A method for photocuring additive manufacturing of transparent zirconia ceramic brackets
Through photocuring additive manufacturing technology and the design of lithium disilicate glass ceramic layer, the problems of low strength and poor bonding performance of alumina brackets are solved, and the flexural strength and tooth bonding of transparent zirconia ceramic brackets are improved. Performance improves the effectiveness of correction treatment and patient comfort.
Patent Information
- Application Number
- CN202410135539.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-31
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-01-31
AI Technical Summary
The existing transparent ceramic bracket material uses alumina, which has low strength, high friction, insufficient flexural strength, and poor adhesive performance with teeth, which affects the effect of correction treatment and patient comfort.
Using photocuring additive manufacturing technology, transparent zirconia ceramic brackets are prepared. The design of graded zirconia particles and photocuring additive manufacturing paste is improved by combining the adhesion of lithium disilicate glass ceramic layer. and bonding properties.
Achieve higher flexural strength and light transmittance, reduce correction treatment cycles, improve tooth bonding performance, and enhance bracket comfort and strength of use.
Smart Images

Figure CN117944142B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to oral medical treatment, and in particular to a method for photocuring additive manufacturing of a transparent zirconia ceramic bracket. Background Art
[0002] A bracket is a medical device used to fix and correct teeth. The bracket is bonded to the surface of the crown with adhesive, so that the archwire can be fixedly connected through the bracket to apply various types of corrective forces to the teeth, thereby achieving the purpose of orthodontic correction of teeth.
[0003] Stainless steel is the most common material for brackets because it is easy to shape and has a low cost. However, stainless steel brackets have the following problems: 1. The color difference between stainless steel and teeth is too large, which makes the patient look ugly during treatment and affects the patient's mental health; 2. Some patients may suffer from metal allergies, so these patients are not suitable for wearing stainless steel brackets; 3. Long-term wearing of stainless steel brackets may cause metal poisoning in patients. In order to solve the above problems, with the development of technology, ceramic brackets have gradually appeared on the market.
[0004] If distinguished by color, the existing ceramic brackets can be divided into two categories: white ceramic brackets and transparent ceramic brackets. Since the color of each patient's teeth is different, patients may still have unsightly appearance after wearing white ceramic brackets, which affects their mental health. In comparison, transparent ceramic brackets can be used for more patients, taking care of the patient's mental health as much as possible during the treatment and correction period, laying the foundation for obtaining better correction treatment results.
[0005] The existing transparent ceramic brackets have the following problems: 1. The material of the existing transparent ceramic brackets is mostly alumina, which has the disadvantages of low strength and large friction of the grooves, limiting its application. The flexural strength of alumina is not high, less than half of that of zirconia. Therefore, the thickness of the alumina bracket is relatively thick, and the comfort of the patient to wear is relatively poor; 2. The existing zirconia ceramic brackets have poor bonding performance with teeth, and the brackets may fall off during the patient's orthodontic treatment, prolonging the patient's orthodontic treatment cycle; 3. The existing zirconia brackets have a tetragonal phase (t phase) crystal structure after sintering, and have poor light transmittance. Summary of the invention
[0006] Purpose of the invention: The purpose of the present invention is to provide a method for manufacturing a transparent zirconia ceramic bracket using a light-curing additive manufacturing technology.
[0007] Technical solution: The method for photocuring additive manufacturing of transparent zirconia ceramic brackets described in the present invention comprises the following steps:
[0008] Step 1: prepare a light-curing additive manufacturing paste with a solid content G ≥ 58 vol% (volume ratio, i.e., the total volume of zirconium oxide particles accounts for more than 58% of the light-curing additive manufacturing paste), and place the light-curing additive manufacturing paste into a vacuum machine for vacuum degassing;
[0009] Step 2: Put the light-curing additive manufacturing paste after vacuum degassing in the first step into the additive manufacturing equipment for light-curing forming to obtain a green body;
[0010] Step 3: putting the green body obtained after the second step into an ultrasonic cleaning device for cleaning, and drying after cleaning to obtain a dried green body;
[0011] Step 4: placing the dried green body obtained after the third step into a first heating device for thermal degreasing, wherein the air pressure in the first heating device is normal pressure, the temperature in the first heating device is increased from room temperature to 200°C, and the heating rate is 1.7-2.3°C / min; the temperature is increased from 200°C to 350°C, and the heating rate is 0.8-1.2°C / min; the temperature is kept at 350°C for 1 hour; the temperature is increased from 350°C to 400°C, and the heating rate is 0.8-1.2°C / min; the temperature is kept at 400°C for 1 hour; the temperature is increased from 400°C to 600°C, and the heating rate is 1.8-2.3°C / min;
[0012] Step 5: Pre-sintering: pure oxygen is introduced into the first heating device at 600°C (oxygen is introduced for carbon removal, and the carbon removal effect is better in a pure oxygen environment), the temperature in the first heating device is increased from 600°C to 1350°C, and the heating rate is 2-4°C / min; keep warm at 1350°C for 1 hour; then the temperature in the first heating device is reduced from 1350°C to 1000°C, and the cooling rate is 1.9-2.4°C / min, and then cooled with the furnace to obtain the pre-sintered bracket matrix;
[0013] Step 6: Sintering, placing the pre-sintered bracket substrate obtained after the fifth step into a hot isostatic pressing furnace, wherein the atmosphere in the hot isostatic pressing furnace is pure argon, the gas pressure in the hot isostatic pressing furnace is 190 MPa to 220 MPa, the temperature in the hot isostatic pressing furnace is increased from room temperature to 1250° C., the heating rate is 1.5 to 3° C. / min, and the temperature is kept at 1250° C. for 4 hours to obtain a sintered bracket substrate;
[0014] Step 7: annealing, placing the sintered bracket substrate obtained after the sixth step into a second heating device, wherein the atmosphere in the second heating device is air at normal pressure, the temperature in the second heating device is 1200° C., the annealing time is 2 hours, and then the bracket is cooled with the furnace to obtain a cooled bracket. The purpose of annealing is to eliminate oxygen vacancies in the bracket substrate;
[0015] Step 8: A lithium disilicate glass ceramic layer is attached to the bonding surface of the bracket base obtained after the seventh step.
[0016] Furthermore, the steps of preparing the light-curing additive manufacturing paste in the first step are as follows:
[0017] The photosensitive resin premix is mixed with the photoinitiator, and then the graded zirconium oxide particles and the surfactant are added in sequence three times. After each addition of the graded zirconium oxide particles and the surfactant, the mixture is placed in a homogenizer for homogenization. After all the graded zirconium oxide particles and the surfactant are added, the mixture is placed in a roller press for rolling to obtain a rolled mixture. A rheological additive is added to the rolled mixture to adjust its rheological properties to obtain a photocurable additive manufacturing paste. The photocurable additive manufacturing paste is placed in a vacuum machine for vacuum degassing. The photocurable additive manufacturing paste after the rheological properties are adjusted has no fluidity without external force, which makes it possible for the photocurable additive manufacturing paste to be used without support in subsequent photocurable additive manufacturing, and is convenient for cleaning, support removal and other operations after photocurable additive manufacturing, thereby reducing damage to the green body.
[0018] Furthermore, the amount of the graded ceramic particles added for the third time is 10% of the total mass of the graded ceramic particles.
[0019] Furthermore, the mass of the graded ceramic particles added for the first time is greater than the mass of the graded ceramic particles added for the second time.
[0020] Furthermore, the mass of the graded ceramic particles added for the first time is 50% of the total mass of the graded ceramic particles, and the mass of the graded ceramic particles added for the second time is 40% of the total mass of the graded ceramic particles.
[0021] Furthermore, the rheological additive is any one of polyvinyl alcohol, polyacrylic acid, modified urea solution, and hydroxypropyl methylcellulose, and the mass of the rheological additive is 0.1% to 0.5% of the total mass of the photocurable additive manufacturing paste.
[0022] Furthermore, the graded zirconia particles are a mixture of zirconia particles with a particle size of 200 nanometers and zirconia particles with a particle size of 5 to 25 micrometers, and the mass ratio of the zirconia particles with a particle size of 200 nanometers to the zirconia particles with a particle size of 5 to 25 micrometers is 3:1 to 2:1.
[0023] Furthermore, the zirconium oxide particles with a particle size of 5 to 25 microns are obtained by spray granulation of zirconium oxide powder with an original particle size of 20 to 50 nanometers.
[0024] Furthermore, the zirconia particles with a particle size of 200 nanometers are 5 mol% yttria-stabilized zirconia particles, and the zirconia powders with an original particle size of 20 nanometers to 50 nanometers are all 5 mol% yttria-stabilized zirconia powders. The use of 5 mol% yttria-stabilized zirconia has a higher yttria content, and more cubic phase (c-phase) crystal structures can be generated after sintering, which can achieve higher light transmittance.
[0025] Furthermore, the parameters of the additive manufacturing equipment in the second step are a light intensity of 130 to 150 mW, a laser printing speed of 1000 to 7000 mm / s, a printing spacing of 0.01 mm to 0.03 mm, and a printing layer thickness of 25 to 50 μm.
[0026] Furthermore, in the third step, the ultrasonic cleaning device is internally filled with pure resin monomer to perform ultrasonic cleaning on the green body.
[0027] Furthermore, in the eighth step, the steps of attaching and setting a lithium disilicate glass ceramic layer on the bonding surface of the obtained bracket base are as follows:
[0028] A: Spraying lithium disilicate glass ceramic solution onto the bonding surface of the bracket base obtained after step 8;
[0029] B: Place the bracket sprayed with lithium disilicate glass ceramic solution into the third heating device, the temperature of the third heating device is raised from room temperature to 1500°C, the heating rate is 1.8-2.3°C / min, keep warm for 0.5-2 hours, then take it out and cool it at room temperature. In order to improve the adhesion to teeth, the existing brackets mainly achieve adhesion to teeth by setting a surface-increasing structure on the bonding surface (such as setting a number of grooves or protrusions), and then setting an adhesive layer on the bonding surface, but the surface-increasing structure will reduce the use strength of the bracket, and the bonding strength of the traditional adhesive layer to the teeth is low. The present invention instead sets a lithium disilicate glass ceramic layer on the bonding surface of the bracket substrate, and part of the lithium disilicate glass ceramic layer will react with zirconium oxide at high temperature and penetrate into the interior, modifying the surface of zirconium oxide, thereby improving the bonding performance of the ceramic bracket and the tooth surface.
[0030] Furthermore, the pressure of spraying the lithium disilicate glass ceramic solution is 0.1 MPa to 0.8 MPa.
[0031] Furthermore, the raw materials of the lithium disilicate glass ceramic solution include lithium carbonate, silicon oxide, phosphorus pentoxide, zirconium oxide and aluminum oxide.
[0032] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: 1. The present invention adopts the technology of light-curing additive manufacturing to manufacture brackets, which can be customized according to the different shapes of the patient's teeth and fit the patient's teeth better; 2. The present invention adopts graded zirconium oxide particles, which are a mixture of zirconium oxide particles with a particle size of 200 nanometers and zirconium oxide particles with a particle size of 5 to 25 micrometers, and the zirconium oxide particles of 5 to 25 micrometers are obtained by spray granulation of zirconium oxide powder with an original particle size of 20 nanometers to 50 nanometers. The original particle size of 20 nanometers to 50 nanometers is highly active, and the spray The zirconia particles of 5 to 25 microns obtained after granulation have a small specific surface area and are easier to disperse in subsequent processes. Therefore, the graded zirconia particles have the advantages of high activity and good dispersibility, are easier to sinter, and not only have higher flexural strength than alumina brackets, but also have a greatly shortened preparation cycle compared to existing zirconia brackets, and have higher light transmittance; 3. A lithium disilicate glass-ceramic layer is attached to the bonding surface of the present invention, which can improve the bonding performance between the bracket and the patient's teeth, prevent the bracket from falling off during orthodontic treatment, improve the patient's treatment comfort, and reduce the cost of orthodontic treatment. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 It is a flow chart of the present invention.
[0034] Figure 2 It is a time trend diagram of thermal debinding and sintering of the present invention.
[0035] Figure 3 It is a stereoscopic diagram of the bracket obtained after the present invention.
[0036] Figure 4 It is a cross-sectional view of the bracket obtained after the present invention.
[0037] Figure 5 This is the XRD pattern of 5 mol % yttria-stabilized zirconia used in the present invention.
[0038] Figure 6 This is a SEM image of 5 mol % yttria-stabilized zirconia used in the present invention.
[0039] Wherein: 1. substrate; 101. groove; 102. lithium disilicate glass ceramic layer. DETAILED DESCRIPTION
[0040] The technical solution of the present invention is further described below in conjunction with the accompanying drawings.
[0041] Example 1
[0042] See attached Figure 1 to Figure 6 The present invention provides a method for light-curing additive manufacturing of a transparent zirconia ceramic bracket, the steps of which are as follows:
[0043] The first step is to mix the photosensitive resin premix with the photoinitiator, and then add the graded zirconium oxide particles and the surfactant in three times in sequence. The graded zirconium oxide particles are a mixture of 5 mol% yttria-stabilized zirconium oxide particles with a particle size of 200 nanometers and 5 mol% yttria-stabilized zirconium oxide particles with a particle size of 5 to 25 microns. The mass ratio of the 5 mol% yttria-stabilized zirconium oxide particles with a particle size of 200 nanometers to the 5 mol% yttria-stabilized zirconium oxide particles with a particle size of 5 to 25 microns is 2.5:1, wherein the 5 mol% yttria-stabilized zirconium oxide particles with a particle size of 5 to 25 microns are 5 mol% yttria-stabilized zirconium oxide particles with an original particle size of 20 nanometers to 50 nanometers. Yttria-stabilized zirconia powder is obtained by spray granulation; the amount of graded ceramic particles added three times is 45%, 45% and 10% of the total mass of the graded ceramic particles respectively, and the graded zirconia particles and surfactant are added each time and then put into a homogenizer for homogenization, and when all the graded zirconia particles and surfactant are added, they are put into a roller press to obtain a roller-pressed mixture, and polyvinyl alcohol is added to the roller-pressed mixture to adjust its rheological properties, and the mass of the polyvinyl alcohol is 0.3% of the total mass of the photocurable additive manufacturing paste, so as to obtain a photocurable additive manufacturing paste with a solid content G ≥ 58 vol%, and the photocurable additive manufacturing paste is placed in a vacuum machine for vacuum degassing;
[0044] Step 2: Place the light-curing additive manufacturing paste after vacuum degassing in the first step into the additive manufacturing equipment for light-curing forming. The parameters of the additive manufacturing equipment are light intensity of 140mW, laser printing speed of 5000mm / s, printing spacing of 0.01mm, and printing layer thickness of 30μm to obtain a green body;
[0045] Step 3: Place the green body obtained after the second step into an ultrasonic cleaning device for cleaning for 5 seconds. The ultrasonic cleaning device contains pure resin monomers to perform ultrasonic cleaning on the green body. After cleaning, the green body is dried under room temperature wind to obtain a dried green body.
[0046] Step 4: placing the dried green body obtained after the third step into the first heating device for thermal debinding, the air pressure in the first heating device is normal pressure, the temperature in the first heating device is increased from room temperature to 200°C, the heating rate is 2°C / min; the temperature is increased from 200°C to 350°C, the heating rate is 1°C / min; the temperature is kept at 350°C for 1 hour; the temperature is increased from 350°C to 400°C, the heating rate is 1°C / min; the temperature is kept at 400°C for 1 hour; the temperature is increased from 400°C to 600°C, the heating rate is 2°C / min;
[0047] Step 5: Pre-sintering: pure oxygen is introduced into the first heating device at 600°C, and the temperature in the first heating device is increased from 600°C to 1350°C at a heating rate of 3°C / min; the temperature is kept at 1350°C for 1 hour; then the temperature in the first heating device is reduced from 1350°C to 1000°C at a cooling rate of 2.2°C / min, and then cooled with the furnace to obtain a pre-sintered bracket matrix;
[0048] Step 6: Sintering, the pre-sintered bracket substrate obtained after the fifth step is placed in a hot isostatic pressing furnace, the atmosphere in the hot isostatic pressing furnace is pure argon, the gas pressure in the hot isostatic pressing furnace is 210 MPa, the temperature in the hot isostatic pressing furnace is increased from room temperature to 1250°C, the heating rate is 2.5°C / min, and the temperature is kept at 1250°C for 4 hours to obtain a sintered bracket substrate;
[0049] Step 7: annealing, placing the sintered bracket substrate obtained after the sixth step into a second heating device, the atmosphere in the second heating device is air at normal pressure, the temperature in the second heating device is 1200° C., the annealing time is 2 hours, and then the bracket is cooled with the furnace to obtain a cooled bracket;
[0050] Step 8: Spray lithium disilicate glass ceramic solution onto the bonding surface of the bracket base obtained after the seventh step. The pressure of spraying the lithium disilicate glass ceramic solution is 0.5 MPa. Put the bracket sprayed with the lithium disilicate glass ceramic solution into the third heating device. The temperature of the third heating device is increased from room temperature to 1500°C at a heating rate of 2°C / min. The temperature is kept for 1.5 hours, and then taken out and cooled at room temperature. The raw materials of the lithium disilicate glass ceramic solution include lithium carbonate, silicon oxide, phosphorus pentoxide, zirconium oxide and aluminum oxide.
[0051] Example 2
[0052] See attached Figure 1 to Figure 6 The present invention provides a method for light-curing additive manufacturing of a transparent zirconia ceramic bracket, the steps of which are as follows:
[0053] The first step is to mix the photosensitive resin premix with the photoinitiator, and then add the graded zirconium oxide particles and the surfactant in three times in sequence. The graded zirconium oxide particles are a mixture of 5 mol% yttria-stabilized zirconium oxide particles with a particle size of 200 nanometers and 5 mol% yttria-stabilized zirconium oxide particles with a particle size of 5 to 25 microns. The mass ratio of the 5 mol% yttria-stabilized zirconium oxide particles with a particle size of 200 nanometers to the 5 mol% yttria-stabilized zirconium oxide particles with a particle size of 5 to 25 microns is 3:1 to 2:1, wherein the 5 mol% yttria-stabilized zirconium oxide particles with a particle size of 5 to 25 microns are 5 mol% yttria-stabilized zirconium oxide particles with an original particle size of 20 nanometers to 50 nanometers. The yttria-stabilized zirconia powder is obtained by spray granulation; the amount of the graded ceramic particles added three times is 60%, 30% and 10% of the total mass of the graded ceramic particles respectively, and the graded zirconia particles and the surfactant are added each time and then put into a homogenizer for homogenization, and when all the graded zirconia particles and the surfactant are added, they are put into a roller press to obtain a roller-pressed mixture, and a modified urea solution is added to the roller-pressed mixture to adjust its rheological properties, and the mass of the modified urea solution is 0.45% of the total mass of the photocurable additive manufacturing paste, thereby obtaining a photocurable additive manufacturing paste with a solid content G ≥ 58 vol%, and the photocurable additive manufacturing paste is placed in a vacuum machine for vacuum degassing;
[0054] Step 2: Place the light-curing additive manufacturing paste after vacuum degassing in the first step into the additive manufacturing equipment for light-curing forming. The parameters of the additive manufacturing equipment are light intensity of 120mW, laser printing speed of 4000mm / s, printing spacing of 0.01mm, and printing layer thickness of 45μm to obtain a green body;
[0055] Step 3: Place the green body obtained after the second step into an ultrasonic cleaning device for cleaning for 5 seconds. The ultrasonic cleaning device contains pure resin monomers to perform ultrasonic cleaning on the green body. After cleaning, the green body is dried under room temperature wind to obtain a dried green body.
[0056] Step 4: placing the dried green body obtained after the third step into the first heating device for thermal debinding, the air pressure in the first heating device is normal pressure, the temperature in the first heating device is increased from room temperature to 200°C, the heating rate is 1.9°C / min; the temperature is increased from 200°C to 350°C, the heating rate is 0.9°C / min; the temperature is kept at 350°C for 1 hour; the temperature is increased from 350°C to 400°C, the heating rate is 0.85°C / min; the temperature is kept at 400°C for 1 hour; the temperature is increased from 400°C to 600°C, the heating rate is 1.95°C / min;
[0057] Step 5: Pre-sintering: pure oxygen is introduced into the first heating device at 600°C, and the temperature in the first heating device is increased from 600°C to 1350°C at a heating rate of 3.5°C / min; the temperature is kept at 1350°C for 1 hour; then the temperature in the first heating device is reduced from 1350°C to 1000°C at a cooling rate of 1.85°C / min, and then cooled with the furnace to obtain a pre-sintered bracket matrix;
[0058] Step 6: Sintering, the pre-sintered bracket substrate obtained after the fifth step is placed in a hot isostatic pressing furnace, the atmosphere in the hot isostatic pressing furnace is pure argon, the gas pressure in the hot isostatic pressing furnace is 220 MPa, the temperature in the hot isostatic pressing furnace is increased from room temperature to 1250°C, the heating rate is 1.8°C / min, and the temperature is kept at 1250°C for 4 hours to obtain a sintered bracket substrate;
[0059] Step 7: annealing, placing the sintered bracket substrate obtained after the sixth step into a second heating device, the atmosphere in the second heating device is air at normal pressure, the temperature in the second heating device is 1200° C., the annealing time is 2 hours, and then the bracket is cooled with the furnace to obtain a cooled bracket;
[0060] Step 8: Spray lithium disilicate glass ceramic solution onto the bonding surface of the bracket obtained after the seventh step. The pressure of spraying the lithium disilicate glass ceramic solution is 0.6MPa. Put the bracket sprayed with the lithium disilicate glass ceramic solution into the third heating device. The temperature of the heating device is increased from room temperature to 1500°C at a heating rate of 1.85°C / min. The temperature is kept for 0.5 to 2 hours, and then taken out and cooled at room temperature. The raw materials of the lithium disilicate glass ceramic solution include lithium carbonate, silicon oxide, phosphorus pentoxide, zirconium oxide and aluminum oxide.
[0061] like Figure 3 and Figure 4 As shown, the bracket prepared by the present invention includes a base 1, a groove 101 for the arch wire to pass through is provided on the top of the base 1, the bottom surface of the base 1 is a bonding surface for bonding to the teeth, and a lithium disilicate glass ceramic layer is provided on the bonding surface of the base 1.
[0062] Figure 5 The XRD pattern of 5 mol% yttria-stabilized zirconia is shown, showing that it contains 65% cubic phase (c phase). Figure 6 Shown is a SEM image of 5 mol% yttria stabilized zirconia. Figure 6 It shows that there are no voids in the 5 mol % yttria-stabilized zirconia, so the product prepared by the present invention has better light transmittance.
Claims
1. A method for photocuring additive manufacturing of a transparent zirconia ceramic bracket, comprising the following steps: The first step: prepare a light-curing additive manufacturing paste with a solid content G ≥ 58 vol%, and place the light-curing additive manufacturing paste in a vacuum machine for vacuum degassing. The steps of preparing the light-curing additive manufacturing paste are as follows: mix the photosensitive resin premix with the photoinitiator, and then add the graded zirconium oxide particles and the surfactant in three times in sequence, and put them into a homogenizer after adding the graded zirconium oxide particles and the surfactant each time, and put them into a roller press to obtain a roller-pressed mixture after all the graded zirconium oxide particles and the surfactant are added. a material, adding a rheological additive to the rolled mixture to adjust its rheological properties, thereby obtaining a light-cured additive manufacturing paste, wherein the graded zirconium oxide particles are a mixture of zirconium oxide particles with a particle size of 200 nanometers and zirconium oxide particles with a particle size of 5 to 25 micrometers, the mass ratio of the zirconium oxide particles with a particle size of 200 nanometers to the zirconium oxide particles with a particle size of 5 to 25 micrometers is 3:1 to 2:1, and the zirconium oxide particles with a particle size of 5 to 25 micrometers are obtained by spray granulation of zirconium oxide powder with an original particle size of 20 nanometers to 50 nanometers; Step 2: Place the light-curing additive manufacturing paste after vacuum degassing in the first step into an additive manufacturing device for light-curing forming to obtain a green body. The parameters of the additive manufacturing device are: light intensity of 130-150 mW, laser printing speed of 1000-7000 mm / s, printing spacing of 0.01 mm-0.03 mm, and printing layer thickness of 25-50 μm; Step 3: putting the green body obtained after the second step into an ultrasonic cleaning device for cleaning, and drying it under room temperature wind after cleaning to obtain a dried green body; Step 4: placing the dried green body obtained after the third step into a first heating device for thermal degreasing, wherein the air pressure in the first heating device is normal pressure, the temperature in the first heating device is increased from room temperature to 200°C, and the heating rate is 1.7-2.3°C / min; the temperature is increased from 200°C to 350°C, and the heating rate is 0.8-1.2°C / min; the temperature is kept at 350°C for 1 hour; the temperature is increased from 350°C to 400°C, and the heating rate is 0.8-1.2°C / min; the temperature is kept at 400°C for 1 hour; the temperature is increased from 400°C to 600°C, and the heating rate is 1.8-2.3°C / min; Step 5: Pre-sintering: pure oxygen is introduced into the first heating device at 600°C, and the temperature in the first heating device is increased from 600°C to 1350°C at a heating rate of 2-4°C / min; the temperature is kept at 1350°C for 1 hour; then the temperature in the first heating device is reduced from 1350°C to 1000°C at a cooling rate of 1.9-2.4°C / min, and then cooled with the furnace to obtain a pre-sintered bracket matrix; Step 6: Sintering, placing the pre-sintered bracket substrate obtained after the fifth step into a hot isostatic pressing furnace, wherein the atmosphere in the hot isostatic pressing furnace is pure argon, the gas pressure in the hot isostatic pressing furnace is 190 MPa to 220 MPa, the temperature in the hot isostatic pressing furnace is increased from room temperature to 1250° C., the heating rate is 1.5 to 3° C. / min, and the temperature is kept at 1250° C. for 4 hours to obtain a sintered bracket substrate; Step 7: annealing, placing the sintered bracket substrate obtained after the sixth step into a second heating device, wherein the atmosphere in the second heating device is air at normal pressure, the temperature in the second heating device is 1200° C., the annealing time is 2 hours, and then the bracket is cooled with the furnace to obtain a cooled bracket; Step 8: A lithium disilicate glass ceramic layer is attached to the bonding surface of the bracket base obtained after step 7, and the steps are as follows: A: Spraying a lithium disilicate glass ceramic solution onto the bonding surface of the bracket base obtained after the eighth step, the pressure of spraying the lithium disilicate glass ceramic solution being 0.1 MPa to 0.8 MPa; B: Place the bracket sprayed with lithium disilicate glass ceramic solution into the third heating device, raise the temperature of the third heating device from room temperature to 1500°C at a heating rate of 1.8-2.3°C / min, keep the temperature for 0.5-2 hours, then take it out and cool it at room temperature.
2. The method for photocuring additive manufacturing of transparent zirconia ceramic brackets according to claim 1, characterized in that: The amount of the graded zirconium oxide particles added for the third time is 10% of the total mass of the graded zirconium oxide particles.
3. The method for photocuring additive manufacturing of transparent zirconia ceramic brackets according to claim 1, characterized in that: The rheological additive is any one of polyvinyl alcohol, polyacrylic acid, modified urea solution, and hydroxypropyl methylcellulose, and the mass of the rheological additive is 0.1% to 0.5% of the total mass of the photocurable additive manufacturing paste.
4. The method for photocuring additive manufacturing of transparent zirconia ceramic brackets according to claim 1, characterized in that: The zirconia particles with a particle size of 200 nanometers are 5 mol % yttria-stabilized zirconia particles, and the zirconia powders with an original particle size of 20 nanometers to 50 nanometers are 5 mol % yttria-stabilized zirconia powders.
5. The method for photo-curing additive manufacturing of transparent zirconia ceramic brackets according to claim 1, characterized in that: In the third step, the ultrasonic cleaning device is internally provided with pure resin monomer to perform ultrasonic cleaning on the green body.
Citation Information
Patent Citations
Formula of high-transmittance zirconia ceramic, preparation method of paste and manufacturing method of dental crown
CN113336542A
Graded zirconia paste for 3D printing as well as preparation method and application thereof
CN113754430A
Ceramic material and repair material for improving surface adhesion of dental zirconia, and preparation method and bonding method of ceramic material and repair material