A method for recycling graphite negative electrodes of waste lithium-ion batteries
By using a deep eutectic solvent prepared by mixing choline chloride and glucose and a heat treatment step, the problems of electrochemical performance improvement and environmental pollution of waste lithium-ion battery graphite anode materials are solved, and efficient metal impurity removal and structural repair are achieved. Improved electrochemical performance and cycle stability.
Patent Information
- Application Number
- CN202311750567.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-19
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-12-19
AI Technical Summary
It is difficult to effectively improve electrochemical performance when recycling waste lithium-ion battery graphite anode materials using existing technology, and the use of acidic reagents leads to environmental pollution and high sewage treatment costs.
The deep eutectic solvent prepared by mixing choline chloride and glucose is used to leach and wash metal impurities. Combined with heat treatment and carbonization steps, the metal impurities are effectively removed through the hydrogen bonding of the deep eutectic solvent and the graphite structure is repaired at high temperatures. Defects, improve the purity and electrochemical performance of graphite anode materials.
It improves the purity and electrochemical performance of recycled graphite anode materials, reduces sewage treatment costs, achieves efficient metal impurity removal and structural repair, and improves the material's first Coulombic efficiency and long-term cycle stability.
Smart Images

Figure CN117623301B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of recycling of waste lithium-ion batteries, and in particular relates to a method for recycling graphite negative electrodes of waste lithium-ion batteries. Background Art
[0002] Lithium-ion batteries are widely used in portable devices, electric vehicles and other electronic products due to their high operating voltage, light weight, no memory effect and long cycle life. At the same time, the number of retired lithium-ion batteries is also growing rapidly. Waste lithium-ion batteries contain a variety of resources including lithium, cobalt, nickel, graphite, etc., and have high recycling value. Recycling key materials (such as graphite, valuable metals, etc.) in retired batteries is of great significance to sustainable development such as economic growth and environmental protection.
[0003] The main component of the negative electrode material of waste lithium-ion batteries is graphite. After a long period of charge and discharge cycles, graphite particles will produce a large number of structural defects and bulk impurities, which greatly affect the battery's life and other electrochemical properties. Therefore, how to improve the electrochemical performance of the negative electrode material recycled from graphite materials in waste batteries is the main problem currently faced.
[0004] In addition, the waste graphite negative electrode contains a large amount of metal element impurities. The current common impurity treatment method is mainly acid leaching. However, the large-scale use of acidic reagents can easily cause serious pollution to the environment, and the cost of subsequent sewage treatment is high. Therefore, it is necessary to solve the defects of the above-mentioned prior art. Summary of the invention
[0005] The present invention aims to solve the technical problems existing in the above-mentioned prior art. To this end, the present invention provides a method for recycling and regenerating graphite negative electrodes of waste lithium-ion batteries, the method comprising the following steps:
[0006] (1) Pre-treating waste lithium-ion batteries to obtain negative electrode material powder;
[0007] (2) heat-treating the negative electrode material powder in an air or oxygen atmosphere to oxidize metal impurities in the negative electrode material powder, then cooling to room temperature, and sieving to obtain graphite negative electrode material powder;
[0008] (3) mixing and stirring choline chloride and glucose at a molar ratio of 1:1-1:2.5 in a water bath to obtain a clear and transparent deep eutectic solvent, and dividing the deep eutectic solvent into two parts, solvent A and solvent B;
[0009] (4) adding the graphite negative electrode material powder obtained by screening in step (2) to the solvent A in step (3), heating, stirring and mixing, leaching the metal oxide in the graphite negative electrode material powder, and then separating the solid and the liquid, and collecting the solid;
[0010] (5) Using the solvent B to wash the solid in step (4), directly transferring the washed solid to a sintering device without drying, and heat-treating and carbonizing it under an inert atmosphere to obtain a regenerated graphite negative electrode material.
[0011] Furthermore, the waste lithium-ion battery is pretreated in step (1), including disassembling the waste lithium-ion battery in an argon atmosphere to obtain a negative electrode sheet, immersing the negative electrode sheet in deionized water for ultrasonic treatment to separate the copper foil current collector from the negative electrode material, and filtering, washing, and drying the negative electrode material to obtain a negative electrode material powder.
[0012] Furthermore, the heat treatment temperature in step (2) is 300-500° C., and the heat treatment time is 3-12 h.
[0013] Furthermore, the particle size of the graphite negative electrode material powder obtained by screening in step (2) is below 25-70 μm.
[0014] Furthermore, the water bath temperature in step (3) is 40-60°C;
[0015] Furthermore, the stirring time in step (3) is 30-60 min.
[0016] Furthermore, in step (4), the graphite negative electrode material powder and the solvent A are mixed at a solid-liquid ratio of 10-30 g / L.
[0017] Furthermore, in step (4), the heating and stirring temperature is 60-250° C., and the stirring time is 3-24 h.
[0018] Furthermore, the inert atmosphere in step (5) is any one or more of helium, argon, and nitrogen.
[0019] Furthermore, the temperature of the heat treatment carbonization in step (5) is 2500-3000°C, and the heat treatment time is 2-6h.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] (1) When recycling the regenerated graphite negative electrode material, the present invention uses a deep eutectic solvent prepared by mixing choline chloride and glucose as a leaching agent for metal element impurities. Glucose serves as a hydrogen bond donor and choline chloride serves as a hydrogen bond acceptor. The eutectic solvent has a good solvating effect on metal oxides within a certain temperature range, and can effectively leach metal element impurities in the graphite negative electrode material powder, thereby improving the purity of the recycled graphite. In addition, while ensuring the impurity removal effect, the use of acid solution is avoided, thereby reducing the burden of sewage treatment.
[0022] (2) The present invention divides the deep eutectic solvent into two parts, one part is used to remove metal elements in the graphite negative electrode material powder, and the other part is used to wash the solid obtained after the leaching reaction and solid-liquid separation. Since the washing reagent and the leaching reagent are both deep eutectic solvents, it is beneficial to improve the washing effect on the solid.
[0023] (3) The present invention uses a deep eutectic solvent B (also known as a washing reagent) to wash the leached solid. Choline chloride and glucose in the deep eutectic solvent are adsorbed on the solid surface. The washed solid is directly transferred to a sintering device without drying. The choline chloride and glucose adsorbed on the solid surface can be used as a carbon source and graphitized at high temperature to repair the structural defects in the graphite negative electrode, thereby improving the electrochemical performance of the recycled graphite negative electrode material.
[0024] (4) The graphite negative electrode material recovered and regenerated by the present invention has excellent electrochemical performance, good first coulombic efficiency and long cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is the SEM image of the regenerated graphite negative electrode material obtained in Example 1. DETAILED DESCRIPTION
[0026] The present invention is further described below with reference to examples and comparative examples. Example 1
[0027] Dismantle the waste lithium cobalt oxide battery in an argon atmosphere to obtain a negative electrode sheet, soak the negative electrode sheet in deionized water for ultrasonic treatment to separate the copper foil current collector from the negative electrode material, and filter, wash, and dry the negative electrode material to obtain a negative electrode material powder. Heat treat the negative electrode material powder at 500° C. for 3 hours in an air atmosphere to oxidize metal impurities in the negative electrode material powder, then cool to room temperature, and sieve through a sieve to obtain a graphite negative electrode material powder with a particle size of less than 25 μm.
[0028] Under the condition of 60°C water bath, choline chloride and glucose were mixed and stirred for 30 minutes at a molar ratio of 1:1 to obtain a clear and transparent deep eutectic solvent, and the deep eutectic solvent was divided into two parts, solvent A and solvent B. The graphite negative electrode material powder obtained by screening was added to the solvent A, and the graphite negative electrode material powder and the solvent A were mixed at a solid-liquid ratio of 10g / L, heated to 250°C and stirred for 3h, and the metal oxides in the graphite negative electrode material powder were leached, and then filtered to collect the solid; the filtered solid was washed with solvent B, and the washed solid was directly transferred to a muffle furnace without drying, and heat-treated at 2500°C for graphitization under a nitrogen atmosphere, and kept warm for 6h to obtain a regenerated graphite negative electrode material.
[0029] The obtained regenerated graphite negative electrode material was analyzed by ICP, and the results are shown in Table 1 below.
[0030] Table 1 ICP analysis results of graphite negative electrode material powder
[0031] element Co Cu Li Impurity content (wt.%) 0.0004 0.0008 0.0013
[0032] And through testing with carbon-sulfur analysis equipment, the carbon content in the recycled graphite negative electrode material is 99.7wt.%. Example 2
[0033] Dismantle the waste nickel-cobalt-manganese-oxide lithium ternary lithium battery in an argon atmosphere to obtain a negative electrode sheet, soak the negative electrode sheet in deionized water for ultrasonic treatment to separate the copper foil current collector from the negative electrode material, and filter, wash, and dry the negative electrode material to obtain a negative electrode material powder. Heat treat the negative electrode material powder at 300° C. for 12 hours in an air atmosphere to oxidize metal impurities in the negative electrode material powder, then cool to room temperature, and sieve through a sieve to obtain a graphite negative electrode material powder with a particle size of less than 45 μm.
[0034] Under the condition of a 50°C water bath, choline chloride and glucose were mixed and stirred for 45 minutes at a molar ratio of 1:2 to obtain a clear and transparent deep eutectic solvent, and the deep eutectic solvent was divided into two parts, solvent A and solvent B. The graphite negative electrode material powder obtained by screening was added to the solvent A, and the graphite negative electrode material powder and the solvent A were mixed at a solid-liquid ratio of 20g / L, heated to 160°C and stirred for 12h, and the metal oxides in the graphite negative electrode material powder were leached, and then centrifuged to collect the solid; the solid obtained by centrifugation was washed with solvent B, and the washed solid was directly transferred to a muffle furnace without drying, and heat-treated at 3000°C for graphitization under a nitrogen atmosphere, and kept warm for 3h to obtain a regenerated graphite negative electrode material.
[0035] The obtained regenerated graphite negative electrode material was analyzed using ICP, and the results are shown in Table 2 below.
[0036] Table 2 ICP analysis results of graphite negative electrode material powder
[0037] element Co Ni Mn Cu Li Impurity content (wt.%) 0.0005 0.0004 0.0005 0.0007 0.0016
[0038] And through carbon-sulfur analysis equipment testing, the carbon content in the recycled graphite negative electrode material is 99.5 wt.%. Example 3
[0039] Dismantle the waste lithium manganese oxide battery in an argon atmosphere to obtain a negative electrode sheet, soak the negative electrode sheet in deionized water for ultrasonic treatment to separate the copper foil current collector from the negative electrode material, and filter, wash, and dry the negative electrode material to obtain a negative electrode material powder. Heat treat the negative electrode material powder at 400° C. for 6 hours in an air atmosphere to oxidize metal impurities in the negative electrode material powder, then cool to room temperature, and sieve through a sieve to obtain a graphite negative electrode material powder with a particle size of less than 70 μm.
[0040] Under 40°C water bath conditions, choline chloride and glucose were mixed and stirred for 60 minutes at a molar ratio of 1:2.5 to obtain a clear and transparent deep eutectic solvent, and the deep eutectic solvent was divided into two parts, solvent A and solvent B. The graphite negative electrode material powder obtained by screening was added to the solvent A, and the graphite negative electrode material powder and the solvent A were mixed at a solid-liquid ratio of 30g / L, heated to 60°C and stirred for 24h, and the metal oxides in the graphite negative electrode material powder were leached, and then filtered to collect the solid; the filtered solid was washed with solvent B, and the washed solid was directly transferred to a muffle furnace without drying, and heat-treated at 3000°C for graphitization under an argon atmosphere, and kept warm for 4h to obtain a regenerated graphite negative electrode material.
[0041] The obtained regenerated graphite negative electrode material was analyzed using ICP, and the results are shown in Table 3 below.
[0042] Table 3 ICP analysis results of graphite negative electrode material powder
[0043] element Mn Cu Li Impurity content (wt.%) 0.0009 0.0006 0.0018
[0044] And through testing with carbon-sulfur analysis equipment, the carbon content in the recycled graphite negative electrode material is 99.6wt.%.
[0045] Comparative Example
[0046] Dismantle the waste lithium cobalt oxide battery in an argon atmosphere to obtain a negative electrode sheet, soak the negative electrode sheet in deionized water for ultrasonic treatment to separate the copper foil current collector from the negative electrode material, and filter, wash, and dry the negative electrode material to obtain a negative electrode material powder. Heat treat the negative electrode material powder at 500° C. for 3 hours in an air atmosphere to oxidize metal impurities in the negative electrode material powder, then cool to room temperature, and sieve through a sieve to obtain a graphite negative electrode material powder with a particle size of less than 25 μm.
[0047] The graphite negative electrode material powder obtained by screening is added to a 1 mol / L hydrochloric acid solution, the graphite negative electrode material powder and the hydrochloric acid solution are mixed at a solid-liquid ratio of 10 g / L, stirred for 3 hours, and then filtered to collect the solid; the filtered solid is washed with deionized water, and the washed solid is directly transferred to a muffle furnace without drying, and heat-treated at 2500°C for graphitization under a nitrogen atmosphere, and kept warm for 6 hours to obtain a graphite negative electrode material.
[0048] Battery performance test
[0049] The graphite negative electrode material obtained in the above examples 1-3 and the comparative example was made into an electrode slurry, and the slurry ratio was graphite negative electrode material: binder (PAA): conductive agent (SP) = 75:15:10. The slurry was evenly stirred and coated on a copper foil, and then dried under vacuum. The dried electrode sheet was punched out as the working electrode of the button battery, the lithium sheet was used as the counter electrode, and the electrolyte was 1 mol / L lithium hexafluorophosphate (LiPF6) electrolyte dissolved in ethylene carbonate (EC) and diethyl carbonate (DEC) solvents with a volume ratio of 1:1. The constant current charge and discharge voltage range was 0.01~1.5V. The current density used for the first charge and discharge cycle experiment was 0.1C, and the first charge and discharge coulomb efficiency of the battery was tested at this current density; the current density used for the long cycle test was 1C.
[0050] The test results are shown in Table 4 below.
[0051] Table 4
[0052] <![CDATA[Initial discharge specific capacity (mAh·g -1 )]]> First coulombic efficiency Capacity retention after 500 cycles at 1C Example 1 356.8 91.3% 95.2% Example 2 354.3 90.1% 96.4% Example 3 353.9 92.3% 96.1% Comparative Example 298.6 83.6% 82.5%
Claims
1. A method for recycling graphite negative electrodes of waste lithium-ion batteries, characterized in that: The following steps are involved: (1) pre-treating the waste lithium-ion batteries, including disassembling the waste lithium-ion batteries in an argon atmosphere to obtain negative electrode sheets, immersing the negative electrode sheets in deionized water for ultrasonic treatment to separate the copper foil current collector from the negative electrode material, and filtering, washing, and drying the negative electrode material to obtain negative electrode material powder; (2) heat-treating the negative electrode material powder in an air or oxygen atmosphere to oxidize metal impurities in the negative electrode material powder, then cooling to room temperature, and sieving to obtain graphite negative electrode material powder; (3) mixing and stirring choline chloride and glucose in a water bath at a temperature of 40-60° C. and a molar ratio of 1:1-1:2.5 for 30-60 min to obtain a clear and transparent deep eutectic solvent, and dividing the deep eutectic solvent into two parts, solvent A and solvent B; (4) adding the graphite negative electrode material powder obtained by screening in step (2) to the solvent A in step (3), mixing the graphite negative electrode material powder and the solvent A at a solid-liquid ratio of 10-30 g / L, heating and stirring the mixture, wherein the heating and stirring temperature is 60-250° C., and the stirring time is 3-24 h; leaching the metal oxide in the graphite negative electrode material powder, and then separating the solid and the liquid, and collecting the solid; (5) Using the solvent B to wash the solid in step (4), directly transferring the washed solid to a sintering device without drying, and heat-treating and carbonizing it under an inert atmosphere to obtain a regenerated graphite negative electrode material; the inert atmosphere is any one or more of helium, argon, and nitrogen; the temperature of the heat treatment carbonization is 2500-3000°C, and the heat treatment time is 2-6h.
2. The method according to claim 1, characterized in that The heat treatment temperature in step (2) is 300-500°C, and the heat treatment time is 3-12h.
3. The method according to claim 1, characterized in that The particle size of the graphite negative electrode material powder obtained by screening in step (2) is 25-70 μm.
Citation Information
Patent Citations
Direct regeneration method for treating waste graphite by using eutectic solvent
CN115051062A
Lithium battery graphite negative electrode regeneration method
CN115954572A
Method for recycling valuable metal in positive electrode material of waste lithium ion battery by using natural eutectic solvent
CN116732322A