A 14.9 grade non-quenched and tempered cold heading steel wire rod for bolts and a manufacturing method thereof
By using microalloying, high-carbon chemical composition design, and online molten salt isothermal and precipitation control technology, a high proportion of tempered sorbite and tempered pearlite microstructures are formed, solving the problem of insufficient strength and plasticity of cold heading steel wire rod for grade 14.9 non-quenched and tempered bolts, and achieving efficient and green production and improved yield.
Patent Information
- Application Number
- CN202411133215.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-19
AI Technical Summary
The existing 14.9 grade non-quenched and tempered cold heading steel wire rods for bolts have deficiencies in strength and plasticity, resulting in low manufacturing efficiency, high energy consumption, and insufficient utilization of microalloying components, which poses risks of wire breakage during drawing and cold heading cracking.
By employing microalloying and high-carbon chemical composition design, combined with online molten salt isothermal precipitation control and roller conveyor strong slow cooling technology, a high proportion of tempered sorbite and tempered pearlite structures are formed through microstructure regulation. Combined with high-carbon solid solution strengthening and microalloyed dispersion precipitation strengthening, the matrix strength and resistance to delayed fracture are improved.
It has enabled efficient and green production of grade 14.9 non-heat-treated bolts, improved yield, reduced the risk of wire breakage during pull-out and cold heading cracking, and enhanced the strength and plasticity of the material, making it suitable for industrial machinery and equipment.
Smart Images

Figure CN118653095B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of hot-rolled cold-heading steel wire rods, and in particular relates to a cold-heading steel wire rod for 14.9-grade non-quenched and tempered bolts and a manufacturing method thereof. Background Art
[0002] Bolt connections are important connecting components of industrial machinery and equipment and are widely used. Improving the strength grade of bolts can not only achieve the goal of lightweighting industrial machinery and equipment, but also improve the performance and service life of the equipment in complex service environments such as high-frequency stress loading. Cold heading steel wire rod for bolts is used as the base material for bolt manufacturing. Its insufficient performance will lead to low efficiency, increased energy consumption and cost of bolt manufacturing, and even seriously restrict the further development of bolts. With the increase of strength grade, the delayed fracture performance of the material is outstanding. At present, domestic cold heading steel wire rod for 14.9 grade bolts is mainly concentrated in the modulation type, and non-quenched and tempered cold heading steel wire rod for bolts is rarely developed. For example: Patent CN116083806A discloses a delayed fracture resistant 14.9 grade quenched and tempered cold heading steel hot rolled wire rod for bolts and its preparation method, which adopts C-Si-Mn-Al-B component design, obtains wire rod by low temperature controlled rolling, water-cooled hot curling after rolling, and then heat-insulated cooling, and then produces bolts by drawing, cold heading, quenching and tempering heat treatment. However, on the one hand, the strength and plasticity of the obtained wire rod are insufficient, and it is also necessary to use modulation heat treatment. The processing improves the comprehensive mechanical properties of the material, but it also brings about problems such as many processes, high energy consumption and low efficiency. On the other hand, the composition system contains a high Mn content, which results in high material cost and hardenability, and also increases the risk of coarse grains, cold work hardening sensitivity and temper brittleness of the steel. When the cooling rate is insufficient, blocky carbides are easily produced and precipitated along the grain boundaries to make the steel brittle, and the billet opening after rolling takes a long time. Although water cooling and hot curling are adopted after low-temperature sizing, a large number of bubbles will be generated during the water cooling process and adhere to the surface of the wire rod, affecting heat transfer, resulting in a large difference in the cooling rate of the wire rod, further increasing the risk of precipitation of abnormal tissues, resulting in increased fluctuations in mechanical properties and affecting the yield rate. The hot curling temperature of the wire rod is high and the wire rod is soft, and there is also a risk of easy scratches on the surface of the wire rod and reduced surface quality, which limits the production and application of cold heading steel wire rod.
[0003] The existing non-quenched and tempered cold heading steel wire rods need to omit the spheroidizing annealing and quenching and tempering processes, and reach the final performance level through drawing and cold heading, so the requirements for strength and plasticity are relatively high. At present, the research and development of wire rods for non-adjustable bolts of grade 8.8~10.9 is mainly focused on. Under the limitation of the cooling control capacity of the Stelmor air cooling line after spinning, medium and low carbon steels are generally used to reduce the difficulty of improving plasticity, increase the alloy content to improve the hardenability of the material, and add microalloy components to strengthen the matrix. Combined with rapid cooling on the Stelmor line after spinning, the microstructure of all or doped bainite or martensite is obtained to improve the matrix strength. However, on the one hand, too high hardenability The content of brittle alloy or micro-alloy brings material cost pressure. In order to obtain a certain proportion of hard and brittle phase structure, the micro-alloy components and precipitate phases are coarsened or cannot be precipitated in large quantities under high cooling rate, so that the micro-alloy cannot be effectively utilized, and the improvement of strength and delayed fracture resistance is limited. On the other hand, the bainite or martensite structure produced is highly distorted, which greatly deteriorates the plasticity of the wire rod. The wire rod is too brittle, which makes the wire rod break during downstream unwinding, transportation to downstream by steel mills, and even during the coiling process of steel mills, resulting in waste of raw materials and low yield rate. It also greatly increases the risk of drawing fracture and cold heading cracking under the non-quenching and tempering process.
[0004] Carbon is a relatively cheap element in steel that can improve the strength of steel. Replacing alloy components is beneficial to reducing material costs. However, the existing high-carbon steel wire rods are mainly used to increase the content of troostite in the organization to improve the strength and drawing performance. They are used in applications such as cords and bridge cables. On the one hand, the Stelmor air-cooled wire adopts insulation or delayed cooling to promote the incubation of troostite, but the precipitation temperature range of secondary cementite is long, and the level of network carbides is high, which destroys the continuity of the matrix and increases the brittleness of the material, making the drawing and cold heading process It is easy to crack. On the other hand, due to the small degree of supercooling and the short time the wire rod passes through the troostite phase region, the wire rod is already in a low temperature state after being inoculated with troostite under continuous cooling and insulation. Therefore, the interlamellar spacing of the obtained troostite structure is large, and the tissue stress and dislocation density are high, which makes the wire rod ultimately have insufficient plasticity, poor cold deformation ability, easy drawing hardening, and unable to meet the requirements of drawing and cold heading. Increasing the ferrite content in the structure will cause a significant loss of wire rod strength, which is not conducive to the performance level of fasteners reaching grade 14.9 without quenching and tempering. Summary of the invention
[0005] The present invention aims to solve at least one of the above-mentioned technical problems to a certain extent. The present invention provides a cold heading steel wire rod for 14.9-grade non-quenched and tempered bolts and a manufacturing method thereof, which can improve the use value of carbon elements and micro-alloy components, take into account the strength, plasticity and delayed fracture resistance of the wire rod, and is suitable for the efficient and green production of 14.9-grade non-quenched and tempered bolts, which is beneficial to improving the yield rate and reducing the risk of wire breakage during drawing and cracking during cold heading.
[0006] The technical solution adopted by the present invention to solve its technical problem is:
[0007] A 14.9-grade cold heading steel wire rod for non-quenched and tempered bolts, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.80%-0.84%, Si: 0.20%-0.40%, Mn: 0.45%-0.55%, Cr: 0.10%-0.30%, Nb: 0.030%-0.050%, V: 0.040%-0.050%, Mo: 0.37%-0.50%, P≤0.015%, S≤0.015%, and the rest is Fe and unavoidable impurities; the microstructure thereof includes a mixed structure consisting of tempered troostite with a volume percentage of ≥88%, tempered pearlite with a volume percentage of ≥5%, and the rest is fused pearlite.
[0008] The design basis of the chemical composition and mass percentage of the above-mentioned cold heading steel wire rod includes:
[0009] (1) Carbon: As the main added element, the addition of C to replace alloy components is beneficial to reducing material costs. Through solid solution strengthening and precipitation strengthening, the matrix strength and high hardenability of steel can be ensured, so that the performance level of 14.9 bolts can be achieved through drawing and cold heading after omitting annealing and tempering processes. However, it also increases the risk of decarburization and the risk of cementite being distributed in a network along the grain boundary. In addition, if the C content is too high, the bainite phase transformation temperature range will increase, which is not conducive to microstructure control. Therefore, in order to facilitate microstructure control and take into account the cold deformation performance and strength characteristics of cold heading steel wire rod, the mass percentage of C is controlled to be 0.80%~0.84%.
[0010] (2) Silicon: The Si element is a deoxidizer in the steelmaking process. It can dissolve in austenite to increase the hardness and strength of steel and inhibit grain coarsening in the online molten salt isothermal process. However, excessive silicon will increase the risk of non-metallic inclusions and decarburization and reduce the plasticity and toughness of steel. Therefore, the mass percentage of Si is controlled to be 0.20%~0.40%.
[0011] (3) Manganese: Mn is often added to steel as a deoxidizer during the smelting process. It can improve the strength and hardenability of steel by dissolving in austenite. However, too high Mn content will aggravate the segregation during the solidification of the steel billet, resulting in poor uniformity of the steel and increasing the tendency of grain coarsening during the heating process of the material. Too high Mn content will also increase material costs. Therefore, the mass percentage of Mn is controlled to be 0.45%~0.55%.
[0012] (4) Chromium: As a ferrite-forming element, Cr can greatly improve the hardenability of the material. Through the online molten salt precipitation control, fine dispersed carbide particles can be precipitated, which can improve the strength of the material and is beneficial to the refinement of the pearlite lamellar spacing and the melting of the pearlite lamellar. However, if the Cr content is too high, quenching structure is likely to appear, which is not conducive to structure control and will increase the temper brittleness tendency of the steel. In addition, the precipitation and coarsening of Cr is not conducive to the strength and plasticity of the wire rod. Therefore, the mass percentage of Cr is controlled to be 0.10%~0.30%.
[0013] (5) Niobium: As a microalloying element, Nb can precipitate during high-temperature rolling to pin grain boundaries and refine grains, while reducing the overheating sensitivity of steel. It can disperse and precipitate in the high-temperature isothermal range, thereby improving the strength and delayed fracture resistance of the material. However, its cost is relatively high. Based on the role of Nb and cost considerations, the mass percentage of Nb is controlled to be 0.030%~0.050%.
[0014] (6) Vanadium: As a microalloying element, V can be dispersed and precipitated in large quantities in the high-temperature isothermal range, greatly improving the strength, toughness and delayed fracture resistance of the material. However, its cost is relatively high. Based on the role of V and cost considerations, the mass percentage of V is controlled to be 0.040%~0.050%.
[0015] (7) Molybdenum: The Mo element can increase the tempering temperature of the material and inhibit the coarsening of the precipitated phase in the isothermal range, thereby improving the strength and delayed fracture resistance of the material. However, the cost of Mo is relatively high and it will promote decarburization. Based on the role of the Mo element and cost considerations, the mass percentage of Mo is controlled to be 0.37%~0.50%.
[0016] (8) Phosphorus and sulfur: P and S are impurity elements. The lower the better. Therefore, P is controlled to be ≤ 0.015% and S is ≤ 0.015%.
[0017] The above-mentioned cold heading steel wire rod is designed with a micro-alloy and high-carbon chemical composition of C-Si-Mn-Cr-Nb-V-Mo, and the Mn and Cr contents are relatively low. Compared with the non-quenched and tempered steel wire rod obtained after existing controlled rolling and controlled cooling, which is all or doped with bainite or martensite, the microstructure in the cold heading steel wire rod includes a higher proportion of tempered troostite structure. The troostite has finer interlamellar spacing and higher strength than the pearlite structure. The troostite has smaller distortion and dislocation density than the bainite or martensite structure, and better plasticity and toughness. After melting and initial transformation to spheroidization into tempered troostite, the dislocation density is further reduced, so that the tempered troostite retains the strength characteristics of troostite and the plasticity is further improved. Combined with the high-carbon solid solution strengthening and micro-alloy dispersion precipitation strengthening, it makes up for the strength loss caused by reducing the content of hardenability alloy and micro-alloy components, and provides higher matrix strength and material delayed fracture resistance.
[0018] The cold heading steel wire rod structure also includes a small amount of tempered pearlite and fused pearlite structure. The pearlite has a coarser interlamellar spacing and higher plasticity than the troostite structure, and has higher strength than the ferrite structure. The pearlite structure is melted and initially spheroidized to transform into fused pearlite and tempered pearlite structure, and the organizational stress and dislocation density are further reduced, so that the tempered pearlite retains the characteristics of moderate pearlite strength and higher plasticity, avoiding excessive deterioration of the wire rod strength due to the increase of ferrite. At the same time, compared with the high troostitization rate microstructure of the existing high-carbon steel wire rod, the tempered state of the troostite and pearlite structures is used to regulate the wire rod to fully soften. On the basis of avoiding excessive loss of wire rod strength, the plastic toughness and cold deformation performance of the wire rod are effectively improved, which is more convenient for drawing and cold heading, reduces the risk of wire breakage during drawing and cracking during cold heading, and obtains higher strength and plasticity.
[0019] In a preferred embodiment, the lamellar spacing of the tempered troostite is 55-95 nm, and the lamellar spacing of the tempered pearlite is 155-185 nm. The lamellar spacing of the tempered troostite and the tempered pearlite is relatively fine, which is more convenient for improving the strength of the wire rod and promoting melting tempering.
[0020] In a preferred embodiment, the network carbide level of the cold heading steel wire rod is level 0, which can effectively eliminate the adverse effects of the network carbide deterioration phase and enhance the use value of the carbon element.
[0021] In a preferred embodiment, the diameter of the cold heading steel wire rod is 10.0~26.0mm, the tensile strength is 1350~1400MPa, and the cross-sectional shrinkage rate is 42%~48%. It has a high match between tensile strength and cross-sectional shrinkage rate, so that the cold heading steel wire rod can achieve the performance level of 14.9 grade bolts by reducing the surface and strengthening without spheroidizing annealing and tempering processes, avoiding drawing hardening and excessive loss of plasticity in the process, thereby reducing the risk of wire breakage during drawing and cracking during cold heading, and simplifying the bolt manufacturing process.
[0022] A method for manufacturing a 14.9-grade non-quenched and tempered cold-heading steel wire rod for bolts, the method comprising: producing a wire rod by controlled rolling according to the chemical composition of the above-mentioned 14.9-grade non-quenched and tempered cold-heading steel wire rod for bolts, after the wire rod is spun into a wire rod at a spinning temperature of ≥900°C, the wire rod first undergoes online molten salt isothermal treatment, so that the wire rod is cooled to a pearlite phase region at a cooling rate of ≥42°C / s for isothermal phase transformation, promoting the transformation of high-temperature austenite to a troostite structure, the wire rod then undergoes online molten salt precipitation control, raising the molten salt temperature to promote the dispersion and precipitation of Nb and V, promoting the initial spheroidization transformation and melting of troostite and pearlite, and finally undergoing strong slow cooling on a hot air roller to produce a cold-heading steel wire rod having a microstructure comprising a mixed structure consisting of tempered troostite with a volume percentage of ≥88%, tempered pearlite with a volume percentage of ≥5%, and the rest being fused pearlite.
[0023] The manufacturing method adopts micro-alloy, high-carbon chemical composition design combined with online molten salt isothermal and precipitation control and roller strong slow cooling technology. On the one hand, it avoids the wire-spinning temperature being too low, which is not conducive to the induced precipitation of Nb in the controlled rolling stage. After the wire-spinning, the online salt bath isothermal isothermal is directly carried out. Compared with the Stelmor air cooling and fast cooling, the high heat exchange capacity of the molten salt can be used to make the wire rod quickly pass through the precipitation interval of the secondary cementite at a faster cooling rate, eliminate the network carbide, and suppress the influence of the network carbon deterioration phase through the online molten salt ultra-fast cooling technology, thereby improving the use value of the carbon element and obtaining a larger degree of supercooling. The online molten salt isothermal process has a lower molten salt temperature than the online molten salt precipitation control process. At a lower isothermal temperature in the pearlite phase region, it can promote the transformation of high-temperature austenite to troostite structure, increase the proportion of troostite in the structure, and reduce the spacing between troostite lamellae to ensure the strength and plasticity of the matrix, and make organizational preparations for the initial spheroidization transformation of troostite after the subsequent increase in the molten salt temperature. Compared with the air cooling and water cooling processes, the molten salt can cover the surface of the wire rod when the wire rod passes through the molten salt, without the influence of wind volume differences or bubble interference, making the heat transfer more uniform and avoiding the risk of abnormal structure transformation into bainite or martensite.
[0024] On the other hand, when the wire rod continues to pass through the molten salt with a higher temperature for online molten salt precipitation control, compared with the continuous cooling of the Stelmore line, a higher precipitation control temperature can be used to promote the large-scale dispersion precipitation of Nb and V elements in the high-temperature isothermal range, and Mo is used to inhibit the coarsening of the precipitation phase, so that the precipitation of Cr, Nb, and V is finer, so as to give full play to the micro-alloy strengthening effect, improve the matrix strength and the material's delayed fracture resistance. At the same time, compared with the Stelmore insulation cooling, the wire rod temperature can be kept consistent with the molten salt temperature instead of the continuous slow cooling of the insulation cooling, thereby keeping the wire rod in a high-temperature isothermal state for a longer time, and a small amount of residual austenite in the wire rod structure becomes pearlescent. The high molten salt temperature promotes the melting and initial spheroidization of troostite and pearlite, and transforms them into tempered troostite, tempered pearlite and fused pearlite structures, reducing the organizational stress and dislocation density. The high temperature state of the wire rod after the online molten salt precipitation control is continued by hot air roller strong slow cooling, which promotes further softening of the organization to adjust the overall strength and plasticity matching of the material. Compared with the existing high-temperature coiling before the phase transformation, the coiling temperature after the phase transformation after the hot air roller strong slow cooling is relatively lower, which can avoid the surface scratch problem caused by the wire rod being too soft, improve the surface quality, and compared with the bainite or martensite wire rod organizational plasticity is significantly improved, the wire rod coiling and uncoiling are not easy to be brittle fracture, and the wire rod yield rate is guaranteed.
[0025] In a preferred embodiment, during the controlled rolling, the soaking temperature of the heating furnace is controlled to be 1100~1150℃ before rolling, the soaking time is 2~3h, and the furnace time is ≥4h. A higher soaking temperature and time of the heating furnace are selected to promote the homogenization of the chemical composition of the material and avoid the risk of burning or decarburization caused by too long soaking time.
[0026] In a preferred embodiment, during the controlled rolling, the initial rolling temperature is controlled to be 1080~1130℃, the initial rolling reduction is 26%~33%, and an appropriate initial rolling temperature is selected to control the subsequent rolling temperature. With an appropriate initial rolling reduction, the induced precipitation of Nb element in the initial rolling stage is promoted to pin the grain boundary, so as to avoid excessive initial rolling reduction, and avoid excessive initial rolling reduction causing the precipitation distribution of Nb to be too small and coarsening in the final rolling stage, so as to prepare for grain refinement.
[0027] In a preferred embodiment, during the controlled rolling, the final rolling temperature is controlled to be ≥920°C, the final rolling reduction is 35%~45%, and a higher final rolling temperature and final rolling reduction are selected to promote the induced precipitation of Nb element in the final rolling stage, refine the grains, and strengthen the matrix.
[0028] In a preferred embodiment, the spinning temperature is 900-930° C., which can further avoid grain coarsening caused by excessively high spinning temperature.
[0029] In a preferred embodiment, the molten salt temperature of the online molten salt isotherm is 455~500℃, and the processing time is 30~70s. The lower the molten salt temperature and the longer the processing time of the online molten salt isotherm, the more austenite is transformed into troostite structure, the finer the troostite lamella spacing, the higher the wire rod strength and the lower the plasticity. However, if the molten salt temperature is too low, there is a risk of precipitation of abnormal bainite structure, and too long a processing time is not conducive to the plasticity regulation of the matrix. On the contrary, if the molten salt temperature is too high and the processing time is too short, it is not conducive to the formation of a higher degree of supercooling, the phase transformation of the troostite structure is reduced, and the troostite structure lamella spacing is coarse, which is not conducive to the transformation from high-temperature softening to spheroidization. Therefore, the molten salt temperature and processing time of the online molten salt isotherm can be further controlled to promote the transformation of high-temperature austenite to a troostite structure with finer lamella spacing, so as to prepare for the regulation of the strength and plasticity of the structure and matrix.
[0030] In a preferred embodiment, the molten salt circulation rate of the online molten salt isotherm is 500~650t / h, and the molten salt temperature rise is ≤10°C. Selecting a larger molten salt circulation rate to reduce the molten salt temperature rise can improve the temperature accuracy of the online molten salt isotherm and avoid the generation of abnormal tissue.
[0031] In a preferred embodiment, the molten salt temperature of the online molten salt precipitation control is 575-625°C, and the processing time is 500-700s. The lower the molten salt temperature of the online molten salt precipitation control, the finer the interlamellar spacing of the pearlite structure after the phase transformation, which is beneficial to the regulation of melting and tempering. However, if the molten salt temperature is too low, it is not conducive to the precipitation of Nb and V microalloying elements. On the contrary, if the molten salt temperature of the online molten salt precipitation control is higher, the interlamellar spacing of the pearlite structure after the phase transformation is coarser, the strength of the wire rod decreases, and the plasticity increases. However, if the molten salt temperature is too high, exceeding the precipitation temperature range of Nb and V microalloying elements, and even increasing the ferrite structure, it will cause the strength and plasticity of the wire rod to decrease. The longer the processing time, the better the wire rod. The more obvious the tempering softening effect of troostite and pearlite is, the more the fused pearlite structure increases, the strength of the wire rod decreases and the plasticity increases. However, if the treatment time is too long, there is a risk of precipitation and coarsening of Cr, Nb, and V, which will significantly deteriorate the strength and plasticity of the wire rod. On the contrary, if the treatment time is too short, the troostite and pearlite structures are not fully softened, the matrix strength is high but the plasticity is insufficient, which is not conducive to drawing and cold heading. Therefore, the molten salt temperature and treatment time of the online molten salt precipitation control can be further controlled, the strength and plasticity of the matrix can be further regulated to match the strength and plasticity of the matrix, and Nb and V elements can be dispersed and precipitated in large quantities in the high temperature isothermal range, thereby improving the utilization value of micro-alloying elements and greatly improving the strength and delayed fracture resistance of the material.
[0032] In a preferred embodiment, the molten salt circulation rate of the online molten salt precipitation control is 300~450t / h, the molten salt temperature rise is ≤3°C, and an appropriate molten salt circulation rate is selected to avoid increasing production energy consumption due to excessive molten salt circulation rate while maintaining the molten salt temperature and precipitation control accuracy.
[0033] In a preferred embodiment, the hot air roller strong slow cooling adopts closing the insulation cover, blowing hot air above 320°C to the insulation roller, and controlling the wire rod to be cooled to below 300°C at a cooling rate of 0.10~0.30°C / s. Due to the limited length of roller conveying, closing the insulation cover and inputting hot air further reduce the cooling rate of the wire rod after online molten salt precipitation control, thereby continuing the high temperature softening effect, regulating the strong plasticity of the wire rod, and cooling to below 300°C before coiling, which also reduces the risk of scratches on the wire rod surface, so that the coiling has better circle consistency and surface quality after coiling.
[0034] In a preferred embodiment, the hot air originates from the hot air above the salt bath tank controlled by online molten salt isothermal and online molten salt precipitation. Since hot air is generated above the salt bath tank after the high-temperature wire rod passes through the high-temperature molten salt, hot air can be used for hot air roller intensive slow cooling treatment to further recycle heat energy and reduce production energy consumption.
[0035] Compared with the prior art, the beneficial effects of the present invention are at least:
[0036] (1) In view of the current situation that there is little development of cold heading steel wire rod for 14.9 grade non-quenched and tempered bolts in China, and the insufficient performance of the parent material leads to low efficiency, increased energy consumption and cost in bolt manufacturing, the cold heading steel wire rod of the present invention is designed with microalloy and high carbon chemical composition, and the microstructure includes a high proportion of tempered troostite, a small amount of tempered pearlite and fused pearlite structure, combined with high carbon solid solution strengthening and microalloy dispersion precipitation strengthening, which makes up for the strength loss caused by reducing the content of hardenability alloy and microalloy components, provides higher matrix strength and material delayed fracture resistance, and significantly improves the plasticity of the wire rod through the regulation of tempered state structure, so that the tensile strength Rm of the product can reach 1350~1400MPa, and the cross-sectional shrinkage Z is 42%~48%. It is used in the application fields such as manufacturing 14.9 grade non-quenched and tempered bolts, can improve the yield rate, reduce the risk of wire breakage and cold heading cracking, and achieve the improvement of the strength grade of bolts in the field of industrial machinery and equipment, and has good market application prospects.
[0037] (2) The manufacturing method of the present invention adopts a micro-alloy and high-carbon chemical composition design combined with online molten salt isothermal and precipitation control and roller strong slow cooling technology process design. Through the online molten salt ultra-fast cooling technology, the influence of the network carbon deterioration phase is suppressed, the use value of the carbon element is improved, and a large degree of supercooling and cooling rate are used to promote the transformation of high-temperature austenite to a troostite structure with finer interlamellar spacing. Then, through online molten salt precipitation control, the elevated molten salt temperature is used to promote the initial spheroidization transformation of the material troostite and pearlite. While regulating the structure, Mo is used to suppress the coarsening of the precipitation phase. Nb and V are used to disperse and precipitate in large quantities in the high-temperature isothermal range to improve the use value of carbon elements and micro-alloy components, greatly improve the strength and delayed fracture resistance of the material, achieve structure control and strength-plasticity matching, significantly improve the yield rate, reduce the risk of surface quality deterioration, and have good industrial adaptability.
[0038] (3) The manufacturing method of the present invention selects a higher heating temperature and time to promote the homogenization of the chemical composition of the material, control different rolling reduction amounts, promote the rolling-induced precipitation of the Nb element to pin the grain boundaries, refine the grains, further strengthen the matrix, and is also suitable for online molten salt isothermal and precipitation control and regulation. It can also recycle the air thermal energy after online molten salt treatment to reduce energy consumption, and has good industrial adaptability. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0040] Figure 1 is a metallographic structure diagram of Example 1 of the present invention;
[0041] Figure 2 is the metallographic structure diagram of Example 2 of the present invention;
[0042] Figure 3 It is the metallographic structure diagram of Example 3 of the present invention. DETAILED DESCRIPTION
[0043] The embodiments described below with reference to the accompanying drawings are exemplary and are only for the purpose of illustration and do not limit the description of the features and characteristics of the present invention. They are intended to be used to explain the present invention and are sufficient to enable those skilled in the art to implement the present invention, but should not be construed as limiting the scope of the present invention. Embodiment 1:
[0044] A preferred embodiment of the manufacturing method of the 14.9 grade non-quenched and tempered bolt cold heading steel wire rod of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.83%, Si: 0.38%, Mn: 0.45%, Cr: 0.1%, Nb: 0.03%, V: 0.04%, Mo: 0.41%, P: 0.015%, S: 0.014%, and the rest is Fe and unavoidable impurities; the manufacturing method is manufactured according to the process flow of controlled rolling → wire laying → online molten salt isothermal → online molten salt precipitation control → hot air roller strong slow cooling → coiling, specifically:
[0045] The controlled rolling is used to heat the steel billet with a specification of 180mm×180mm through a heating furnace to achieve a high-temperature steel billet that can be rolled into plasticity. A higher heating temperature and time are selected to promote the homogenization of the chemical composition of the material, and then the steel billet coming out of the heating furnace is rolled into a wire with a diameter of 10mm through a rolling line. Appropriate rolling temperature and different reduction amounts for initial rolling and final rolling are used to promote the rolling-induced precipitation of Nb elements to pin the grain boundaries, refine the grains, and strengthen the wire rod matrix. Specifically: the heating procedure of the heating furnace is a preheating process with a sequential increase in temperature The wire-spinning process comprises the following steps: the first rolling process comprises a first rolling process, a second ...
[0046] The online molten salt isotherm adopts a salt bath tank A with molten salt inside. The wire rod after spinning is first conveyed by a roller to pass through the salt bath tank A, and is quickly cooled to the molten salt temperature, so that the wire rod is cooled at a cooling rate of 44°C / s, and quickly passes through the secondary network carbon precipitation interval to enter the pearlite phase region for isothermal phase transformation, and a higher degree of supercooling is used to promote the transformation of high-temperature austenite to troostite structure and refine the troostite lamella spacing. Specifically: the molten salt temperature of the online molten salt isotherm is 455°C, the processing time is 70s, the molten salt circulation volume is 650t / h, and the molten salt temperature rise is ≤10°C.
[0047] The online molten salt precipitation control adopts a salt bath tank B with molten salt inside. The wire rod that has passed through the online molten salt isotherm is transported by a roller through the salt bath tank B and quickly changes to the molten salt temperature. The increase in molten salt temperature promotes the large-scale dispersion and precipitation of Nb and V. A small amount of residual austenite in the wire rod structure is converted into pearlite structure, which promotes the initial spheroidization transformation and melting of troostite and pearlite. Specifically, the molten salt temperature of the online molten salt precipitation control is 604°C, the processing time is 500s, the molten salt circulation volume is 400t / h, and the molten salt temperature rise is ≤3°C.
[0048] The hot air roller strong slow cooling process adopts closing the insulation cover, using the insulation roller to transport the wire rod coming out of the salt bath tank B into the insulation cover, collecting the hot air above the salt bath tank A and the salt bath tank B, and blowing it as hot air above 320°C to the insulation roller, so as to perform strong slow cooling treatment on the wire rod and promote further softening of the wire rod structure. Specifically: the wire rod is controlled to cool to 290°C at a cooling rate of 0.25°C / s, and then coiled; the coiling process is used to coil the wire rod into a coil through a coiling drum, and the finished cold heading steel wire rod is obtained after packaging and storage. Its metallographic structure diagram is as follows Figure 1 shown.
[0049] Comparative Example 1:
[0050] A method for manufacturing wire rod, which differs from Example 1 in that the method is manufactured according to the process flow of controlled rolling → low-temperature wire spinning → Stelmor insulation and slow cooling → coiling, specifically: the heating furnace is controlled to have an average heating temperature of 1060°C, an average heating time of 3.5h, a furnace time of 4.5h, an initial rolling temperature of 1035°C, a final rolling temperature of 875°C, and a wire spinning temperature of 855°C. The Stelmor insulation and slow cooling adopts the method of shutting down all fans and insulation covers, and conveying the wire rod with rollers. The wire rod completes phase change in the cover at a cooling rate of 1.5°C / s, and the finished wire rod is obtained after coiling off the line.
[0051] Comparative Example 2:
[0052] A method for manufacturing wire rod, which differs from Example 1 in that the method is manufactured according to the process flow of controlled rolling → low-temperature wire spinning → air cooling → Stelmor insulation slow cooling → coiling, specifically: controlling the heating furnace to have an average heating temperature of 1075°C, an average heating time of 2.5h, a furnace time of 4.5h, an initial rolling temperature of 1050°C, a final rolling temperature of 890°C, and a wire spinning temperature of 870°C; the air cooling adopts opening a heat preservation cover, closing a fan, and conveying the wire rod with a roller, so that the wire rod is cooled to 690°C at a cooling rate of 2.3°C / s; the Stelmor insulation slow cooling adopts closing a fan and a heat preservation cover, and conveying the wire rod with a roller, so that the wire rod completes a phase change in the cover at a cooling rate of 1.2°C / s, and the finished wire rod is obtained after coiling off the line.
[0053] Comparative Example 3:
[0054] A method for manufacturing wire rod, which differs from Example 1 in that the method is manufactured according to a process flow of controlled rolling → spinning → Stelmor rapid cooling + insulation slow cooling, specifically: controlling the heating furnace to have an average heating temperature of 1130°C, the initial rolling temperature of 1105°C, the final rolling temperature of 935°C, and the spinning temperature of 915°C; the Stelmor rapid cooling + insulation slow cooling uses 1~7# fans to be turned on at 70%, so that the wire rod is cooled to 680°C at a cooling rate of 7.5°C / s, then the rear fan and insulation cover are turned off, and the wire rod is conveyed by a roller conveyor. The wire rod completes a phase change in the cover at a cooling rate of 1°C / s, and a finished wire rod is obtained after it comes off the line.
[0055] The wire rods obtained in the above-mentioned Example 1 and Comparative Examples 1 to 3 were subjected to organization and performance testing: the tensile test was conducted using "GB-T228.1-2021 Metal Material Tensile Test Part 1: Room Temperature Test Method" to obtain tensile strength and cross-sectional shrinkage, and the organization was tested according to the metal microstructure detection method of GB / T13298 standard. The comparative results obtained are shown in Table 1 below:
[0056] Table 1. Comparison of wire rod structure and properties by different manufacturing methods
[0057]
[0058] From the comparison results of Example 1 and Comparative Example 1, it can be seen that compared with low-temperature spinning, the rolling temperature is too low, which is not conducive to the precipitation of Nb grain refinement. After Stelmor insulation cooling, the level of network carbides is higher. Under continuous insulation cooling, the wire rod after troostite inoculation is already in a low-temperature state, so the interlamellar spacing of the obtained troostite structure is larger, the tissue stress and dislocation density are higher, the strength of the wire rod is limited but the plasticity is obviously insufficient. The present invention adopts micro-alloy and high-carbon chemical composition design, and suppresses the influence of network carbon deterioration phase through online molten salt ultra-fast cooling technology, improves the use value of carbon element, and utilizes large supercooling and cooling rate to promote the transformation of high-temperature austenite to troostite structure with finer interlamellar spacing, and then through online molten salt precipitation control, utilizes Nb and V to disperse and precipitate in large quantities in the high-temperature isothermal range, improves the use value of carbon element and micro-alloy components, greatly improves the strength and delayed fracture resistance of the material, realizes tissue regulation and strong plasticity matching, and can significantly improve the plasticity of the wire rod.
[0059] From the comparison results of Example 1 and Comparative Example 2, it can be seen that compared with the low-temperature wire drawing, the rolling temperature is too low, which is not conducive to the precipitation of Nb and grain refinement. Although the structure containing bainite obtained after air cooling can improve the strength of the wire rod, the plasticity is obviously insufficient and the yield rate is not high. The present invention does not contain abnormal bainite structure, and the network carbide level and wire rod plasticity are significantly improved through the regulation of tempered state structure.
[0060] From the comparison results of Example 1 and Comparative Example 3, it can be seen that compared with the appropriate rolling and spinning temperature, increasing the air cooling rate after spinning leads to the presence of martensite hard and brittle phases in the structure and coarse pearlite lamella spacing, high stress and dislocation density, and easy fracture. The present invention does not contain abnormal martensite structure, and the microstructure includes a high proportion of tempered troostite, a small amount of tempered pearlite and fused pearlite structure, combined with high carbon solid solution strengthening and microalloy dispersion precipitation strengthening, which makes up for the strength loss caused by reducing the content of hardenability alloy and microalloy components, and can significantly improve the yield rate. Embodiment 2:
[0061] A preferred embodiment of the manufacturing method of the 14.9 grade non-quenched and tempered cold heading steel wire rod for bolts of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.82%, Si: 0.4%, Mn: 0.51%, Cr: 0.15%, Nb: 0.033%, V: 0.043%, Mo: 0.45%, P: 0.012%, S: 0.013%, and the rest are Fe and unavoidable impurities; the manufacturing method is manufactured according to the process flow of controlled rolling → wire laying → online molten salt isothermal → online molten salt precipitation control → hot air roller strong slow cooling → coiling, specifically:
[0062] The controlled rolling is used to heat the steel billet with a specification of 220mm×220mm through a heating furnace to achieve a high-temperature steel billet that can be rolled into plasticity. A higher heating temperature and time are selected to promote the homogenization of the chemical composition of the material, and then the steel billet coming out of the heating furnace is rolled into a wire with a diameter of 26mm through a rolling line. Appropriate rolling temperature and different reduction amounts for initial rolling and final rolling are used to promote the rolling-induced precipitation of Nb elements to pin the grain boundaries, refine the grains, and strengthen the wire rod matrix. Specifically: the heating procedure of the heating furnace is a preheating section with sequentially increasing temperatures, In the heating section and the soaking section, the soaking temperature of the heating furnace is 1125°C, the soaking time is 2.5h, the time in the furnace is 4.5h, the initial rolling temperature is 1100°C, the initial rolling reduction is 26%, the final rolling temperature is 930°C, and the final rolling reduction is 35%; the wire-spinning process is used to make the wire rods coming out of the rolling line into wire rods through the wire-spinning mechanism, and the wire rods are spread on the rollers and transported along the rollers. A higher wire-spinning temperature is selected to control the precipitation of secondary carbon in the wire rods and form a larger degree of supercooling, so as to promote the nucleation of sorbite. Specifically, the wire-spinning temperature is controlled to be 910°C.
[0063] The online molten salt isotherm adopts a salt bath tank A with molten salt inside. The wire rod after spinning is first conveyed by a roller to pass through the salt bath tank A, and is quickly cooled to the molten salt temperature, so that the wire rod is cooled at a cooling rate of 44°C / s, and quickly passes through the secondary network carbon precipitation interval to enter the pearlite phase region for isothermal phase transformation, and a higher degree of supercooling is used to promote the transformation of high-temperature austenite to troostite structure and refine the troostite lamella spacing. Specifically: the molten salt temperature of the online molten salt isotherm is 468°C, the processing time is 58s, the molten salt circulation volume is 610t / h, and the molten salt temperature rise is ≤10°C.
[0064] The online molten salt precipitation control adopts a salt bath tank B with molten salt inside. The wire rod that has passed through the online molten salt isotherm is transported by a roller through the salt bath tank B and quickly changes to the molten salt temperature. The increase in molten salt temperature promotes the large-scale dispersion and precipitation of Nb and V. A small amount of residual austenite in the wire rod structure is converted into pearlite structure, which promotes the initial spheroidization transformation and melting of troostite and pearlite. Specifically, the molten salt temperature of the online molten salt precipitation control is 625°C, the processing time is 620s, the molten salt circulation volume is 450t / h, and the molten salt temperature rise is ≤3°C.
[0065] The hot air roller strong slow cooling process adopts closing the insulation cover, using the insulation roller to transport the wire rod coming out of the salt bath tank B into the insulation cover, collecting the hot air above the salt bath tank A and the salt bath tank B, and blowing it as hot air above 320°C to the insulation roller, so as to perform strong slow cooling treatment on the wire rod and promote further softening of the wire rod structure. Specifically: the wire rod is controlled to cool to 285°C at a cooling rate of 0.3°C / s, and then coiled; the coiling process is used to coil the wire rod into a coil through a coiling drum, and the finished cold heading steel wire rod is obtained after packaging and storage. Its metallographic structure diagram is as follows Figure 2 shown.
[0066] Comparative Example 4:
[0067] A method for manufacturing a wire rod, which differs from Example 2 in that the heating furnace soaking temperature is controlled to be 1070°C, the soaking time is 3 hours, the furnace time is 5 hours, the initial rolling temperature is 1045°C, the final rolling temperature is 885°C, and the spinning temperature is 865°C. The online molten salt isotherm cools the wire rod at a cooling rate of 38°C / s, and the finished wire rod is obtained after coiling off the line.
[0068] Comparative Example 5:
[0069] A method for manufacturing wire rod, which differs from Example 2 in that the online molten salt isothermally cools the wire rod at a cooling rate of 45°C / s, the molten salt temperature is 450°C, the processing time is 75s, the molten salt circulation rate is 700t / h, and the finished wire rod is obtained after the coil is rolled off the line.
[0070] Comparative Example 6:
[0071] A method for manufacturing wire rod, which differs from Example 2 in that the online molten salt isothermally cools the wire rod at a cooling rate of 39°C / s, the molten salt temperature is 505°C, the processing time is 25s, and the finished wire rod is obtained after coiling off the line. Embodiment 3:
[0072] A preferred embodiment of the manufacturing method of the 14.9 grade non-quenched and tempered bolt cold heading steel wire rod of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.8%, Si: 0.2%, Mn: 0.55%, Cr: 0.26%, Nb: 0.05%, V: 0.05%, Mo: 0.5%, P: 0.013%, S: 0.015%, and the rest are Fe and unavoidable impurities; the manufacturing method is manufactured according to the process flow of controlled rolling → wire laying → online molten salt isothermal → online molten salt precipitation control → hot air roller strong slow cooling → coiling, specifically:
[0073] The controlled rolling is used to heat the steel billet with a specification of 220mm×220mm through a heating furnace to achieve a high-temperature steel billet that can be rolled into plasticity. A higher heating temperature and time are selected to promote the homogenization of the chemical composition of the material, and then the steel billet coming out of the heating furnace is rolled into a wire with a diameter of 20mm through a rolling line. Appropriate rolling temperature and different reduction amounts for initial rolling and final rolling are used to promote the rolling-induced precipitation of Nb elements to pin the grain boundaries, refine the grains, and strengthen the wire rod matrix. Specifically: the heating procedure of the heating furnace is a preheating process with a sequential increase in temperature The rolling process comprises a rolling process of: a rolling mill, a rolling process of a heating section, a heating section and a soaking section, the soaking temperature of the heating furnace is 1150°C, the soaking time is 3h, the time in the furnace is 5h, the initial rolling temperature is 1130°C, the initial rolling reduction is 28%, the final rolling temperature is 955°C, and the final rolling reduction is 42%; the wire-spinning process is used to convert the wire rods exiting the rolling line into wire rods through a wire-spinning mechanism, the wire rods are spread on the roller table and transported along the roller table, and a higher wire-spinning temperature is selected to control the precipitation of secondary carbon in the wire rod and form a larger degree of supercooling, thereby promoting the nucleation of sorbite. Specifically, the wire-spinning temperature is controlled to be 930°C.
[0074] The online molten salt isotherm adopts a salt bath tank A with molten salt inside. The wire rod after spinning is first conveyed by a roller to pass through the salt bath tank A, and is quickly cooled to the molten salt temperature, so that the wire rod is cooled at a cooling rate of 42°C / s, and quickly passes through the secondary network carbon precipitation interval to enter the pearlite phase region for isothermal phase transformation, and a higher degree of supercooling is used to promote the transformation of high-temperature austenite to troostite structure and refine the troostite lamella spacing. Specifically: the molten salt temperature of the online molten salt isotherm is 500°C, the processing time is 30s, the molten salt circulation volume is 500t / h, and the molten salt temperature rise is ≤10°C.
[0075] The online molten salt precipitation control adopts a salt bath tank B with molten salt inside. The wire rod that has passed through the online molten salt isotherm is transported by a roller through the salt bath tank B and quickly changes to the molten salt temperature. The increase in molten salt temperature promotes the large-scale dispersion and precipitation of Nb and V. A small amount of residual austenite in the wire rod structure is converted into pearlite structure, which promotes the initial spheroidization transformation and melting of troostite and pearlite. Specifically, the molten salt temperature of the online molten salt precipitation control is 584°C, the processing time is 700s, the molten salt circulation volume is 300t / h, and the molten salt temperature rise is ≤3°C.
[0076] The hot air roller strong slow cooling process adopts closing the insulation cover, using the insulation roller to transport the wire rod coming out of the salt bath tank B into the insulation cover, collecting the hot air above the salt bath tank A and the salt bath tank B, and blowing it as hot air above 320°C to the insulation roller, so as to perform strong slow cooling treatment on the wire rod and promote further softening of the wire rod structure. Specifically: the wire rod is controlled to cool to 280°C at a cooling rate of 0.2°C / s, and then coiled; the coiling process is used to coil the wire rod into a coil through a coiling drum, and the finished cold heading steel wire rod is obtained after packaging and storage. Its metallographic structure diagram is as follows Figure 3 shown.
[0077] Comparative Example 7:
[0078] A method for manufacturing a wire rod, which differs from that of Example 3 in that the molten salt temperature of the online molten salt precipitation control is 570°C, the processing time is 450s, and the finished wire rod is obtained after the coil is rolled off the line.
[0079] Comparative Example 8:
[0080] A method for manufacturing wire rod, which differs from Example 3 in that the molten salt temperature of the online molten salt precipitation control is 630°C, the processing time is 750s, the molten salt circulation rate is 370t / h, and the finished wire rod is obtained after the coil is rolled off the line.
[0081] Comparative Example 9:
[0082] A method for manufacturing a wire rod, which differs from that of Example 3 in that the processing time of the online molten salt precipitation control is 850s, and the finished wire rod is obtained after the coil is rolled off the line. Embodiment 4:
[0083] A preferred embodiment of the manufacturing method of the 14.9 grade non-quenched and tempered bolt cold heading steel wire rod of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.84%, Si: 0.27%, Mn: 0.52%, Cr: 0.3%, Nb: 0.045%, V: 0.046%, Mo: 0.37%, P: 0.013%, S: 0.013%, and the rest is Fe and unavoidable impurities; the manufacturing method is manufactured according to the process flow of controlled rolling → wire laying → online molten salt isothermal → online molten salt precipitation control → hot air roller strong slow cooling → coiling, specifically:
[0084] The controlled rolling is used to heat a steel billet with a specification of 220mm×220mm through a heating furnace to achieve a high-temperature steel billet that can be rolled into plasticity. A higher heating temperature and time are selected to promote the homogenization of the chemical composition of the material, and then the steel billet coming out of the heating furnace is rolled into a wire with a diameter of 15mm through a rolling line. Appropriate rolling temperature and different reduction amounts for initial rolling and final rolling are used to promote the rolling-induced precipitation of Nb elements to pin the grain boundaries, refine the grains, and strengthen the wire rod matrix. Specifically: the heating procedure of the heating furnace is a preheating section, a heating section, and a soaking section with sequentially rising temperatures. The soaking temperature of the heating furnace is 1135°C, the soaking time is 2.5h, the time in the furnace is 5.5h, the initial rolling temperature is 1110°C, the initial rolling reduction is 31%, the final rolling temperature is 945°C, and the final rolling reduction is 37%.
[0085] The spinning process is used to turn the wire rod coming out of the rolling line into a wire rod through a spinning mechanism. The wire rod is spread on a roller and transported along the roller. A higher spinning temperature is selected to control the secondary carbon precipitation of the wire rod and form a larger supercooling degree, thereby promoting the nucleation of sorbite. Specifically, the spinning temperature is controlled to be 920°C.
[0086] The online molten salt isotherm adopts a salt bath tank A with molten salt inside. The wire rod after spinning is first conveyed by a roller to pass through the salt bath tank A, and is quickly cooled to the molten salt temperature, so that the wire rod is cooled at a cooling rate of 43°C / s, and quickly passes through the secondary network carbon precipitation interval to enter the pearlite phase area for isothermal phase transformation, and a higher degree of supercooling is used to promote the transformation of high-temperature austenite to troostite structure and refine the troostite lamella spacing. Specifically: the molten salt temperature of the online molten salt isotherm is 483°C, the processing time is 46s, the molten salt circulation volume is 550t / h, and the molten salt temperature rise is ≤10°C.
[0087] The online molten salt precipitation control adopts a salt bath tank B with molten salt inside. The wire rod that has been isothermally heated by the online molten salt is conveyed by a roller through the salt bath tank B and quickly changes to the molten salt temperature. The increase in molten salt temperature promotes the large-scale dispersion and precipitation of Nb and V. A small amount of residual austenite in the wire rod structure is converted into pearlite structure, which promotes the initial spheroidization transformation and melting of troostite and pearlite. Specifically, the molten salt temperature of the online molten salt precipitation control is 575°C, the processing time is 575s, the molten salt circulation volume is 330t / h, and the molten salt temperature rise is ≤3°C.
[0088] The hot air roller strong slow cooling process adopts closing the insulation cover, using the insulation roller to transport the wire rod coming out of the salt bath tank B into the insulation cover, collecting the hot air above the salt bath tank A and the salt bath tank B, and blowing it as hot air above 320°C to the insulation roller, so as to perform strong slow cooling treatment on the wire rod and promote further softening of the wire rod structure. Specifically: the wire rod is controlled to be cooled to 295°C at a cooling rate of 0.1°C / s, and then rolled; the rolling process is used to roll the wire rod into a coil by a rolling drum, and the finished cold heading steel wire rod is obtained after packaging and storage.
[0089] Comparative Example 10:
[0090] A method for manufacturing a wire rod, which differs from Example 4 in that the method is manufactured according to a process flow of controlled rolling → spinning → online molten salt isothermal → online molten salt precipitation control → roller slow cooling → coiling. Specifically: the roller slow cooling adopts a closed insulation cover, and the wire rod coming out of the salt bath tank B is conveyed into the insulation cover by a roller, and the wire rod is controlled to be cooled to 280°C at a cooling rate of 1.2°C / s, and then coiled, and the finished wire rod is obtained after the coiling is offline.
[0091] The wire rods obtained in the above-mentioned Examples 2 to 4 and Comparative Examples 4 to 10 were subjected to organization and performance testing: the tensile test was conducted using "GB-T 228.1-2021 Metallic Material Tensile Test Part 1: Room Temperature Test Method" to obtain tensile strength and cross-sectional shrinkage, and the organization was tested according to the metal microstructure detection method of GB / T13298 standard. The comparative results obtained are shown in Table 2 below:
[0092] Table 2. Comparison of the microstructure and properties of cold heading steel wire rods with different compositions and manufacturing methods
[0093]
[0094] It can be seen from the results of Examples 1 to 4 that the use of micro-alloy and high-carbon chemical composition design combined with online molten salt isothermal and precipitation control and roller strong slow cooling technology process design can achieve a product tensile strength Rm of 1350~1400MPa and a cross-sectional shrinkage rate Z of 42%~48%, which can be used in the manufacture of 14.9 grade non-quenched and tempered bolts and other application fields, improve the yield rate, reduce the risk of wire breakage during drawing and cracking during cold heading, and achieve an improvement in the strength grade of bolts in the field of industrial machinery and equipment.
[0095] From the comparison results of Example 2 and Comparative Example 4, it can be seen that the spinning temperature and rolling temperature are low, which is not conducive to the induced precipitation of the Nb element in the controlled rolling stage. After the cooling rate is reduced, it is not conducive to the nucleation of troostite. The resulting tempered troostite is less and the interlamellar spacing is larger, which is not conducive to the strength of the cold heading steel wire rod; From the comparison results of Example 2 and Comparative Example 5, it can be seen that the lower the molten salt temperature of the online molten salt isotherm and the longer the treatment time, the more austenite is transformed into troostite structure, the finer the troostite interlamellar spacing, the wire rod strength increases, and the plasticity decreases, but the molten salt temperature is too low and the treatment time is too long, the tempered troostite is more and the tempered pearlite is too little, which is not conducive to the plasticity of the wire rod; From the comparison results of Example 2 and Comparative Example 6, it can be seen that the molten salt temperature is too high and the treatment time is too short, which is not conducive to the formation of a higher degree of supercooling, the troostite structure phase transformation is reduced, and the interlamellar spacing of the resulting troostite structure is coarse, resulting in strength loss.
[0096] From the comparison results of Example 3 and Comparative Example 7, it can be seen that the lower the molten salt temperature of the online molten salt precipitation control, the finer the interlamellar spacing of the pearlite structure after the phase transformation, but the molten salt temperature is too low, which is not conducive to the precipitation of Nb and V microalloying elements. If the treatment time is too short, the troostite and pearlite structures are not fully softened, which is not conducive to the plasticity of the cold heading steel wire rod; From the comparison results of Example 3 and Comparative Example 8, it can be seen that the higher the molten salt temperature of the online molten salt precipitation control, the pearlite structure sheet after the phase transformation The coarser the interlayer spacing and the longer the treatment time, the more obvious the tempering softening effect of troostite and pearlite, the more the fused pearlite structure increases, the wire rod strength decreases and the plasticity increases, but the molten salt temperature is too high, exceeding the precipitation temperature range of Nb and V microalloying elements, the treatment time is too long, and excessive softening is not good for the strength of cold heading steel wire rod; from the comparison results of Example 3 and Comparative Example 9, it can be seen that if the treatment time is too long, there is a risk of precipitation and coarsening of Cr, Nb, and V, which will significantly deteriorate the strength and plasticity of the wire rod.
[0097] From the comparison results of Example 4 and Comparative Example 10, it can be seen that the high temperature state of the wire rod after online molten salt precipitation control by strong slow cooling on a hot air roller can promote further softening of the structure, and can also recycle the air thermal energy after online molten salt treatment to reduce energy consumption, and has good industrial adaptability.
[0098] The series of detailed descriptions listed above are only specific descriptions of feasible embodiments of the present invention, and they are not intended to limit the scope of protection of the present invention. For example, steel billets can be obtained by sequentially performing converter smelting, refining, and continuous casting processes on steelmaking raw materials. Any equivalent embodiments or changes that do not deviate from the technical spirit of the present invention should be included in the scope of protection of the present invention.
Claims
1. A 14.9 grade non-quenched and tempered cold heading steel wire rod for bolts, It is characterized in that The chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.80%-0.84%, Si: 0.20%-0.40%, Mn: 0.45%-0.55%, Cr: 0.10%-0.30%, Nb: 0.030%-0.050%, V: 0.040%-0.050%, Mo: 0.37%-0.50%, P≤0.015%, S≤0.015%, and the rest are Fe and unavoidable impurities; its microstructure includes tempered troostite with a volume percentage of ≥88%, tempered pearlite with a volume percentage of ≥5%, and the rest is a mixed structure composed of fused pearlite; the lamellar spacing of the tempered troostite is 55-95nm, the lamellar spacing of the tempered pearlite is 155-185nm, and the network carbide level of the cold heading steel wire rod is level 0.
2. The 14.9 grade non-quenched and tempered cold heading steel wire rod for bolts according to claim 1, It is characterized in that The cold heading steel wire rod has a diameter of 10.0-26.0 mm, a tensile strength of 1350-1400 MPa, and a cross-sectional shrinkage of 42%-48%.
3. A method for manufacturing a cold heading steel wire rod for non-quenched and tempered bolts of grade 14.
9. It is characterized in that The method comprises: producing a wire rod by controlled rolling according to the chemical composition of the 14.9 grade non-quenched and tempered cold heading steel wire rod for bolts as claimed in claim 1, after the wire rod is spun into a wire rod at a spinning temperature of ≥900°C, the wire rod is first subjected to online molten salt isothermal treatment, so that the wire rod is cooled to the pearlite phase region at a cooling rate of ≥42°C / s for isothermal phase transformation, promoting the transformation of high-temperature austenite to sorbite structure, and then the wire rod is subjected to online molten salt precipitation control, the molten salt temperature is increased to promote the dispersion and precipitation of Nb and V, and promote the transformation of sorbite and pearlite. The steel wire rod is subjected to preliminary spheroidizing transformation and melting, and finally subjected to strong slow cooling by a hot air roller to be made into a cold heading steel wire rod having a mixed structure consisting of tempered troostite with a volume percentage of ≥88%, tempered pearlite with a volume percentage of ≥5%, and the rest being melted pearlite. The molten salt temperature of the online molten salt isotherm is 455-500°C, and the processing time is 30-70s; the molten salt temperature of the online molten salt precipitation control is 575-625°C, and the processing time is 500-700s.
4. The method for manufacturing the 14.9 grade non-quenched and tempered steel wire rod for bolts according to claim 3, It is characterized in that During the controlled rolling, the soaking temperature of the heating furnace is controlled to be 1100-1150° C. before rolling, the soaking time is 2-3 hours, and the time in the furnace is ≥4 hours.
5. The method for manufacturing the 14.9 grade non-quenched and tempered cold heading steel wire rod for bolts according to claim 3, It is characterized in that During the controlled rolling, the initial rolling temperature is controlled to be 1080-1130° C., the initial rolling reduction is 26%-33%, the final rolling temperature is ≥920° C., and the final rolling reduction is 35%-45%.
6. The method for manufacturing the 14.9 grade non-quenched and tempered cold heading steel wire rod for bolts according to claim 3, It is characterized in that The molten salt circulation volume of the online molten salt isotherm is 500-650 t / h, and the molten salt temperature rise is ≤10°C; the molten salt circulation volume of the online molten salt precipitation control is 300-450 t / h, and the molten salt temperature rise is ≤3°C.
7. The method for manufacturing the 14.9 grade non-quenched and tempered cold heading steel wire rod for bolts according to claim 3, It is characterized in that The hot air roller strong slow cooling adopts closing the heat preservation cover, blowing hot air above 320°C to the heat preservation roller, and controlling the wire rod to be cooled to below 300°C at a cooling rate of 0.10~0.30°C / s.
8. The method for manufacturing the 14.9 grade non-quenched and tempered cold heading steel wire rod for bolts according to claim 7, It is characterized in that The hot air comes from the hot air above the salt bath tank controlled by online molten salt isothermal and online molten salt precipitation.
Citation Information
Patent Citations
Cold forging steel hot-rolled wire rod for delayed fracture-resistant 14.9-grade quenched and tempered bolt and preparation method of cold forging steel hot-rolled wire rod
CN116083806A
Ultrahigh-strength hot-rolled wire rod with tensile strength of 1600 MPa and manufacturing method thereof
CN117987742A
Hot-rolled 1300MPa-grade B-containing spring steel wire rod and production process thereof
CN118007026A
High-plasticity hot-rolled wire rod for 8.8-grade non-adjustable bolt and manufacturing method of high-plasticity hot-rolled wire rod
CN118086782A
10.9-grade hot-rolled carbon non-adjusted cold heading steel wire rod and manufacturing method thereof
CN118345307A
Cited By
Delayed-fracture-resistant non-quenched-tempered 14.9-grade high-strength cold heading steel wire rod and preparation method thereof
CN121228119A