A high-nitrogen manganese nitride and its continuous production method and application

Through the combination of the multi-tube furnace continuous production process and water vapor reactant, the problems of low nitrogen content and high oxygen content in manganese nitride production are solved, and manganese nitride products with high nitrogen content and low oxygen content are achieved, reducing the Production costs and energy consumption improve product uniformity and environmental friendliness.

CN118387843BActive Publication Date: 2024-11-15HUNAN ZHONGXINDA NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410510503.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-26
Publication Date
2024-11-15
Estimated Expiration
2044-04-26

AI Technical Summary

Technical Problem

In the existing manganese nitride production methods, the nitrogen content is low and the oxygen content is high, resulting in uneven product quality. The traditional method requires vacuum equipment, which is poor in environmental friendliness, high production cost and high energy consumption.

Method used

The continuous production process of multi-tube furnace is adopted to reduce the negative impact of oxygen by using water vapor reactants. Through the dual guarantee of nitrogen pressurization and water vapor reactants, the temperature gradient and pressure are controlled to achieve continuous production of high nitrogen manganese nitride .

Benefits of technology

Significantly reduce the oxygen content of manganese nitride, ensure product uniformity, reduce production costs and energy consumption, and achieve continuous production with high nitrogen content, which is environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118387843B_ABST
    Figure CN118387843B_ABST
Patent Text Reader

Abstract

The invention provides a high-nitrogen manganese nitride and a continuous production method and application thereof, belonging to the technical field of chemistry and chemical engineering. The method for realizing continuous production is as follows: nitrogen is introduced into each tube of a multi-tube furnace, a water vapor reactant is installed and filled above the inner wall of each tube furnace body, furnace doors at both ends are closed, and the furnace body of the multi-tube furnace is divided into six areas, which are heated to different temperatures respectively; metal manganese raw materials are loaded into a boat, a furnace door at a furnace head is opened, a first batch of boats are pushed into each furnace tube of the multi-tube furnace, the furnace door at the furnace head is closed, nitrogen is continuously introduced for reaction, the pressure of the furnace tube is controlled, and after the reaction is completed, the furnace door at the furnace tail is opened to push out the first batch of boats; the product in the boat is high-nitrogen manganese nitride; the above steps are repeated to continuously push in the next batch of boats to realize continuous production; the water vapor reactant can greatly reduce the negative impact of oxygen, no vacuum equipment is required, and nitrogen is pressurized in multiple furnace tubes, which is environmentally friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of chemistry and chemical engineering, and in particular to a manganese nitride with a high nitrogen content and a continuous production method and application thereof. Background Art

[0002] In the traditional steel smelting process, manganese nitride is often added to alloy steel in the form of an intermediate alloy to adjust the composition of the alloy steel to improve its performance. Among them, manganese mainly plays the role of deoxidation, desulfurization and alloying, and nitrogen can improve the strength, toughness, creep resistance and corrosion resistance of steel. Therefore, it is an economical and reasonable process to select manganese as a carrier of nitrogen and add manganese nitride in the process of smelting high nitrogen steel. Secondly, manganese nitride is increasingly used in the field of new energy. In the field of solar cells, the application of manganese nitride nanomaterials to photosensitive materials can improve the photoelectric conversion efficiency of solar cells; in the field of ion batteries, manganese nitride has high specific capacity and long cycle life, which provides new possibilities for the development of energy storage technology; in the field of photocatalytic water decomposition, manganese nitride has also been widely studied and applied.

[0003] At present, there are many methods for producing manganese nitride. According to the nitriding reaction pressure, it can be divided into normal pressure method and pressurized method, etc.; according to the equipment used, it can be divided into pit furnace method, rotary furnace method, push plate kiln method, tunnel kiln method, vacuum furnace method, fluidized bed reactor method, etc. These preparation methods have their own advantages and disadvantages. The normal pressure method (push plate kiln method, tunnel kiln method, pit furnace method, rotary kiln method and fluidized bed reactor method usually use normal pressure) has low production cost, but the nitrogen content of the prepared manganese nitride is also low, which does not meet the requirements of industrial application; the pressurized method (vacuum furnace method usually uses pressurization) prepares manganese nitride with high nitrogen content, but the equipment structure is complex and the production cost is high. The pit furnace method, vacuum furnace method, etc. are intermittent production, with long production cycle, low production capacity, high energy consumption, and uneven temperature in various parts of the furnace body, resulting in inconsistent nitrogen content of products produced at different positions of the furnace, some of which are higher than 8%, and some are even lower than 3%, and the uniformity of product quality cannot be guaranteed. Although patents CN202210328863.6 and CN201510170143.1 use push-plate kilns and tunnel kilns for continuous production, toxic and harmful ammonia is used, and the nitrogen content of the product is less than 8%. From the disclosed text, it can be seen that continuous production in the true sense has not been achieved. In addition, the manganese nitride prepared by the existing process methods has a common disadvantage, that is, the manganese nitride produced has a high oxygen content. The reason is that the moisture in the raw material reacts with the surface of metallic manganese during the nitriding process to form a dense manganese oxide layer. The presence of a dense manganese oxide layer not only increases the oxygen content in the product, but also hinders the increase of the nitrogen content in the product, thereby affecting the product quality, which is not conducive to subsequent steel smelting and new energy batteries. Summary of the invention

[0004] In order to solve the above technical problems, this scheme uses water vapor reactant in the continuous production process to achieve continuous production of high-nitrogen manganese nitride. The water vapor reactant can greatly reduce the negative impact of the presence of oxygen. The continuous production process does not require vacuum equipment and multiple furnace tubes are nitrogen pressurized, which is environmentally friendly.

[0005] To achieve the above object, the present invention provides a continuous production method of high-nitrogen manganese nitride, comprising the following steps:

[0006] S1. Nitrogen is introduced into each tube of the multi-tube furnace. A water vapor reactant is installed on the inner wall of each tube. The furnace doors at both ends are closed. The multi-tube furnace body is divided into six areas, and the temperatures are raised to different temperatures respectively.

[0007] S2, loading the metallic manganese raw material into a boat, opening the furnace door, pushing the first batch of boats into each furnace tube of the multi-tube furnace, closing the furnace door, continuing to feed nitrogen to react, and controlling the pressure of each furnace tube;

[0008] S3, after the reaction in step S2 is completed, the furnace door at the tail of the furnace is opened and the first batch of boats are pushed out; the product in the boats is high-nitrogen manganese nitride;

[0009] S4. Repeat steps S2-S3 to continuously push in the next batch of boats to achieve continuous production.

[0010] Preferably, the number of tube furnaces in the multi-tube furnace in step S1 is 2-100.

[0011] Preferably, the source of nitrogen in step S1 is liquid nitrogen, compressed nitrogen or a nitrogen generator.

[0012] Preferably, in step S1, the water vapor reactant is selected from one or more of elemental iron, elemental aluminum, elemental magnesium, elemental zinc, iron alloy, aluminum alloy, magnesium alloy, and zinc alloy, and the shape of the water vapor reactant is one or more of powder, flake or block.

[0013] Preferably, the temperatures of the six zones in step S1 are 100-400°C, 400-700°C, 700-1000°C, 700-1000°C, 400-700°C, and 100-400°C, respectively.

[0014] Preferably, in step S2, the metallic manganese raw material is selected from one or more of manganese powder, manganese flakes, manganese blocks, manganese peaches and manganese pillows.

[0015] Preferably, the reaction time in step S2 is 3 to 600 min, and the pressure is 102 to 500 KPa.

[0016] Preferably, in step S2, the lengths of the furnace head, furnace body and furnace tail of the furnace tube are 1 to 50 meters respectively.

[0017] Based on a general inventive concept, the present invention also provides a high-nitrogen manganese nitride prepared by a continuous production method.

[0018] Based on a general inventive concept, the present invention also provides an application of a continuous production method in the preparation of high-nitrogen manganese nitride.

[0019] The preparation mechanism of high nitrogen manganese nitride in this scheme:

[0020] The present invention provides a process for continuously producing high-nitrogen manganese nitride. The baked metal manganese material is used as a raw material, put into a boat, and pushed into a multi-tube furnace into which nitrogen is introduced. The multi-tube furnace body is divided into six zones, which are heated to different temperatures respectively. The temperature of the heating zone 1 is 100-400°C, the temperature of the heating zone 2 is 400-700°C, the temperature of the constant temperature zone 1 and the constant temperature zone 2 are both 700-1000°C, the temperature of the cooling zone 1 is 400-700°C, and the temperature of the cooling zone 2 is 100-400°C. The multi-tube furnace is in a closed state after the door is closed. The filling of nitrogen enables the nitriding process of manganese to maintain a relatively high pressure. The boat moves slowly from the heating zone to the constant temperature zone driven by an electric cylinder. As the temperature gradient increases, the rate of manganese nitriding changes from slow to fast. The constant temperature zone is relatively long, which is conducive to the nitriding reaction. The outlet temperature is set relatively low, which can shorten the cooling time of the manganese nitriding product and increase the output of the manganese nitriding product. During the continuous production process, nitrogen has been maintaining the pressure in the furnace, but the raw materials contain water and trace oxidized surfaces. After the water evaporates at high temperature, it quickly undergoes a redox reaction with the water vapor reactant. The oxygen atoms in it are combined with the water vapor reactant and consumed, avoiding the oxidation of the metal manganese raw materials; the generated hydrogen atoms penetrate into the metal manganese raw materials together with the nitrogen molecules, which, on the one hand, loosens the raw materials and facilitates the nitriding reaction, and on the other hand, can reduce the trace oxidized surfaces in the raw materials.

[0021] The double insurance of nitrogen pressure and water vapor reactant ensures that the product will hardly be oxidized, and the nitrogen can maintain a high pressure in the tube while serving as a reaction raw material.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] (1) The manganese metal raw material contains water and trace amounts of surface oxidation. After the water evaporates at high temperature, it can quickly undergo a redox reaction with the water vapor reactant. The oxygen atoms in the water vapor reactant are combined with the water vapor reactant and consumed, thereby avoiding the oxidation of the manganese metal raw material. The generated hydrogen atoms penetrate into the manganese metal raw material together with the nitrogen molecules. On the one hand, they play a role in loosening the raw material and facilitating the nitriding reaction. On the other hand, they can reduce the trace amounts of surface oxidation in the raw material, thereby significantly reducing the oxygen content of the manganese nitride product.

[0024] (2) Both the water vapor reactant and nitrogen can remove the interference of oxygen elements, which can provide double protection and minimize the oxygen content of the final product manganese nitride to less than 0.12%.

[0025] (3) This method loads the water vapor reactant into the components on the walls of the reactor, which will not contaminate the product, and the reactant can be disassembled and regenerated after deactivation.

[0026] (4) The manganese nitride production method provided by the present invention is a continuous production method with high production capacity, which can be adjusted by the number of furnace tubes, has low energy consumption and low production cost. The nitrogen source used is only nitrogen gas, which not only serves as a raw material for nitridation, but also can maintain the pressure of the reaction system. The quality of the products produced by the present invention is uniform and stable. Through the action of the water vapor reactant, the adjustment of temperature and the change of pressure, the nitrogen content in the manganese nitride produced by this scheme can be adjusted between 10 and 20%. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0028] Figure 1 These are pictures of the manganese raw material and manganese nitride product in Experimental Example 1, where (a) is a metallic manganese peach, (b) is the manganese nitride product of Example 1, and (c) is the manganese nitride product of Comparative Example 1. DETAILED DESCRIPTION

[0029] In order to make the technical problems, technical solutions and advantages to be solved by the present invention more clear, a detailed description will be given below with reference to the accompanying drawings and specific embodiments.

[0030] The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention. Without departing from the spirit and substance of the present invention, modifications or substitutions made to the methods, steps or conditions of the present invention are within the scope of the present invention.

[0031] Example 1

[0032] Continuous production of high-nitrogen manganese nitride

[0033] S1. A wire groove is cut on the inner wall of each tube of the multi-tube furnace, and the parts for placing elemental iron are embedded in the groove. Nitrogen is introduced into each tube of the multi-tube furnace, and the furnace doors at both ends are closed. The multi-tube furnace body is divided into six areas, and the temperatures are raised to different temperatures, namely 400°C, 700°C, 1000°C, 1000°C, 700°C, and 400°C;

[0034] S2, put the manganese peach into the boat, open the furnace door, push the first batch of boats into each furnace tube of the multi-tube furnace, close the furnace door, continue to introduce nitrogen to react for 0.5h, and control the pressure of the furnace tube to 500KPa;

[0035] S3, after the reaction in step S2 is completed, the furnace door at the tail of the furnace is opened and the first batch of boats are pushed out; the product in the boats is high-nitrogen manganese nitride;

[0036] S4. Repeat steps S2-S3 to continuously push in the next batch of boats to achieve continuous production.

[0037] Example 2

[0038] Continuous production of high-nitrogen manganese nitride

[0039] S1. A wire groove is dug on the inner wall of each furnace tube of the multi-tube furnace, and the parts containing the single aluminum are embedded in the groove. Nitrogen is introduced into each tube of the multi-tube furnace, and the furnace doors at both ends are closed. The multi-tube furnace body is divided into six areas, and the temperatures are raised to different temperatures, namely 100°C, 400°C, 700°C, 700°C, 400°C, and 100°C;

[0040] S2. Load the manganese flakes into the boat, open the furnace door, push the first batch of boats into each furnace tube of the multi-tube furnace, close the furnace door, continue to introduce nitrogen to react for 2h, and control the pressure of the furnace tube to 200KPa;

[0041] S3, after the reaction in step S2 is completed, the furnace door at the tail of the furnace is opened and the first batch of boats are pushed out; the product in the boats is high-nitrogen manganese nitride;

[0042] S4. Repeat steps S2-S3 to continuously push in the next batch of boats to achieve continuous production.

[0043] Example 3

[0044] Continuous production of high-nitrogen manganese nitride

[0045] S1. A wire groove is dug on the inner wall of each furnace tube of the multi-tube furnace, and the parts containing the single aluminum are embedded in the groove. Nitrogen is introduced into each tube of the multi-tube furnace, and the furnace doors at both ends are closed. The multi-tube furnace body is divided into six areas, and the temperatures are raised to different temperatures, namely 200°C, 500°C, 900°C, 900°C, 400°C, and 200°C;

[0046] S2, put manganese powder into the boat, open the furnace door, push the first batch of boats into each furnace tube of the multi-tube furnace, close the furnace door, continue to introduce nitrogen to react for 3h, and control the pressure of the furnace tube to 300KPa;

[0047] S3, after the reaction in step S2 is completed, the furnace door at the tail of the furnace is opened and the first batch of boats are pushed out; the product in the boats is high-nitrogen manganese nitride;

[0048] S4. Repeat steps S2-S3 to continuously push in the next batch of boats to achieve continuous production.

[0049] Comparative Example 1

[0050] Continuous production of high nitrogen manganese nitride by removing water vapor reactant

[0051] S1. Introduce nitrogen into each tube of the multi-tube furnace, close the furnace doors at both ends, divide the multi-tube furnace into six areas, and heat them to different temperatures, namely 400°C, 700°C, 1000°C, 1000°C, 700°C, and 400°C;

[0052] S2, put the manganese peach into the boat, open the furnace door, push the first batch of boats into each furnace tube of the multi-tube furnace, close the furnace door, continue to introduce nitrogen to react for 0.5h, and control the pressure of the furnace tube to 500KPa;

[0053] S3, after the reaction in step S2 is completed, the furnace door at the tail of the furnace is opened and the first batch of boats are pushed out; the product in the boats is high-nitrogen manganese nitride;

[0054] S4. Repeat steps S2-S3 to continuously push in the next batch of boats to achieve continuous production.

[0055] Comparative Example 2

[0056] Continuous production of high-nitrogen manganese nitride without temperature gradient

[0057] S1. A wire groove is drilled on the inner wall of each tube of the multi-tube furnace, and the parts containing the single aluminum are embedded in the groove. Nitrogen is introduced into each tube of the multi-tube furnace, and the furnace doors at both ends are closed. The temperature of the multi-tube furnace is raised to 1000°C.

[0058] S2. Load the manganese flakes into the boat, open the furnace door, push the first batch of boats into each furnace tube of the multi-tube furnace, close the furnace door, continue to introduce nitrogen to react for 2h, and control the pressure of the furnace tube to 200KPa;

[0059] S3, after the reaction in step S2 is completed, the furnace door at the tail of the furnace is opened and the first batch of boats are pushed out; the product in the boats is high-nitrogen manganese nitride;

[0060] S4. Repeat steps S2-S3 to continuously push in the next batch of boats to achieve continuous production.

[0061] Comparative Example 3

[0062] Removal of water vapor reactant for continuous production of high nitrogen manganese nitride without temperature gradient

[0063] S1. Introduce nitrogen into each tube of the multi-tube furnace, close the furnace doors at both ends, and heat the multi-tube furnace to 1000°C.

[0064] S2, put manganese powder into the boat, open the furnace door, push the first batch of boats into each furnace tube of the multi-tube furnace, close the furnace door, continue to introduce nitrogen to react for 3h, and control the pressure of the furnace tube to 300KPa;

[0065] S3, after the reaction in step S2 is completed, the furnace door at the tail of the furnace is opened and the first batch of boats are pushed out; the product in the boats is high-nitrogen manganese nitride;

[0066] S4. Repeat steps S2-S3 to continuously push in the next batch of boats to achieve continuous production.

[0067] Experimental Example 1

[0068] Study on the oxygen content of the metallic manganese raw material and the product manganese nitride in Example 1 and Comparative Example 1

[0069] The oxygen content and surface microscopic differences in the manganese metal raw material and the product manganese nitride in Example 1 and Comparative Example 1 are investigated. The results are shown in Table 1. Figure 1 As shown:

[0070] Table 1 Example 1 Comparative Example 1 Oxygen content of metallic manganese raw material and product manganese nitride

[0071] Material Oxygen content of raw materials (%) Oxygen content of manganese nitride (%) Example 1 2.32 0.12 Comparative Example 1 2.32 1.72

[0072] The results show that the oxygen content of the manganese nitride prepared in Example 1 is much lower than that of the manganese nitride prepared in Comparative Example 1, and the oxidized surface is improved. This is because the baked metal manganese raw material contains moisture and a trace amount of oxidized surface. After entering the furnace, the moisture evaporates at high temperature and quickly undergoes a redox reaction with the water vapor reactant. The oxygen atoms therein are combined with the water vapor reactant and consumed, thereby avoiding the oxidation of the metal manganese raw material. The generated hydrogen atoms penetrate into the metal manganese raw material together with the nitrogen molecules, which, on the one hand, loosens the raw material and facilitates the nitridation reaction, and on the other hand, can reduce the trace amount of oxidized surface in the raw material. The water vapor reactant provided in this scheme can effectively reduce the oxygen content in the product manganese nitride. If the water vapor reactant is not used, the oxygen content of the product manganese nitride is significantly increased. Figure 1 As shown in (c), the oxidized surface is not improved.

[0073] Experimental Example 2

[0074] The nitrogen content and oxygen content of the manganese nitride prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were investigated.

[0075] The nitrogen content and oxygen content of the manganese nitride prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were tested, and the results are shown in Table 2 below:

[0076] Table 2 Oxygen content and nitrogen content of manganese nitride prepared in Examples 1-3 and Comparative Examples 1-3

[0077]

[0078]

[0079] The results are shown in Table 1. The nitrogen content of manganese nitride prepared by continuous production of Examples 1-3 using this scheme can reach 10-20%. The oxygen content is lower than 0.12%. Compared with Comparative Example 1, the removal of the water vapor reactant significantly affects the nitrogen content and oxygen content of the product. Compared with Comparative Example 2, setting a constant temperature without a temperature gradient has a significant effect on the nitrogen content of the manganese nitride product, and the setting of the temperature gradient improves the quality of manganese nitride. Compared with Comparative Example 3, the synergistic effect of the water vapor reactant and the temperature gradient significantly affects the quality of manganese nitride.

[0080] The above is only a preferred embodiment of the present invention, and the protection scope of the present invention is not limited to the above embodiments. For those skilled in the art, improvements and changes obtained without departing from the technical concept of the present invention should also be regarded as the protection scope of the present invention.

Claims

1. A continuous production method of high-nitrogen manganese nitride, characterized in that: The following steps are involved: S1. Nitrogen is introduced into each tube of the multi-tube furnace. A water vapor reactant is installed on the inner wall of each tube. The furnace doors at both ends are closed. The multi-tube furnace body is divided into six areas, and the temperatures are raised to different temperatures respectively. S2, loading the metallic manganese raw material into a boat, opening the furnace door, pushing the first batch of boats into each furnace tube of the multi-tube furnace, closing the furnace door, continuing to introduce nitrogen to react, and controlling the pressure of the furnace tube; S3, after the reaction in step S2 is completed, the furnace door at the tail of the furnace is opened, and the first batch of boats are pushed out, and the product in the boats is high-nitrogen manganese nitride; S4, repeating steps S2-S3 to continuously push in the next batch of boats to achieve continuous production; In step S1, the water vapor reactant is selected from one or more of elemental iron, elemental aluminum, elemental magnesium, elemental zinc, iron alloy, aluminum alloy, magnesium alloy, and zinc alloy, and the shape of the water vapor reactant is one or more of powder, flake, or block; The temperatures of the six regions in step S1 are 100-400°C, 400-700°C, 700-1000°C, 700-1000°C, 400-700°C, and 100-400°C, respectively; The reaction time in the step S2 is 3-600 min, and the pressure is 102-500 KPa.

2. The continuous production method according to claim 1, characterized in that: In the step S2, the metallic manganese raw material is selected from one or more of manganese powder, manganese flakes, manganese blocks, manganese peaches, and manganese pillows.

3. The continuous production method according to claim 1, characterized in that: In step S2, the lengths of the furnace head, furnace body and furnace tail of the furnace tube are 1 to 50 meters respectively.

4. The continuous production method according to claim 1, characterized in that: The number of tube furnaces in the multi-tube furnace in step S1 is 2-100.

5. The continuous production method according to claim 1, characterized in that: The source of nitrogen in step S1 is liquid nitrogen, compressed nitrogen or a nitrogen generator.

6. Use of the continuous production method according to any one of claims 1 to 5 in the preparation of high-nitrogen manganese nitride.