A kind of organic silicone adhesive for battery energy storage station

By using modified thermal fillers and epoxy resin components in the silicone adhesives in the battery energy storage station, the problems of insufficient high temperature resistance and flame retardant properties of polyurethane thermal conductivity are solved, and high thermal conductivity, strong mechanical properties and good resistance are achieved. Adhesives with combustion performance are suitable for battery storage stations and new energy electric vehicle batteries.

CN118725816BActive Publication Date: 2024-11-22SHANDONG WOSAI NEW MATERIALS TECHNOLOGY CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411231352.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-22
Estimated Expiration
2044-09-04

AI Technical Summary

Technical Problem

The existing polyurethane thermally conductive structural adhesives have poor high temperature resistance, aging resistance and flame retardant properties in battery storage stations and new energy electric vehicle battery applications, and cannot meet the reliability requirements of long service life.

Method used

Use silicone adhesive composed of components A and components B. Component A includes α,ω-dihydroxypolydimethylsiloxane, end epoxy silicone oil, modified thermal filler and liquid flame retardant. Components include bisphenol A diallyl ether, curing agent and crosslinking agent, which improves the thermal conductivity, mechanical and flame retardant properties of the adhesive by surface hydroxylation and the introduction of epoxy resin components.

Benefits of technology

It has achieved high temperature resistance, aging resistance, high thermal conductivity and flame retardancy. The thermal conductivity coefficient is between 2.28 and 2.44W/(m·k), the bonding strength and tensile strength are significantly improved, and the flame retardant level reaches V0. And maintain good performance after thermal oxygen aging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses an organic silicone adhesive for a battery energy storage station, belonging to the technical field of adhesives. The organic silicone adhesive for the battery energy storage station consists of a component A and a component B. When applying the adhesive, the component A and the component B are evenly mixed in a mass ratio of 10:3-6 and then used. The component A consists of α,ω-dihydroxy polydimethylsiloxane, epoxy-terminated silicone oil, fumed silica, modified thermal conductive filler, liquid flame retardant, and crosslinking agent 1. The component B consists of bisphenol A bisallyl ether, a curing agent, a catalyst, and a crosslinking agent 2. The organic silicone adhesive for the battery energy storage station obtained by the invention has a thermal conductivity of 2.28-2.44 W / (m·k), a bonding strength of 5.2-5.6 MPa, a tensile strength of 5.8-6.1 MPa, a flame retardant grade of V0, a ​​bonding strength of 4.2-4.5 MPa, and a tensile strength of 5.0-5.3 MPa after heat-resistant oxygen aging.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an organic silicone adhesive for a battery energy storage station, belonging to the technical field of adhesives. Background Art

[0002] Battery energy storage stations and ultra-large capacity batteries involved in the new energy vehicle industry require adhesives with high thermal conductivity and high bonding strength in their battery modules and battery packs. Currently, polyurethane adhesives are mainly used, but polyurethane adhesives have poor high temperature resistance, aging resistance and flame retardancy, and cannot meet the stringent reliability requirements during a long service life.

[0003] Chinese patent CN113736419A discloses a two-component polyurethane thermal conductive structural adhesive, including component A and component B with a volume ratio of (0.8-1.2):1; the component A includes: 10-40 parts by weight of polyether polyol; 1-10 parts by weight of chain extender; 50-90 parts by weight of first thermal conductive filler; 0.5-3 parts by weight of dispersant; 0.1-1 parts by weight of metal catalyst; the component B includes: 10-35 parts by weight of high-activity polyisocyanate; 1-15 parts by weight of polyether diol; 1-3 parts by weight of silane coupling agent; 1-5 parts by weight of low-activity polyisocyanate; 50-90 parts by weight of second thermal conductive filler. Although the two-component polyurethane thermal conductive structural adhesive obtained in this patent has very good mechanical properties and thermal conductivity, it has relatively poor high temperature resistance, aging resistance and flame retardancy, and is not suitable for long-term use of equipment with ultra-long service life such as battery energy storage stations.

[0004] Chinese patent CN114196365A discloses a high-hardness and high-adhesive thermally conductive polyurethane structural adhesive and its preparation method, wherein the structural adhesive comprises component A and component B, wherein component A comprises polyol, chain extender, castor oil, diluent, thermally conductive filler, white carbon black, antioxidant, silane coupling agent, water absorbent and catalyst; component B comprises diisocyanate, polyol, thermally conductive filler, white carbon black, silane coupling agent and water absorbent. The thermally conductive polyurethane structural adhesive obtained in this patent has good mechanical strength, but its thermal conductivity, flame retardancy and aging resistance are not ideal.

[0005] From the above, we can see that the polyurethane thermal conductive structural adhesive currently used on a large scale in battery energy storage stations or new energy electric vehicle batteries still has outstanding problems such as poor high temperature resistance, aging resistance and flame retardancy. Therefore, the development of organic silicone adhesives with high temperature resistance, aging resistance, high thermal conductivity and good flame retardancy is of great practical significance for battery energy storage stations or new energy electric vehicle batteries. Summary of the invention

[0006] In view of the shortcomings of the above-mentioned prior art, the present invention provides an organic silicone adhesive for a battery energy storage station to achieve the following invention objectives: to prepare an organic silicone adhesive that is resistant to high temperature, aging, highly thermally conductive, flame retardant and has high mechanical strength, and to provide a thermally conductive structural adhesive with good reliability during a long service life for battery energy storage stations or new energy electric vehicle batteries.

[0007] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:

[0008] An organic silicone adhesive for a battery energy storage station, the organic silicone adhesive for a battery energy storage station consisting of a component A and a component B, wherein the component A and the component B are mixed evenly in a mass ratio of 10:3-6 before use;

[0009] The specific formula of the component A is, in parts by weight:

[0010] 80-130 parts of α,ω-dihydroxy polydimethylsiloxane,

[0011] 13~30 parts of epoxy-terminated silicone oil,

[0012] 0.5~2.5 parts of fumed silica,

[0013] 50~85 parts of modified thermal conductive filler,

[0014] 15~35 parts of liquid flame retardant,

[0015] Cross-linking agent 1 4~10 parts;

[0016] The viscosity of the epoxy-terminated silicone oil is 40-80 cs, and the epoxy value is 0.04-0.06 mol / 100 g;

[0017] The particle size of the fumed silica is 10-100 nm;

[0018] The liquid flame retardant is bisphenol A bis(diphenyl phosphate);

[0019] The crosslinking agent 1 is 3-epoxypropyltrimethoxysilane;

[0020] The specific formula of the B component is, in parts by weight:

[0021] 8-18 parts of bisphenol A bisallyl ether,

[0022] 6~15 parts of curing agent,

[0023] Catalyst 0.4~0.9 parts,

[0024] Cross-linking agent 2 8-15 parts;

[0025] The curing agent is m-xylylenediamine;

[0026] The catalyst is dibutyltin dilaurate;

[0027] The crosslinking agent 2 is vinyl trimethoxy silane;

[0028] The following are further improvements to the above technical solution:

[0029] Step 1: Preparation of modified thermal conductive filler

[0030] The α-alumina and boron nitride are placed in a 100-120°C oven and dried for 7-11 hours, cooled to room temperature in a dry environment, and then added to a high-speed dispersion kettle, followed by the addition of anhydrous ethanol, and strongly dispersed at a speed of 6000-11000 rpm for 3-6 hours, and then the dispersion rate is reduced to 3000-5000 rpm, tetramethylammonium hydroxide and potassium hydroxide are added, and the temperature is raised and kept constant at 40-60°C, and after the constant temperature reaction for 2-5 hours, the temperature is reduced to room temperature, and centrifuged. The separated solid is washed with anhydrous ethanol for 2-4 times, and then placed in a 60-75°C oven and dried for 3-6 hours to obtain an alkali-treated thermal conductive filler, then add the alkali-treated thermal conductive filler to the reactor, then add an alcohol aqueous solution with an ethanol mass fraction of 70-94wt%, control the stirring rate to 500-900 rpm, heat and keep the temperature constant at 70-90°C, add glacial acetic acid to adjust the pH value of the reaction system to 4.5-5.5, add bis-[γ-(triethoxysilyl)propyl]tetrasulfide after the pH value is stable, and then stir and react at a constant temperature for 4-8 hours, cool to room temperature, centrifuge, wash the separated solid with anhydrous ethanol for 3-5 times, put it in a vacuum drying oven at 60-80°C and dry it for 5-9 hours to obtain a modified thermal conductive filler;

[0031] The α-alumina is spherical and has a particle size of 30 to 800 nm;

[0032] The particle size of the boron nitride is 10-100 nm;

[0033] The mass ratio of α-alumina, boron nitride, anhydrous ethanol, tetramethylammonium hydroxide and potassium hydroxide is 30-70:10-25:150-260:10-20:15-35;

[0034] The feed mass ratio of the alkali-treated thermal conductive filler, the alcohol aqueous solution, and bis-[γ-(triethoxysilyl)propyl]tetrasulfide is 20-60:140-220:2-5.

[0035] Step 2: Preparation of component A

[0036] According to the specific formula of component A of the organic silicone adhesive for battery energy storage station, in parts by weight, α, ω-dihydroxy polydimethylsiloxane, epoxy-terminated silicone oil, liquid flame retardant and crosslinking agent 1 are placed in a double planetary mixer. The stirring rate is controlled at 100-130 rpm and the dispersion rate is 7500-10000 rpm. Silica is added and the stirring and dispersion are continued for 5-8 hours. Then, the modified thermal conductive filler is added and the stirring and dispersion are continued for 6-10 hours to obtain the adhesive solution. After vacuum degassing, the adhesive solution is filled into a plastic finished product bottle and sealed with nitrogen to obtain the finished product of component A.

[0037] Step 3: Preparation of component B

[0038] According to the specific formula of component B of the organic silicone adhesive for battery energy storage station, in parts by weight, bisphenol A bisallyl ether, curing agent, catalyst and cross-linking agent 2 are placed in a stirring kettle, and stirred and mixed for 5 to 10 hours at a stirring rate of 500 to 900 rpm to obtain an adhesive solution, which is then vacuum degassed and filled into plastic finished product bottles, which are then sealed with nitrogen to obtain a finished product of component B.

[0039] Compared with the prior art, the present invention achieves the following beneficial effects:

[0040] 1. The present invention performs surface hydroxylation modification on α-alumina and boron nitride in an alcohol solution of tetramethylammonium hydroxide and potassium hydroxide. The etching of the two strong bases can generate a large number of hydroxyl groups on the surface of α-alumina and boron nitride. These hydroxyl groups react with the triethoxysilane structure in bis-[γ-(triethoxysilyl)propyl] tetrasulfide in an acidic alcohol aqueous solution to convert α-alumina and boron nitride with very high surface polarity into hydrophobic powders with very low polarity, which is beneficial to the dispersion uniformity of the above two high thermal conductive powders in the organic silicone adhesive resin matrix. After bis-[γ-(triethoxysilyl)propyl]tetrasulfide is chemically bonded to the surface of α-alumina and boron nitride, during the subsequent use of the adhesive in the battery energy storage station, bis-[γ-(triethoxysilyl)propyl]tetrasulfide will undergo a slow vulcanization and cross-linking reaction when heated, which further increases the density of the cured adhesive layer of the organic silicone adhesive and greatly increases the high temperature resistance of the adhesive layer during use. In addition, during the vulcanization and cross-linking process, the contact area between the α-alumina and boron nitride thermal conductive particles will be further increased, which is also conducive to maintaining the high thermal conductivity of the organic silicone adhesive for a long time.

[0041] 2. The present invention introduces epoxy resin components such as terminal epoxy silicone oil, bisphenol A bisallyl ether, curing agent m-phenylenediamine, and 3-epoxypropyltrimethoxysilane into the formula of the organic silicone adhesive. The above substances are liquids with relatively low viscosity, which have a very positive effect on reducing the viscosity of the organic silicone adhesive formula, improving fluidity, and accommodating more high thermal conductivity fillers. In addition, the introduction of the above epoxy resin components can increase the crosslinking density of the adhesive layer during curing, improve the mechanical properties of the colloid after curing, and the epoxy group has a strong bonding force, which can effectively improve the bonding strength of the organic silicone adhesive. In particular, 3-epoxypropyltrimethoxysilane, which has highly reactive epoxy groups and methoxysilane groups, is a key substance for epoxy resin molecular segments and organic silicone resin molecular segments to crosslink with each other to form an interpenetrating network polymer structure, and plays a vital role in improving the overall mechanical properties and high temperature resistance of the colloid.

[0042] 3. The present invention adds a liquid flame retardant bisphenol A bis(diphenyl phosphate) to the organic silicone adhesive formula. This flame retardant has good thermal stability and a relatively high phosphorus content, so it can effectively improve the flame retardant properties of the organic silicone adhesive, while not affecting the high temperature resistance and thermal oxygen aging properties of the organic silicone adhesive;

[0043] 4. The organic silicone adhesive for battery energy storage stations obtained by the present invention has a thermal conductivity of 2.28~2.44W / (m·k), a bonding strength of 5.2~5.6MPa, a tensile strength of 5.8~6.1MPa, a flame retardant grade of V0, a ​​bonding strength of 4.2~4.5MPa and a tensile strength of 5.0~5.3MPa after heat-resistant oxygen aging. DETAILED DESCRIPTION

[0044] The preferred embodiments of the present invention are described below. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0045] Example 1: A silicone adhesive for a battery energy storage station

[0046] Step 1: Preparation of modified thermal conductive filler

[0047] The α-alumina and boron nitride were placed in an oven at 112°C and dried for 10 hours, cooled to room temperature in a dry environment, and then added to a high-speed dispersion kettle, followed by the addition of anhydrous ethanol. After intensive dispersion at 9000 rpm for 5 hours, the dispersion rate was reduced to 4500 rpm, tetramethylammonium hydroxide and potassium hydroxide were added, the temperature was raised and kept constant at 55°C, and after a constant temperature reaction for 4 hours, the temperature was reduced to room temperature and centrifuged. The separated solid was washed with anhydrous ethanol for 3 times, placed in an oven at 70°C, and dried for 5 hours to obtain an alkali-treated thermal conductive filler. Then, the alkali-treated thermal conductive filler is added to the reactor, and then an alcohol aqueous solution with an ethanol mass fraction of 80wt% is added, the stirring rate is controlled to 850 rpm, the temperature is raised and kept constant at 83°C, and glacial acetic acid is added to adjust the pH value of the reaction system to 5. After the pH value is stable, bis-[γ-(triethoxysilyl)propyl]tetrasulfide is added, and then the reaction is stirred at a constant temperature for 5 hours, cooled to room temperature, and centrifuged. After the separated solid is washed with anhydrous ethanol for 4 times, it is placed in a vacuum drying oven at 75°C and dried for 8 hours to obtain a modified thermal conductive filler;

[0048] The α-alumina is spherical and has a particle size of 120 nm;

[0049] The particle size of the boron nitride is 30 nm;

[0050] The mass ratio of α-alumina, boron nitride, anhydrous ethanol, tetramethylammonium hydroxide and potassium hydroxide is 55:19:220:17:28;

[0051] The feed mass ratio of the alkali-treated thermal conductive filler, the alcohol aqueous solution, and bis-[γ-(triethoxysilyl)propyl]tetrasulfide is 45:170:4.

[0052] Step 2: Preparation of component A

[0053] The specific formula of the component A is, in parts by weight:

[0054] 110 parts of α,ω-dihydroxy polydimethylsiloxane,

[0055] 19 parts of epoxy-terminated silicone oil,

[0056] 1 part of fumed silica,

[0057] 75 parts of modified thermal conductive filler,

[0058] 28 parts of liquid flame retardant,

[0059] Cross-linking agent 1 8 parts;

[0060] The viscosity of the epoxy-terminated silicone oil is 65 cs, and the epoxy value is 0.05 mol / 100 g;

[0061] The particle size of the fumed silica is 20 nm;

[0062] The liquid flame retardant is bisphenol A bis(diphenyl phosphate);

[0063] The crosslinking agent 1 is 3-epoxypropyltrimethoxysilane;

[0064] According to the specific formula of component A of the organic silicone adhesive for battery energy storage station, in parts by weight, α, ω-dihydroxy polydimethylsiloxane, epoxy-terminated silicone oil, liquid flame retardant and crosslinking agent 1 are placed in a double planetary mixer. The stirring rate is controlled at 110 rpm and the dispersion rate is 9500 rpm. Silica is added and stirred and dispersed for 7 hours. After that, the modified thermal conductive filler is added and stirred and dispersed for 9 hours to obtain the adhesive solution. After vacuum degassing, the adhesive solution is filled into a plastic finished product bottle and sealed with nitrogen to obtain the finished product of component A.

[0065] Step 3: Preparation of component B

[0066] The specific formula of the B component is, in parts by weight:

[0067] 13 parts of bisphenol A bisallyl ether,

[0068] 11 parts of curing agent,

[0069] 0.7 parts of catalyst,

[0070] Cross-linking agent 2 13 parts;

[0071] The curing agent is m-xylylenediamine;

[0072] The catalyst is dibutyltin dilaurate;

[0073] The crosslinking agent 2 is vinyl trimethoxy silane;

[0074] According to the specific formula of component B of the organic silicone adhesive for battery energy storage station, bisphenol A bisallyl ether, curing agent, catalyst and cross-linking agent 2 are placed in a stirring kettle. At a stirring rate of 750 rpm, the mixture is stirred and mixed for 9 hours to obtain a glue solution. After vacuum degassing, the mixture is filled into a plastic finished product bottle, and sealed with nitrogen to obtain a finished product of component B.

[0075] Example 2: A silicone adhesive for a battery energy storage station

[0076] Step 1: Preparation of modified thermal conductive filler

[0077] The α-alumina and boron nitride were placed in a 100°C oven and dried for 7 hours, cooled to room temperature in a dry environment, and then added to a high-speed dispersion kettle, followed by the addition of anhydrous ethanol. After intensive dispersion at 6000 rpm for 3 hours, the dispersion rate was reduced to 3000 rpm, tetramethylammonium hydroxide and potassium hydroxide were added, and the temperature was raised and kept constant at 40°C. After a constant temperature reaction for 2 hours, the temperature was reduced to room temperature and centrifuged. The separated solid was washed twice with anhydrous ethanol, placed in a 60°C oven, and dried for 3 hours to obtain an alkali-treated thermal conductive filler. Then, the alkali-treated thermal conductive filler was added to the reactor, and then an alcohol aqueous solution with an ethanol mass fraction of 70wt% was added, the stirring rate was controlled to 500 rpm, the temperature was raised and kept constant at 70°C, and glacial acetic acid was added to adjust the pH value of the reaction system to 4.5. After the pH value was stable, bis-[γ-(triethoxysilyl)propyl]tetrasulfide was added, and then the reaction was stirred at a constant temperature for 4 hours, cooled to room temperature, and centrifuged. The separated solid was washed with anhydrous ethanol for 3 times, and then placed in a vacuum drying oven at 60°C and dried for 5 hours to obtain a modified thermal conductive filler;

[0078] The α-alumina is spherical and has a particle size of 30 nm;

[0079] The particle size of the boron nitride is 10 nm;

[0080] The mass ratio of α-alumina, boron nitride, anhydrous ethanol, tetramethylammonium hydroxide and potassium hydroxide is 30:10:150:10:15;

[0081] The feed mass ratio of the alkali-treated thermal conductive filler, the alcohol aqueous solution, and bis-[γ-(triethoxysilyl)propyl]tetrasulfide is 20:140:2.

[0082] Step 2: Preparation of component A

[0083] The specific formula of the component A is, in parts by weight:

[0084] 80 parts of α,ω-dihydroxy polydimethylsiloxane,

[0085] 13 parts of epoxy-terminated silicone oil,

[0086] 0.5 parts of fumed silica,

[0087] 50 parts of modified thermal conductive filler,

[0088] 15 parts of liquid flame retardant,

[0089] Cross-linking agent 1 4 parts;

[0090] The viscosity of the epoxy-terminated silicone oil is 40 cs, and the epoxy value is 0.04 mol / 100 g;

[0091] The particle size of the fumed silica is 10 nm;

[0092] The liquid flame retardant is bisphenol A bis(diphenyl phosphate);

[0093] The crosslinking agent 1 is 3-epoxypropyltrimethoxysilane;

[0094] According to the specific formula of component A of the organic silicone adhesive for battery energy storage station, in parts by weight, α, ω-dihydroxy polydimethylsiloxane, terminal epoxy silicone oil, liquid flame retardant and crosslinking agent 1 are placed in a double planetary mixer. The stirring rate is controlled at 100 rpm and the dispersion rate is 7500 rpm. Silica is added and stirred and dispersed for 5 hours. After that, the modified thermal conductive filler is added and stirred and dispersed for 6 hours to obtain the adhesive solution. After vacuum degassing, the adhesive solution is filled into a plastic finished product bottle and sealed with nitrogen to obtain the finished product of component A.

[0095] Step 3: Preparation of component B

[0096] The specific formula of the B component is, in parts by weight:

[0097] 8 parts of bisphenol A bisallyl ether,

[0098] 6 parts of curing agent,

[0099] 0.4 parts of catalyst,

[0100] Cross-linking agent 2 8 parts;

[0101] The curing agent is m-xylylenediamine;

[0102] The catalyst is dibutyltin dilaurate;

[0103] The crosslinking agent 2 is vinyl trimethoxy silane;

[0104] According to the specific formula of component B of the organic silicone adhesive for battery energy storage station, bisphenol A bisallyl ether, curing agent, catalyst and cross-linking agent 2 are put into a stirring kettle. At a stirring rate of 500 rpm, the mixture is stirred and mixed for 5 hours to obtain a glue solution. After vacuum degassing, the mixture is filled into a plastic finished product bottle, and sealed with nitrogen to obtain a finished product of component B.

[0105] Example 3: Organic silicone adhesive for battery energy storage station

[0106] Step 1: Preparation of modified thermal conductive filler

[0107] The α-alumina and boron nitride were placed in a 120°C oven and dried for 11 hours, cooled to room temperature in a dry environment, and then added to a high-speed dispersion kettle, followed by the addition of anhydrous ethanol, and dispersed vigorously at a speed of 11,000 rpm for 6 hours, and then the dispersion rate was reduced to 5,000 rpm, tetramethylammonium hydroxide and potassium hydroxide were added, and the temperature was raised and kept constant at 60°C. After the reaction was kept constant for 5 hours, the temperature was reduced to room temperature and centrifuged. The separated solid was washed with anhydrous ethanol for 4 times, and then placed in a 75°C oven and dried for 6 hours to obtain an alkali-treated thermal conductive filler. Then, the alkali-treated thermal conductive filler is added to the reactor, and then an alcohol aqueous solution with an ethanol mass fraction of 94wt% is added, the stirring rate is controlled to 900 rpm, the temperature is raised and kept constant at 90°C, and glacial acetic acid is added to adjust the pH value of the reaction system to 5.5. After the pH value is stable, bis-[γ-(triethoxysilyl)propyl]tetrasulfide is added, and then the reaction is stirred at a constant temperature for 8 hours, cooled to room temperature, and centrifuged. After the separated solid is washed with anhydrous ethanol for 5 times, it is placed in a vacuum drying oven at 80°C and dried for 9 hours to obtain a modified thermal conductive filler;

[0108] The α-alumina is spherical and has a particle size of 800 nm;

[0109] The particle size of the boron nitride is 100 nm;

[0110] The mass ratio of α-alumina, boron nitride, anhydrous ethanol, tetramethylammonium hydroxide and potassium hydroxide is 70:25:260:20:35;

[0111] The feed mass ratio of the alkali-treated thermal conductive filler, the alcohol aqueous solution, and bis-[γ-(triethoxysilyl)propyl]tetrasulfide is 60:220:5.

[0112] Step 2: Preparation of component A

[0113] The specific formula of the component A is, in parts by weight:

[0114] 130 parts of α,ω-dihydroxy polydimethylsiloxane,

[0115] 30 parts of epoxy-terminated silicone oil,

[0116] 2.5 parts of fumed silica,

[0117] 85 parts of modified thermal conductive filler,

[0118] 35 parts of liquid flame retardant,

[0119] Cross-linking agent 1 10 parts;

[0120] The viscosity of the epoxy-terminated silicone oil is 80 cs, and the epoxy value is 0.06 mol / 100 g;

[0121] The particle size of the fumed silica is 100 nm;

[0122] The liquid flame retardant is bisphenol A bis(diphenyl phosphate);

[0123] The crosslinking agent 1 is 3-epoxypropyltrimethoxysilane;

[0124] According to the specific formula of component A of the organic silicone adhesive for battery energy storage station, in parts by weight, α, ω-dihydroxy polydimethylsiloxane, terminal epoxy silicone oil, liquid flame retardant and crosslinking agent 1 are placed in a double planetary mixer. The stirring rate is controlled at 130 rpm and the dispersion rate is 10,000 rpm. Silica is added and stirred and dispersed for 8 hours. After that, the modified thermal conductive filler is added and stirred and dispersed for 10 hours to obtain the adhesive solution. After vacuum degassing, the adhesive solution is filled into a plastic finished product bottle and sealed with nitrogen to obtain the finished product of component A.

[0125] Step 3: Preparation of component B

[0126] The specific formula of the B component is, in parts by weight:

[0127] 18 parts of bisphenol A bisallyl ether,

[0128] 15 parts of curing agent,

[0129] 0.9 parts of catalyst,

[0130] Cross-linking agent 2 15 parts;

[0131] The curing agent is m-xylylenediamine;

[0132] The catalyst is dibutyltin dilaurate;

[0133] The crosslinking agent 2 is vinyl trimethoxy silane;

[0134] According to the specific formula of component B of the organic silicone adhesive for battery energy storage station, bisphenol A bisallyl ether, curing agent, catalyst and cross-linking agent 2 are put into a stirring kettle. After stirring and mixing for 10 hours at a stirring rate of 900 rpm, a glue solution is obtained. After vacuum degassing, it is filled into a plastic finished product bottle, and sealed with nitrogen to obtain a finished product of component B.

[0135] Comparative Example 1: Based on Example 1, step 1, preparation of modified thermally conductive filler, is not performed. In step 2, preparation of component A, 75 parts of modified thermally conductive filler are replaced by 75 parts of thermally conductive filler, wherein the mass ratio of α-alumina and boron nitride contained in the thermally conductive filler is the same as that in Example 1. The specific operation is as follows:

[0136] Step 1, preparation of modified thermally conductive filler is not performed;

[0137] Step 2: Preparation of component A

[0138] The specific formula of the component A is, in parts by weight:

[0139] 110 parts of α,ω-dihydroxy polydimethylsiloxane,

[0140] 19 parts of epoxy-terminated silicone oil,

[0141] 1 part of fumed silica,

[0142] 75 parts of thermal conductive filler,

[0143] 28 parts of liquid flame retardant,

[0144] Cross-linking agent 1 8 parts;

[0145] The thermal conductive filler is composed of α-aluminum oxide and boron nitride, and the mass ratio of the two is 55:19;

[0146] The α-alumina is spherical and has a particle size of 120 nm;

[0147] The particle size of the boron nitride is 30 nm;

[0148] The viscosity of the epoxy-terminated silicone oil is 65 cs, and the epoxy value is 0.05 mol / 100 g;

[0149] The particle size of the fumed silica is 20 nm;

[0150] The liquid flame retardant is bisphenol A bis(diphenyl phosphate);

[0151] The crosslinking agent 1 is 3-epoxypropyltrimethoxysilane;

[0152] According to the specific formula of component A of the organic silicone adhesive for the battery energy storage station, in parts by weight, α,ω-dihydroxy polydimethylsiloxane, epoxy-terminated silicone oil, liquid flame retardant, and crosslinking agent 1 are placed in a double planetary mixer, and the stirring rate is controlled to be 110 rpm and the dispersion rate is 9500 rpm. , fumed silica is added, and stirring and dispersing is continued for 7 hours. Then, a thermal conductive filler is added, and stirring and dispersing is continued for 9 hours to obtain a glue solution. After vacuum degassing, it is filled into a plastic finished product bottle, and sealed with nitrogen to obtain a finished product of component A;

[0153] The operation of step 3 is the same as that of embodiment 1.

[0154] Comparative Example 2: On the basis of Example 1, in step 2, in the preparation of component A, no terminal epoxy silicone oil is added, 19 parts of terminal epoxy silicone oil are replaced by 19 parts of α, ω-dihydroxy polydimethylsiloxane, 8 parts of cross-linking agent 1 are replaced by 8 parts of cross-linking agent 2, and in step 3, in the preparation of component B, 13 parts of bisphenol A bisallyl ether and 11 parts of curing agent are replaced by 24 parts of α, ω-dihydroxy polydimethylsiloxane. The specific operation is as follows:

[0155] The operation of step 1 is the same as that of embodiment 1;

[0156] Step 2: Preparation of component A

[0157] The specific formula of the component A is, in parts by weight:

[0158] 129 parts of α,ω-dihydroxy polydimethylsiloxane,

[0159] 1 part of fumed silica,

[0160] 75 parts of modified thermal conductive filler,

[0161] 28 parts of liquid flame retardant,

[0162] Cross-linking agent 2 8 parts;

[0163] The particle size of the fumed silica is 20 nm;

[0164] The liquid flame retardant is bisphenol A bis(diphenyl phosphate);

[0165] The crosslinking agent 2 is vinyl trimethoxy silane;

[0166] According to the specific formula of component A of the organic silicone adhesive for the battery energy storage station in parts by weight, α,ω-dihydroxy polydimethylsiloxane, liquid flame retardant, and crosslinking agent 2 are placed in a double planetary mixer, and the stirring rate is controlled to be 110 rpm and the dispersion rate is 9500 rpm. After adding fumed silica, stirring and dispersing for 7 hours, the modified thermal conductive filler is added, and stirring and dispersing for 9 hours is continued to obtain the adhesive solution, which is vacuum degassed and filled into a plastic finished product bottle. After nitrogen is filled and sealed, the finished product of component A is obtained;

[0167] Step 3: Preparation of component B

[0168] The specific formula of the B component is, in parts by weight:

[0169] 24 parts of α,ω-dihydroxy polydimethylsiloxane,

[0170] 0.7 parts of catalyst,

[0171] Cross-linking agent 2 13 parts;

[0172] The catalyst is dibutyltin dilaurate;

[0173] The crosslinking agent 2 is vinyl trimethoxy silane;

[0174] According to the specific formula of component B of the organic silicone adhesive for battery energy storage station, in parts by weight, α, ω-dihydroxypolydimethylsiloxane, a catalyst and a crosslinking agent 2 are placed in a stirring kettle. The mixture is stirred and mixed for 9 hours at a stirring rate of 750 rpm to obtain a glue solution. After vacuum degassing, the solution is filled into a plastic finished product bottle, and sealed with nitrogen to obtain a finished product of component B.

[0175] Comparative Example 3: Based on Example 1, in step 2, in the preparation of component A, 28 parts of liquid flame retardant are replaced by 28 parts of α,ω-dihydroxypolydimethylsiloxane. The specific operation is as follows:

[0176] The operation of step 1 is the same as that of embodiment 1;

[0177] Step 2: Preparation of component A

[0178] The specific formula of the component A is, in parts by weight:

[0179] 138 parts of α,ω-dihydroxy polydimethylsiloxane,

[0180] 19 parts of epoxy-terminated silicone oil,

[0181] 1 part of fumed silica,

[0182] 75 parts of modified thermal conductive filler,

[0183] Cross-linking agent 1 8 parts;

[0184] The viscosity of the epoxy-terminated silicone oil is 65 cs, and the epoxy value is 0.05 mol / 100 g;

[0185] The particle size of the fumed silica is 20 nm;

[0186] The crosslinking agent 1 is 3-epoxypropyltrimethoxysilane;

[0187] According to the specific formula of component A of the organic silicone adhesive for the battery energy storage station, in parts by weight, α,ω-dihydroxy polydimethylsiloxane, epoxy-terminated silicone oil, and crosslinking agent 1 are placed in a double planetary mixer, and the stirring rate is controlled to be 110 rpm and the dispersion rate is 9500 rpm. After adding fumed silica, stirring and dispersing for 7 hours, the modified thermal conductive filler is added, and stirring and dispersing for 9 hours is continued to obtain a glue solution, which is vacuum degassed and filled into a plastic finished product bottle. After nitrogen is filled and sealed, a finished product of component A is obtained;

[0188] The operation of step 3 is the same as that of embodiment 1.

[0189] Performance Test:

[0190] The organic silicone adhesives for battery energy storage stations obtained in Examples 1, 2, 3 and Comparative Examples 1, 2, 3 were mixed uniformly with component A and component B in a mass ratio of 2:1 and then glued. The following performance tests were performed on the gluing process and the obtained glue layer:

[0191] 1. Thermal conductivity: Tested in accordance with ASTM D5470-2012;

[0192] 2. Adhesion performance: Tested in accordance with GB / T 11211-2009;

[0193] 3. Tensile strength: Tested in accordance with GB / T528-2009;

[0194] 4. Flame retardant performance: tested in accordance with the US ANSI / UL-94-1985 standard;

[0195] 5. Resistance to heat and oxygen aging: After the cured adhesive layer is aged at 150°C for 500 hours, the bonding performance and tensile strength are tested;

[0196] The specific test results are shown in Table 1:

[0197] Table 1

[0198]

[0199] From the data in Table 1, it can be seen that in Comparative Example 1 where α-alumina and boron nitride are not modified, the thermal conductivity is greatly reduced, and the bonding strength, tensile strength, and bonding strength and tensile strength after thermal oxidation aging are much lower than those in Example 1, which indicates that if α-alumina and boron nitride are not surface modified, it is difficult to obtain uniform dispersion in the main resin of the organic silicone adhesive, which leads to the above two high thermal conductivity fillers being difficult to exert their excellent thermal conductivity, and also has a serious negative impact on the mechanical properties of the adhesive; in Comparative Example 2, no epoxy-terminated silicone oil, bisphenol A bisallyl ether, curing agent m-phenylenediamine, and 3-epoxypropyltrimethoxysilane are added, that is, no epoxy resin components are added to components A and B, and the thermal conductivity of Comparative Example 2 is significantly reduced, and the bonding strength and tensile strength are reduced to the same level as those in Example 1 and all the comparative examples. The lowest value in the ratio, the bonding strength and tensile strength after thermal oxidative aging are also the lowest values ​​in Example 1 and all comparative examples, which indicates that the epoxy resin components introduced into the adhesive with silicone as the main body can effectively improve the thermal conductivity, mechanical properties and thermal oxidative aging resistance of the adhesive; in Comparative Example 3 without adding the liquid flame retardant bisphenol A bis(diphenyl phosphate), the thermal conductivity is almost the same as that of Example 1, and the bonding strength and tensile strength as well as the bonding strength and tensile strength after thermal oxidative aging are slightly better than those of Example 1, but the flame retardant performance of Comparative Example 3 is much worse than that of Example 1, which indicates that the liquid flame retardant bisphenol A bis(diphenyl phosphate) has no effect on the thermal conductivity of the organic silicone adhesive, has a very slight effect on the mechanical properties of the organic silicone adhesive, and plays a vital role in improving the flame retardant performance of the organic silicone adhesive.

[0200] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. An organic silicone adhesive for a battery energy storage station, characterized in that: The organic silicone adhesive for the battery energy storage station is composed of component A and component B. When applying the adhesive, component A and component B are evenly mixed in a mass ratio of 10:3-6 and then used; The specific formula of the component A is, in parts by weight: 80-130 parts of α,ω-dihydroxy polydimethylsiloxane, 13~30 parts of epoxy-terminated silicone oil, 0.5~2.5 parts of fumed silica, 50~85 parts of modified thermal conductive filler, 15~35 parts of liquid flame retardant, Cross-linking agent 1 4~10 parts; The viscosity of the epoxy-terminated silicone oil is 40-80 cs, and the epoxy value is 0.04-0.06 mol / 100 g; The particle size of the fumed silica is 10-100 nm; The liquid flame retardant is bisphenol A bis(diphenyl phosphate); The crosslinking agent 1 is 3-epoxypropyltrimethoxysilane; The specific formula of the B component is, in parts by weight: 8-18 parts of bisphenol A bisallyl ether, 6~15 parts of curing agent, Catalyst 0.4~0.9 parts, Cross-linking agent 2 8-15 parts; The curing agent is m-xylylenediamine; The catalyst is dibutyltin dilaurate; The crosslinking agent 2 is vinyl trimethoxy silane; The modified thermal conductive filler is prepared by placing α-alumina and boron nitride in an oven at 100-120°C and drying for 7-11 hours, cooling to room temperature in a dry environment, and then adding them to a high-speed dispersion kettle, then adding anhydrous ethanol, and strongly dispersing at a speed of 6000-11000 rpm for 3-6 hours, reducing the dispersion rate to 3000-5000 rpm, adding tetramethylammonium hydroxide and potassium hydroxide, heating and maintaining a constant temperature of 40-60°C, reacting at a constant temperature for 2-5 hours, cooling to room temperature, centrifuging, washing the separated solid with anhydrous ethanol for 2-4 times, and then placing it in an oven at 60-75°C and drying it for 3-6 hours. After the alkali-treated thermal conductive filler is obtained, the alkali-treated thermal conductive filler is then added to the reactor, and then an alcohol aqueous solution with an ethanol mass fraction of 70-94wt% is added, the stirring rate is controlled to 500-900 rpm, the temperature is raised and kept constant at 70-90°C, glacial acetic acid is added to adjust the pH value of the reaction system to 4.5-5.5, after the pH value is stable, bis-[γ-(triethoxysilyl)propyl]tetrasulfide is added, and then the reaction is stirred at a constant temperature for 4-8 hours, cooled to room temperature, centrifuged, and the separated solid is washed with anhydrous ethanol for 3-5 times, and then placed in a vacuum drying oven at 60-80°C for 5-9 hours to obtain a modified thermal conductive filler; The mass ratio of α-alumina, boron nitride, anhydrous ethanol, tetramethylammonium hydroxide and potassium hydroxide is 30-70:10-25:150-260:10-20:15-35; The feed mass ratio of the alkali-treated thermal conductive filler, the alcohol aqueous solution, and bis-[γ-(triethoxysilyl)propyl]tetrasulfide is 20-60:140-220:2-5.

2. The organic silicone adhesive for a battery energy storage station according to claim 1, characterized in that: The α-alumina is spherical and has a particle size of 30 to 800 nm; The particle size of the boron nitride is 10-100 nm.

3. The organic silicone adhesive for a battery energy storage station according to claim 1, characterized in that: The preparation method of the component A is as follows: according to the specific formula of the organic silicone adhesive component A for the battery energy storage station in parts by weight, α, ω-dihydroxy polydimethylsiloxane, terminal epoxy silicone oil, liquid flame retardant, and crosslinking agent 1 are placed in a double planetary mixer, and the stirring rate is controlled at 100-130 rpm and the dispersion rate is 7500-10000 rpm, and fumed silica is added, and stirring and dispersing is continued for 5-8 hours, and then the modified thermal conductive filler is added, and stirring and dispersing is continued for 6-10 hours to obtain the adhesive solution, and after vacuum degassing, it is filled into a plastic finished product bottle, and sealed with nitrogen to obtain the finished product of component A.

4. The organic silicone adhesive for a battery energy storage station according to claim 1, characterized in that: The preparation method of the component B is as follows: according to the specific formula of the organic silicone adhesive component B for the battery energy storage station in parts by weight, bisphenol A bisallyl ether, a curing agent, a catalyst, and a crosslinking agent 2 are placed in a stirring kettle, and stirred and mixed for 5 to 10 hours at a stirring rate of 500 to 900 rpm to obtain an adhesive solution, which is then vacuum degassed and filled into a plastic finished product bottle, and sealed with nitrogen to obtain a finished product of component B.