ti<0.05%, Zn<0.05%, and the balance is Al. The present invention optimizes and adjusts the content of Mn element in the alloy. Mn can increase the strength of the alloy. Controlling the Mn element content at 1.06%-1.20% can avoid forming a large amount of brittle compound MnAl6, which causes the alloy to crack easily during extrusion molding. The present invention controls the Fe element content in the alloy to 0.3%-0.45%, and the chain-like Fe phase is spheroidized after high-temperature homogenization, which can promote particle recrystallization. The present invention reduces the Si element content in the alloy. Since Si is an impurity, the impurity Si can increase the thermal cracking tendency of the alloy and reduce the casting performance, so the present invention reduces the Si element content and can improve the casting performance. The grain structure prepared by the present invention is dense.
[0238] The energy storage battery shell produced by the above method has a dense grain structure and a grain size of less than or equal to 100 μm, so the shell wall thickness is small after one extrusion molding, and the shell wall thickness is less than or equal to 0.8 mm, which can achieve a lightweight structure of the battery pack and improve the battery energy density.
[0239] Although some specific embodiments of the present invention have been described in detail by way of example, it will be appreciated by those skilled in the art that the above examples are for illustration only and are not intended to limit the scope of the present invention. It will be appreciated by those skilled in the art that the above embodiments may be modified without departing from the scope and spirit of the present invention. The scope of the present invention is defined by the appended claims.
Claims
1. A method for producing an energy storage battery shell, wherein the shell has a wall thickness of less than or equal to 0.8 mm, characterized in that: The production method of the battery shell for energy storage includes: The steps of preparing aluminum melt include: Providing a master alloy, controlling the mass percentage of each component in the master alloy: Si 0.06%-0.2%, Mg<0.05%, Fe 0.3%-0.45%, Cu 0.10%-0.18%, Mn 1.06%-1.20%, Cr<0.10%, Ti<0.05%, Zn<0.05%, and the balance is Al; Providing a furnace charge, the furnace charge comprising 20%-80% of electrolytic aluminum liquid, less than or equal to 50% of complex aluminum liquid, less than or equal to 10% of complex ingots, and the furnace charge also includes waste generated in the process of manufacturing the energy storage battery shell; The charge is placed in a smelting furnace for melting, and the smelting temperature is controlled between 720° C. and 760° C. When the charge is melted to 730° C. and 750° C., the master alloy is added; and then an aluminum melt is obtained after refining and standing; the aluminum melt is processed and filtered online by SNIF, and the hydrogen content of the aluminum melt is controlled to be less than or equal to 0.16 ml / 100 g.Al, the Na content is less than or equal to 2 ppm, and the Ca content is less than or equal to 3 ppm; A casting step, wherein the aluminum melt is cooled to form an aluminum rod; In the casting step, the aluminum melt is injected into an ingot, and the aluminum melt is cooled through a crystallizer to form an aluminum rod. The starting casting temperature is 670°C-700°C, the starting casting speed is 135mm / min-175 mm / min, the intermediate casting temperature is 680°C-710°C, the intermediate casting speed is 130mm / min-170 mm / min, the water inlet temperature is 15°C-45°C, and the water flow rate is 590 m 3 / h±100m 3 / h; Homogenizing step, the homogenizing temperature is 620℃+5℃ / 6h; The step of extruding once to obtain the energy storage battery shell comprises: extruding the aluminum rod through a die to produce the energy storage battery shell; In the step of extruding to obtain the energy storage battery shell, the temperature of the extrusion cylinder is 400°C ± 20°C, the mold temperature is 470°C ± 10°C, the aluminum rod heating temperature is 450°C-550°C, the extrusion adopts constant speed extrusion, the filling pressure is less than or equal to 110 bar, the main cylinder limit pressure is less than or equal to 260 bar, the breakthrough pressure slope is less than or equal to 5 sec, the extrusion speed attenuation ratio is -15%~-5%, the extrusion rod length is 500mm-1000mm, and the extrusion rod speed is 3.0 mm / s-7.0 mm / s; The step of quenching and cooling; The straightening step includes straightening and adjusting the energy storage battery casing.
2. The energy storage battery housing manufactured by the production method of the energy storage battery housing according to claim 1, characterized in that: In the quenching and cooling step, the quenching method is wind cooling, and the temperature of the energy storage battery shell after cooling is less than or equal to 250°C.
3. The energy storage battery housing manufactured by the production method of the energy storage battery housing according to claim 1, characterized in that: The straightening requirement is that the error is within 0.5%-1%.
4. The energy storage battery housing manufactured by the production method of the energy storage battery housing according to claim 1, characterized in that: When the waste is Class 1 waste, the mass fraction is less than or equal to 80%, and when the waste is Class 2 waste, the mass fraction is less than or equal to 20%.
5. The energy storage battery casing manufactured by the production method of the energy storage battery casing according to claim 1, characterized in that: The step of preparing the aluminum melt also includes smelting sampling, and the smelting sampling temperature is 725°C-745°C.
6. The energy storage battery casing manufactured by the production method of the energy storage battery casing according to claim 1, characterized in that: In the step of preparing the aluminum melt, the refining temperature is 725-740° C., and the standing time is greater than or equal to 30 minutes.
7. The energy storage battery casing manufactured by the production method of the energy storage battery casing according to claim 6, characterized in that: In the refining step, a mixed gas of argon and chlorine is used, and the amount of chlorine is 2%-5%; the refining time is 40min-60min.
8. The energy storage battery casing manufactured by the production method of the energy storage battery casing according to claim 1, characterized in that: The filtration is CFF bipolar plate filtration.
9. The energy storage battery casing manufactured by the production method of the energy storage battery casing according to claim 1, characterized in that: The size of the grains in the shell is less than or equal to 100 μm.
10. The energy storage battery casing manufactured by the production method of the energy storage battery casing according to claim 1, characterized in that: The shell is circular or rectangular.
11. The energy storage battery casing manufactured by the production method of the energy storage battery casing according to claim 1, characterized in that: The thickness of the shell is not equal, and the thickness at the middle of the shell is greater than the thickness at the edge of the shell.