Blended yarn braided fabric in-situ reinforced fiber reinforced composite board and preparation method thereof

By mechanical degumming and high-temperature boiling, natural fibers are spun to form blended yarns, which are alternately layered with resin fibers and then hot-pressed to prepare composite panels. This solves the problem of insufficient mechanical properties of traditional composite laminates and achieves remarkable performance. Improvement and application scope expansion.

CN118721880APending Publication Date: 2024-10-01JILIN UNIVERSITY

Patent Information

Application Number
CN202410714370.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-04
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Traditional composite laminates have poor mechanical properties, especially insufficient interlaminar shear resistance, which limits their application scope.

Method used

Mechanical degumming and high-temperature boiling are used to treat natural fibers, and then they are spun with resin fibers in a specific proportion to form blended yarns. They are woven into braided fabrics and alternately layered with resin fiber mats, and then prepared into composite panels through a hot pressing process to realize the fiber in situ enhancement.

Benefits of technology

It significantly improves the mechanical properties of composite materials, reduces production costs, expands its application scope, and improves economic benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118721880A_ABST
    Figure CN118721880A_ABST
Patent Text Reader

Abstract

The invention discloses a blended yarn braided fabric in-situ reinforced fiber reinforced composite board and a preparation method thereof, and belongs to the technical field of textiles. The natural fibers are subjected to surface degumming treatment and blended twisting with the resin fibers to prepare the blended yarn, and the performance of the blended yarn can be changed by controlling the proportion of the natural fibers and the resin fibers and the types of the natural fibers and the resin fibers in the blending process; weaving the blended yarns into a braided fabric by using a weaving machine, wherein the braided fabric comprises a non-woven fabric, a woven fabric, a three-dimensional braided fabric and the like; the prepared braided fabric has self-adhesion during hot melting, and then the braided fabric and the fiber felt are molded into the composite laminated board through a hot mold pressing method, so that the purpose of structural reinforcement is achieved. When the braided fabric is used for hot mold pressing, no adhesive is added, and the structure is enhanced by utilizing the self-adhesion characteristic of the braided fabric. The composite material laminated board is subjected to one-dimensional to three-dimensional multi-azimuth enhancement, so that the performance of the composite material laminated board is greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of textiles, and in particular relates to an in-situ reinforced fiber reinforced composite plate of a blended yarn braid and a preparation method thereof. Background Art

[0002] Fiber structure reinforced composite laminate is an emerging material with excellent performance, environmental protection, and light weight. With the development of this field, the performance of composite laminates is constantly improving, and it has replaced metal in many application fields. Nowadays, environmental issues are a hot topic in human development. The development of fiber structure reinforced composite laminates will become more extensive in future material development and application due to its excellent environmental performance.

[0003] Although traditional composite laminates have excellent environmental performance, their mechanical properties are poor and their application range is small. The process selected for the preparation of traditional composite laminates is hot pressing molding. In the preliminary experiment before hot molding, a layer of resin needs to be laid on the natural fiber and the resin fiber. The use of resin laying to improve the adhesion between the woven cloth and the fiber felt often brings some new problems. For example, it is difficult for the resin to impregnate the woven cloth during the molding process, resulting in poor shear resistance between the layers; the thickness of the resin layer will also affect the molding parameters, ultimately resulting in poor performance of the composite laminate. The deficiencies in the various properties of the composite laminate prepared by the traditional process make its application range relatively narrow, so improvements are made on the basis of the existing preparation process to improve the performance of the composite laminate.

[0004] Structural reinforcement is a commonly used reinforcement method for composite materials. In order to achieve the purpose of structural reinforcement, natural fibers and resin fibers are spun into blended yarns. Different proportions and types of natural fibers and resin fibers have different reinforcement effects when spun. The natural fibers and resin fibers are evenly interwoven together through spinning, and the obtained yarn contains two kinds of fibers. The performance of the above yarn has the excellent properties of both natural fibers and resin fibers. The spun fiber lines are used to prepare woven fabrics through different weaving methods. The prepared woven fabrics have self-adhesive properties. Then, the woven fabrics are used to prepare composite laminates through molding. Different laying methods are used during the laying process, and the reinforcement effects are also different, ultimately achieving the purpose of structural reinforcement of composite laminates. Summary of the invention

[0005] In order to solve the problems of poor interlayer shear resistance in preparing fiber structure reinforced composite laminates by resin laying, the present invention proposes a blended yarn braided fabric in-situ reinforced fiber reinforced composite plate and a preparation method thereof. The technical solution adopted by the present invention is as follows:

[0006] A method for preparing a blended yarn braided fabric in-situ reinforced fiber reinforced composite plate, the specific steps are:

[0007] (1) Mechanically degumming natural fibers at room temperature; then boiling the natural fibers in 100° C. boiling water for 1 to 3 hours; the natural fibers are a combination of one or more of hemp fibers, flax fibers, jute fibers, and ramie fibers; the natural fibers and resin fibers are both continuous fibers;

[0008] (2) spinning the natural fiber and the resin fiber treated in step (1) according to a ratio of 4 to 6 strands of natural fiber to 6 to 4 strands of resin fiber; the twist degree of the blended yarn is 30 to 80 twists per meter;

[0009] (3) placing the prepared blended yarn into a braiding machine and weaving it into a braided fabric; the braided fabric is in the form of a combination of one or more of a non-woven braided fabric, a warp and weft braided fabric, and a three-dimensional braided fabric;

[0010] (4) The woven fabric prepared in step (3) is alternately layered with the resin fiber felt; the fiber composition and proportion of the resin fiber felt are consistent with those of the woven fabric. If the woven fabric is composed of 50wt% natural fibers and 50wt% resin fibers, the resin fiber felt also contains the same types of natural fibers and resin fibers, and the ratio is also 50wt% natural fibers and 50wt% resin fibers.

[0011] (5) Prepare in-situ reinforced fiber reinforced composite panels from blended yarn braids through a hot pressing process.

[0012] Preferably, the woven fabric and the resin fiber felt are laid in a sandwich structure.

[0013] Preferably, the fineness of the natural fiber is 0.5 dtex; the fineness of the resin fiber is preferably 0.5 dtex.

[0014] Preferably, the blending method in step (2) is longitudinal blending or wrapping blending.

[0015] Preferably, the temperature of the hot pressing process in step (5) is 150-230° C. and the pressure is 4-10 MPa.

[0016] Preferably, the hot pressing process in step (5) adopts a one-stage molding process or a multi-stage molding process.

[0017] Preferably, after the hot pressing in step (5) is completed, the prepared blended yarn braided fabric in-situ reinforced fiber reinforced composite plate is cooled by mechanical cooling or air cooling.

[0018] Beneficial effects of the present invention:

[0019] The present invention removes impurities on the surface of natural hemp fibers and removes pectin, hemicellulose, lignin and other colloids in the hemp fibers by mechanical degumming and high-temperature boiling, so as to improve the softness and spinnability of hemp fibers, and enhance the spinning effect of hemp fibers and resin fibers and the performance of blended yarns. Then the treated natural hemp fibers are blended with resin fibers to obtain blended yarns. The blended yarns are then woven into braids, which innovates the structure of traditional pure natural fiber braided articles and realizes the effective fusion of resin fiber and natural fiber braided structures.

[0020] The invention obtains the in-situ reinforced fiber reinforced composite board of the blended yarn braid after laminating the blended yarn braid and the resin fiber mat and hot pressing the blended yarn braid to reduce the use of auxiliary materials, effectively reduce the production cost, and thus improve the overall economic benefits.

[0021] In addition, from one-dimensional to three-dimensional multi-directional reinforcement, the composite laminate of the present invention has significantly improved mechanical properties, expanding its potential application range. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a flow chart of preparing the self-adhesive braided fabric of the present invention;

[0023] Among them: 1-natural fiber; 2-resin fiber; 3-spinning machine; 4-fiber thread; 5-weaving machine; 6-woven fabric.

[0024] Figure 2 is a flow chart for preparing the composite laminate of the present invention;

[0025] Among them: 1-woven cloth; 2-fiber felt; 3-molding machine; 4-composite material laminate. DETAILED DESCRIPTION

[0026] The technical solution of the present invention is further explained and illustrated in the form of specific embodiments in conjunction with the accompanying drawings.

[0027] Example 1

[0028] The raw materials of this embodiment are hemp fiber and polypropylene fiber, and the specific implementation method includes the following steps:

[0029] 1) Pretreatment: Mechanical degumming of hemp fiber is performed at room temperature. Mechanical degumming can remove impurities on the surface of hemp fiber and remove pectin, hemicellulose, lignin and other colloids in hemp fiber to improve the softness and spinnability of hemp fiber; then the hemp fiber is boiled in boiling water for 1 hour to further enhance the spinnability of hemp fiber, the spinning effect of hemp fiber and polypropylene fiber, and the performance of blended yarn.

[0030] 2) Spinning the hemp fiber and polypropylene fiber treated in step 1) at a ratio of 4 strands of hemp fiber to 6 strands of polypropylene fiber, the average fineness of the hemp fiber and the polypropylene fiber is 0.5 dext, and the twist degree of the blended yarn is 30-80 twists per meter. The hemp fiber and the polypropylene fiber are blended in the longitudinal direction.

[0031] 3) The blended yarn obtained in step 2) is put into a weaving machine to weave a woven cloth by a plain weave method.

[0032] 4) The woven cloth woven in step 3) and resin fiber felt (made of 40wt% hemp fiber and 60wt% polypropylene fiber) are layered to prepare a preform with a sandwich structure. The layering method is to alternately layer a layer of woven cloth and a layer of resin fiber felt. The preform consists of two layers of woven cloth and a layer of resin fiber felt, wherein both ends of the preform are woven cloth.

[0033] 5) Place the preform in a mold, and place the mold in a molding machine. The molding machine is heated to 180°C, and the preform is molded at a pressure of 2Mpa for 3 minutes. After the molding is completed, the mold is removed and cooled to obtain the desired laminate.

[0034] Example 2

[0035] The raw materials of this embodiment are flax fiber and ABS resin fiber, and the specific implementation method includes the following steps:

[0036] 1) Pretreatment: The flax fibers were mechanically degummed at room temperature; then the flax fibers were boiled in boiling water for 1 hour.

[0037] 2) Spinning the flax fiber and ABS resin fiber treated in step 1) at a ratio of 5 strands of flax fiber to 5 strands of ABS resin fiber, wherein the average fineness of the flax fiber and the ABS resin fiber is 0.5 dext, and the twist degree of the blended yarn is 30-80 twists per meter. The hemp fiber and the polypropylene fiber are blended in the longitudinal direction.

[0038] 3) The blended yarn obtained in step 2) is put into a weaving machine to weave a woven cloth by a plain weave method.

[0039] 4) The woven cloth woven in step 3) and the resin fiber felt (made of 50wt% flax fiber and 50wt% ABS resin fiber) are layered to prepare a preform with a sandwich structure. The layering method is to alternately layer a layer of woven cloth and a layer of resin fiber felt. The preform consists of two layers of woven cloth and a layer of resin fiber felt, wherein both ends of the preform are woven cloth.

[0040] 5) Place the preform in a mold, and place the mold in a molding machine. The molding machine is heated to 220°C, and the preform is molded at a pressure of 2.5 MPa for 3 minutes. After the molding is completed, the mold is removed and cooled to obtain the desired laminate.

[0041] Example 3

[0042] This embodiment uses jute fiber and nylon fiber as synthetic fibers, and the specific implementation method includes the following steps:

[0043] 1) Pretreatment: The jute fiber was mechanically degummed at room temperature; then the jute fiber was boiled in water for 1 hour.

[0044] 2) spinning the jute fibers and nylon fibers treated in step 1) in a ratio of 6 strands of jute fibers to 4 strands of nylon fibers, wherein the average fineness of the jute fibers and the nylon fibers is 0.5 dext; the twist degree of the blended yarn is 30-80 twists per meter; and the blending method is longitudinal blending;

[0045] 3) The blended yarn obtained in step 2) is put into a weaving machine to weave a woven cloth by a plain weave method.

[0046] 4) The woven cloth woven in step 3) and resin fiber felt (made of 60wt% jute fiber and 40wt% nylon fiber) are layered to prepare a preform with a sandwich structure. The layering method is to alternately layer a layer of woven cloth and a layer of resin fiber felt. The preform consists of two layers of woven cloth and a layer of resin fiber felt, wherein both ends of the preform are woven cloth.

[0047] 5) Place the preform in a mold, and place the mold in a molding machine. The molding machine is heated to 210°C, and the preform is molded at a pressure of 2Mpa for 4 minutes. After the molding is completed, the mold is removed and cooled to obtain the desired laminate.

[0048] Example 4

[0049] This embodiment uses hemp fiber woven cloth and polypropylene resin sheet, and the specific implementation method includes the following steps:

[0050] 1) Pretreatment: The hemp fiber is mechanically degummed at room temperature; then the hemp fiber is boiled in water for 1 hour.

[0051] 2) Spinning the hemp fiber treated in step 1), wherein the fineness of the hemp fiber is 0.5 dext; the twist degree of the hemp fiber yarn is 30-80 twists per meter; and the blending method is longitudinal blending.

[0052] 3) Put the hemp fiber yarn obtained in step 2) into a weaving machine and weave it into a woven cloth by a plain weave method. In this embodiment, the total weight ratio of the hemp fiber woven cloth to the total weight of the polypropylene resin sheet is one to one.

[0053] 4) The woven cloth woven in step 3) is layered with a polypropylene resin sheet and a resin fiber felt (made of 50wt% hemp fiber and 50wt% polypropylene fiber) to prepare a preform with a sandwich structure. The layering method is to alternately layer a layer of polypropylene resin sheet, a layer of woven cloth, and a layer of resin fiber felt. The preform consists of four layers of polypropylene resin sheets, two layers of woven cloth, and a layer of resin fiber felt, wherein both ends of the preform are woven cloth.

[0054] 5) Place the preform in a mold, and place the mold in a molding machine. The molding machine is heated to 180°C, and the preform is molded at a pressure of 2Mpa for 3 minutes. After the molding is completed, the mold is removed and cooled to obtain the desired laminate.

[0055] The present invention tests the tensile strength, flexural strength and impact strength of the blended yarn braided fabric in-situ reinforced fiber reinforced composite plate obtained in Examples 1 to 4, as shown in Table 1. The results show that the blended yarn braided fabric in-situ reinforced fiber reinforced composite plate prepared by the present invention has good mechanical properties, which is better than the ordinary laminated plate in Example 4 without braided fabric in-situ reinforcement.

[0056] Table 1

[0057]

[0058] The natural fiber and resin fiber blending method involved in the present invention can adopt longitudinal blending and wrapping blending. The blending process can be carried out at room temperature, and different blending methods will affect the structure, performance and appearance of the yarn. The product obtained by longitudinal blending has better stability and uniformity; the product obtained by wrapping blending has higher strength, but the product application tends to be in a specific direction. The twist degree is adjusted according to the required performance of the braided fabric. For example, if you want to obtain a braided fabric with higher strength and roughness, you need to increase the twist degree appropriately.

[0059] The forms of the woven fabrics in the present invention include: non-woven woven fabrics, warp and weft woven fabrics, three-dimensional woven fabrics, etc. When the woven fabric in the present invention is a thicker woven fabric such as a three-dimensional woven fabric, the laying method with the fiber felt can adopt a sandwich structure; when the woven fabric is a thinner woven fabric such as a warp and weft woven fabric (woven cloth), the laying method with the fiber felt can be multiple layers, for example, one layer of woven cloth and one layer of fiber felt can be laid, or two layers of woven cloth and one layer of fiber felt can be laid alternately, or a total of five layers of materials can be laid alternately, or an asymmetric laying method of adding a layer of fiber felt on two layers of woven cloth and then laying a layer of woven cloth can be selected to achieve a variety of material combinations and performance performance.

[0060] In addition, in the process of molding laminates, one-stage molding or multi-stage molding can be used. One-stage molding simplifies the molding process and is easy to operate; multi-stage molding is a pre-pressing process for the preform before formal molding. This is a process of integrating the preforms that have not been molded after laying, and finally achieving a higher performance composite laminate. After hot molding is completed, the product can be cooled by mechanical cooling or air cooling. Mechanical cooling improves the efficiency of sample preparation; air cooling, the obtained sample has better performance, is not easy to bend, and has higher product quality.

[0061] The basic working principle, key technology and outstanding advantages of the present invention are disclosed above. Professionals and technicians in this field should understand that the embodiments provided are intended to illustrate the fundamental concept of the present invention and do not limit its application. In accordance with the spirit of the present invention and the protection scope sought, the present invention allows various possible adjustments and improvements. All these changes and improvements, as long as they are still within the protection scope of the present invention, should be considered as part of the present invention. Any changes within the protection scope of the present invention or equivalent thereto should be considered to be within the scope of the present invention.

Claims

1. A method for preparing a blended yarn braided fabric in-situ reinforced fiber reinforced composite board, characterized in that: The specific steps of this method are: (1) Mechanically degumming natural fibers at room temperature; then boiling the natural fibers in 100° C. boiling water for 1 to 3 hours; the natural fibers are a combination of one or more of hemp fibers, flax fibers, jute fibers, and ramie fibers; the natural fibers and resin fibers are both continuous fibers; (2) spinning the natural fiber and the resin fiber treated in step (1) according to a ratio of 4 to 6 strands of natural fiber to 6 to 4 strands of resin fiber; the twist degree of the blended yarn is 30 to 80 twists per meter; (3) placing the prepared blended yarn into a braiding machine and weaving it into a braided fabric; the braided fabric is in the form of a combination of one or more of a non-woven braided fabric, a warp and weft braided fabric, and a three-dimensional braided fabric; (4) alternately layering the woven fabric prepared in step (3) and the resin fiber felt, wherein the fiber composition and proportion of the resin fiber felt are consistent with those of the woven fabric; (5) Prepare in-situ reinforced fiber reinforced composite panels from blended yarn braids through a hot pressing process.

2. The method for preparing the blended yarn braided fabric in-situ reinforced fiber reinforced composite board according to claim 1, characterized in that: The fineness of the natural fiber is 0.5 dtex and / or the fineness of the resin fiber is 0.5 dtex.

3. The method for preparing the blended yarn braided fabric in-situ reinforced fiber reinforced composite board according to claim 1, characterized in that: The blending method in step (2) is longitudinal blending or wrapping blending.

4. The method for preparing the blended yarn braided fabric in-situ reinforced fiber reinforced composite board according to claim 1, characterized in that: In step (4), the woven fabric and the resin fiber felt are laid in a sandwich structure.

5. The method for preparing the blended yarn braided fabric in-situ reinforced fiber reinforced composite board according to claim 1, characterized in that: In step (5), the hot pressing process adopts one-stage molding or multi-stage molding.

6. The method for preparing the blended yarn braided fabric in-situ reinforced fiber reinforced composite board according to claim 1, characterized in that: The temperature of the hot pressing process in step (5) is 150-230° C. and the pressure is 4-10 MPa.

7. The method for preparing the blended yarn braided fabric in-situ reinforced fiber reinforced composite board according to claim 1, characterized in that: After the hot pressing in step (5) is completed, the prepared blended yarn braided fabric is cooled by mechanical cooling or air cooling to obtain an in-situ reinforced fiber reinforced composite plate.

8. An in-situ reinforced fiber-reinforced composite plate made of a blended yarn braid prepared by the method according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Blend fiber plate and preparation method thereof

    CN103317801A

  • Fiber reinforced polymer felt material with polypropylene braided fabric surface layer as well as composite board and preparation methods of fiber reinforced polymer felt material and composite board

    CN107415351A

  • Natural plant fiber hybrid composite material and preparation method

    CN110626015A

  • Process of natural fibre reinforced thermoplastic composite material production by fibre wrapping method and the product of the same process

    IN201621000249A

  • Fiber reinforced thermoplastic resin molding

    US20070116923A1

Cited By

  • Blended yarn integrated woven grid reinforcing rib composite material and preparation method thereof

    CN119980543A

  • A kind of blended yarn integrated weaving grid reinforcing rib composite material and preparation method

    CN119980543B