Method for online improving interface of continuous carbon fiber reinforced PAEKs resin-based composite material

By coating the carbon fiber surface with sulfonated polyetherketoneketone SPEKK sizing agent and performing plasma grafting treatment, the problem of interfacial stability of carbon fiber reinforced PAEKs composite materials at high temperatures is solved, and excellent interfacial and mechanical properties at high temperatures are achieved. promote.

CN118727447APending Publication Date: 2024-10-01SHENYANG AEROSPACE UNIVERSITY
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410587721.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-13
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing technology is difficult to maintain the interface stability of carbon fiber reinforced PAEKs composite materials at high temperatures. Traditional sizing agents are prone to thermal decomposition during the high-temperature molding process, destroying the interface and limiting the performance of the material.

Method used

Using a method that combines sulfonated polyetherketoneketone SPEKK sizing agent with plasma surface treatment method, by coating the surface of carbon fiber with sulfonated polyetherketoneketone SPEKK sizing agent and performing plasma grafting treatment, the bonding strength between carbon fiber and resin matrix is ​​significantly improved. Interface bonding strength and adhesion.

Benefits of technology

It improves the interface strength of carbon fiber reinforced PAEKs composite materials at room temperature and maintains superior interface properties at high temperatures, significantly improves the interlaminar shear strength (ILSS value) of composite materials, and extends the mechanical properties of fibers and the service life of materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118727447A_ABST
    Figure CN118727447A_ABST
Patent Text Reader

Abstract

The invention discloses a method for online improving the interface of a continuous carbon fiber reinforced PAEKs resin-based composite material. The method comprises the following steps: coating the surface of a carbon fiber with a sulfonated polyether ketone ketone SPEKK sizing agent, and then carrying out plasma grafting treatment; and grafting the sized carbon fibers by adopting a plasma surface treatment method. According to the method, the SPEKK sizing agent is combined with the plasma to modify the carbon fiber, so that uniform full coverage is realized, the interface bonding strength between the fiber and a matrix is remarkably improved, the interface bonding property of the carbon fiber reinforced PAEKs composite material at high temperature is improved, the mechanical property of the monofilament carbon fiber is well maintained, and the mechanical property of the PAEKs composite material is improved. And the ILSS of the composite material at a high temperature is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention discloses a method for online improving the interface of a continuous carbon fiber reinforced PAEKs type resin-based composite material. Background Art

[0002] As a typical high-performance fiber material, carbon fiber (CF) has excellent properties such as high specific strength, high specific modulus, and fatigue resistance, and has become one of the most advanced reinforcements in the 21st century. PAEKs is a semi-crystalline thermoplastic polymer composed of a benzene ring and ether bonds and ketone bonds in different proportions. The presence of rigid benzene rings in the molecular chain of this type of polymer gives the resin better mechanical strength, corrosion resistance, high temperature stability and electrical insulation, and the flexible ether bonds and ketone bonds give the resin the characteristics of re-molding and easy processing. The composite of CF with special engineering plastic PAEKs resin can not only give full play to the advantages of CF's excellent physical properties and good weavability, but also have the characteristics of thermoplastic resin such as re-processing and high toughness. However, the surface of carbon fiber has a high degree of graphitization and a relatively complete graphite-like structure, while there are fewer non-carbon elements and active functional groups, resulting in a smooth fiber surface, lack of polar components, and high chemical inertness, making it difficult to be impregnated by resin and difficult to closely combine with the resin matrix to form a high interface strength.

[0003] To achieve high-performance composites, the interfacial interaction between the fiber and the resin matrix can be improved by surface modification before preparing the composite. In order to improve the adhesion of the fiber matrix, it is necessary to increase the surface polarity and create more hydrogen bonding sites. And by achieving good stress transfer from the matrix to the fiber, the possibility of covalent bonding between the fiber material and the surrounding polymer matrix is ​​increased to ensure good interfacial adhesion between the polymer and CF.

[0004] Plasma technology can be used to modify carbon fiber composites. Due to the configuration of the plasma system and the selection of treatment parameters, active substances such as positive and negative ions, neutral ions, atoms and free radicals collide with the molecules on the fiber surface, resulting in extensive chemical and physical interactions between the plasma and the fiber surface, increasing the roughness of the fiber surface and generating active free radicals or functional groups, thereby increasing the surface activity of the fiber. Its treatment effect is limited to the surface layer of the material surface, so it only changes the physical and chemical properties of the surface within tens to hundreds of nanometers, without affecting the mechanical properties of the inherent structure of the fiber. In addition, plasma combined with other modification technologies can further improve the interface properties of composite materials.

[0005] As an important component of carbon fiber, sizing agent can give carbon fiber bundling and protect the fiber, and regulate the interface of the composite material by modifying the surface of carbon fiber. It plays an important role in affecting the performance of carbon fiber reinforced thermoplastic resin-based composite materials. Therefore, the sizing agent should match the resin matrix. However, the molding temperature of high-performance PAEKs resins is usually higher than 300℃. The sizing agent of traditional thermosetting composite materials is difficult to meet the requirements of high-temperature molding of high-performance CF / PAEKs composite materials. The high temperature during the molding process will cause the traditional sizing agent to thermally decompose and produce small molecules, which will seriously damage the interface and limit the performance of the composite material.

[0006] In summary, providing a method for improving the interface stability of carbon fiber reinforced PAEKs composites at high temperatures is an urgent problem to be solved. Summary of the invention

[0007] In view of this, the present invention discloses a method for online improving the interface of continuous carbon fiber reinforced PAEKs resin-based composite materials, so as to improve the interface strength of carbon fiber reinforced PAEKs resin-based composite materials at room temperature, and still maintain excellent performance at high temperatures.

[0008] The present invention provides a method for online improving the interface of continuous carbon fiber reinforced PAEKs-type resin-based composite materials, comprising: coating a sulfonated polyetherketoneketone (SPEKK) sizing agent on the surface of carbon fiber to obtain sized carbon fiber; then treating the sized carbon fiber by a plasma surface treatment method to finally obtain grafted modified carbon fiber, and improving the interface of carbon fiber reinforced PAEKs-type resin-based composite materials online by using the grafted modified carbon fiber.

[0009] Preferably, before the sulfonated polyetherketoneketone SPEKK sizing agent is coated on the carbon fiber, if there is a sizing agent on the surface of the carbon fiber, the carbon fiber precursor needs to be pretreated: first remove the sizing agent and dust on the surface of the carbon fiber, and then remove the original sizing agent on the surface of the carbon fiber;

[0010] The method for removing the original sizing agent on the surface of the carbon fiber is as follows: soaking the carbon fiber in an organic solution for 24 hours, washing it with deionized water, taking it out after soaking it for 24 hours, drying it thoroughly, and taking it out;

[0011] The organic solution is one of methanol, ethanol, acetone and ethyl acetate or a mixture of several of them.

[0012] The drying parameters are: drying temperature is 100-120° C., and drying time is 2-3 hours.

[0013] Preferably, the process of grafting carbon fiber with SPEKK sizing agent by plasma surface treatment is as follows: the distance between the plasma electrode and the carbon fiber surface is 0.5-2 cm, the operating power is 300-1000 W, and the plasma treatment speed is 0-10 mm / s; wherein the plasma is a normal pressure continuous plasma, and the gas used to excite the plasma is any one or a mixture of several of air, oxygen with a mass purity ≥99.999%, argon with a mass purity ≥99.999%, and nitrogen with a mass purity ≥99.999%.

[0014] Preferably, the preparation method of the sulfonated polyetherketoneketone SPEKK sizing agent is: uniformly mixing the dried PEKK powder and concentrated sulfuric acid in a mass ratio of 1:10, and heating for reaction; after the reaction is completed, placing it in an ice water bath for replacement reaction; after standing, taking the precipitate, and repeatedly washing it with deionized water until the deionized water is neutral; and vacuum drying to obtain SPEKK powder;

[0015] The SPEKK powder was dissolved in a solvent at 80-100° C. to prepare sizing agent solutions with different concentrations.

[0016] Preferably, the drying temperature of the PEKK powder is 100-120°C, and the drying time is 2-3h; the temperature of the heating reaction of PEKK powder and concentrated sulfuric acid is 80-100°C, and the reaction time is 4-16h; the vacuum drying parameters are: temperature is 100-150°C, and drying time is 8-10h; the solvent is one or a mixture of water, acetone, butanone, N,N-dimethylformamide, N,N-dimethylacetamide, methanol, dimethyl sulfoxide, etc.

[0017] Preferably, the method of coating the sulfonated polyetherketoneketone SPEKK sizing agent on the surface of the carbon fiber is: immersing the carbon fiber in the SPEKK sizing agent solution, taking it out and heating and drying it; the conditions for heating and drying are: temperature of 50-120° C., and drying time of 8-12 hours.

[0018] Preferably, the grafted and modified carbon fibers are immersed in a PAEKs-type resin tank, dried, and then layered, and then formed to obtain a composite material unidirectional laminate.

[0019] Preferably, the PAEKs resin is one of polyetheretherketone PEEK, polyetherketone PEK, polyetherketoneketone PEKK, polyetheretherketoneketone PEEKK, and polyetherketoneetherketoneketone PEKEKK, or a mixture of several of them.

[0020] The present invention provides a method for online improving the interface of continuous carbon fiber reinforced PAEKs resin-based composite materials. The method uses a SPEKK sizing agent combined with plasma to modify the carbon fiber, thereby achieving uniform full coverage, significantly improving the interface bonding strength between the fiber and the matrix, and improving the interface adhesion of the carbon fiber reinforced PAEKs composite materials at high temperatures, thereby maintaining the mechanical properties of the single-filament carbon fiber and improving the ILSS of the composite material at high temperatures.

[0021] It is to be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.

[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0024] Figure 1 This is a surface morphology of carbon fiber that has not been plasma-modified in the disclosed embodiment of the present invention;

[0025] Figure 2 Surface morphology of carbon fiber after plasma modification in the disclosed embodiment of the present invention;

[0026] Figure 3 Schematic diagram of the modified preparation of continuous carbon fiber in the disclosed embodiment of the present invention. DETAILED DESCRIPTION

[0027] The present invention is further explained below in conjunction with specific implementation schemes, but it is not intended to limit the protection scope of the present invention.

[0028] In the prior art, the sizing agent of thermosetting composite materials is difficult to meet the requirements of high-temperature molding of high-performance CF / PAEKs composite materials. The high temperature during the molding process will cause the traditional sizing agent to undergo thermal decomposition and produce small molecules, which seriously damages the interface and limits the performance of the composite material. In this regard, this embodiment provides a method for online improving the interface of continuous carbon fiber reinforced PAEKs resin-based composite materials, including: coating the sulfonated polyetherketoneketone SPEKK sizing agent on the surface of the carbon fiber and then performing plasma grafting treatment; using plasma surface treatment to graft the sized carbon fiber. After treatment by this method, not only the interface strength of the carbon fiber reinforced PAEKs resin-based composite material at room temperature is improved, but also the superior performance is maintained at high temperature.

[0029] Specifically, the steps include:

[0030] 1) Carbon fiber (CF) surface desizing agent

[0031] Before plasma treatment, remove the sizing agent and dust from the carbon fiber surface. Soak the fiber in an organic solution for 24 hours, then wash it with deionized water, soak it for 24 hours, take it out, put it in an oven to dry it thoroughly, and take it out for use. Obtain the pretreated carbon fiber raw yarn with the original sizing agent removed.

[0032] If the carbon fiber has no sizing agent, it can be directly placed in the plasma equipment without pretreatment;

[0033] The organic solution is one or a mixture of methanol, ethanol, acetone and ethyl acetate for cleaning and soaking.

[0034] The carbon fiber desizing heating and drying process is as follows: the drying temperature is 100-120° C., the drying time is 2-3 hours, and the pretreated carbon fiber raw yarn is obtained.

[0035] S2: Synthesis of SPEKK sizing agent: Dry the PEKK powder, mix the PEKK powder and concentrated sulfuric acid in a mass ratio of 1:10, and heat to react. After the reaction is completed, place it in an ice water bath for replacement reaction. After standing, take the precipitate and wash it repeatedly with deionized water until the deionized water is neutral. After vacuum drying, SPEKK powder is obtained.

[0036] Specifically, the PEKK powder drying process: the drying temperature is 100-120°C, and the drying time is 2-3h.

[0037] Specifically, the PEKK powder is reacted with concentrated sulfuric acid at a temperature of 80-100° C. and a reaction time of 4-16 hours.

[0038] Specifically, the vacuum drying process: the temperature is 100-150°C, and the drying time is 8-10h.

[0039] Due to the differences in reaction time and reaction temperature, the degree of sulfonation of the prepared SPEKK powder is different. The degree of sulfonation of the SPEKK powder was determined by acid-base titration; the degree of sulfonation of the SPEKK powder in this embodiment has an important influence on the overall mechanical properties of the composite material. If the sulfonation degree is too low, its hydrophilicity is poor, it is not easily soluble in water or organic solvents, and the molecular chain has a tendency to form spherulites. In addition, the overall mechanical properties of the prepared composite material are not significantly enhanced. If the sulfonation degree is too high, the regularity of the main chain of the SPEKK molecule will decrease and the heterogeneity of the organization will increase, which will lead to the overall mechanical properties of the prepared composite material not being significantly enhanced.

[0040] Specifically, SPEKK was immersed in a 2 mol / L NaCl solution and stirred at 80° C. for 2 h. Then, acid-base titration was performed using a 0.01 mol / L NaOH solution with 0.5 wt % phenolphthalein as an indicator.

[0041] The SPEKK powder is dissolved in a solvent at 80-100°C to prepare sizing solutions of different concentrations. The most important factor affecting the thickness and uniformity of the sizing coating is the concentration of the sizing solution. If the solubility is too low, the amount of SPEKK remaining on the carbon fiber surface after drying is too small to form a uniform coating and cannot protect the carbon fiber surface. On the contrary, if the concentration is too high, too much sizing agent will remain on the carbon fiber surface after drying, the coating will be too thick, and the carbon fibers will easily adhere to each other, resulting in poor toughness of the carbon fiber bundle and reduced spinnability.

[0042] The above solvent is one or a mixture of water, acetone, butanone, N,N-dimethylformamide, N,N-dimethylacetamide, methanol, dimethyl sulfoxide, etc.

[0043] Carbon fiber sizing: Immerse the pretreated carbon fiber in the SPEKK sizing agent solution, take it out and heat and dry it.

[0044] The molding temperature of existing carbon fiber reinforced PAEKs resin-based composite materials is high, which will decompose the epoxy sizing agent on the surface of the carbon fiber, destroy the interface between the fiber and the resin, cause defects and holes, and lead to a decrease in material performance. The SPEKK in this embodiment has a high temperature resistance and can maintain the original structure unchanged at a molding temperature of 360°C.

[0045] S3: Plasma surface treatment etching process:

[0046] The carbon fibers treated with the SPEKK sizing agent are placed on a plasma operating table to obtain plasma grafted carbon fibers.

[0047] Preferably, the distance between the plasma electrode and the carbon fiber surface is 0.5-2 cm, the operating power is 300-1000 W, and the plasma processing speed is 0-10 mm / s; wherein the plasma is a normal pressure continuous plasma, and the gas used to excite the plasma is any one or a mixture of several of air, oxygen with a mass purity ≥99.999%, argon with a mass purity ≥99.999%, and nitrogen with a mass purity ≥99.999%.

[0048] In view of the molecular characteristics of carbon fiber and PAEKs resin matrix, the plasma surface treatment method is used to graft the carbon fiber surface, which further improves the material interface performance and helps to maintain the high activity of the fiber surface for a long time; and improves the service life of carbon fiber reinforced PAEKs composite materials at high temperatures.

[0049] S4: The modified CF is immersed in a PAEKs resin tank, and after drying, it is layered and formed to obtain a composite material unidirectional laminate.

[0050] PAEKs resins include: polyetheretherketone (PEEK), polyetherketone (PEK), polyetherketoneketone (PEKK), polyetheretherketoneketone (PEEKK), polyetherketoneetherketoneketone (PEKEKK), etc., or a mixture of several of them.

[0051] In this embodiment, on the basis of removing the original sizing agent of CF, the prepared SPEKK sizing agent is coated on the surface of the carbon fiber, and a plasma grafting treatment is performed to significantly increase the surface roughness of the carbon fiber, thereby forming abundant polar groups, which react physically and chemically with the prepared SPEKK sizing agent, thereby further improving the compatibility of the carbon fiber with the PAEKs resin matrix and the interface strength at high temperature.

[0052] The modification method of combining sizing agent with plasma can not only improve the interfacial mechanical properties at room temperature, but also further improve the interfacial stability of carbon fiber reinforced PAEKs composites at high temperatures and maintain good interfacial bonding strength.

[0053] The present invention is further explained below in conjunction with specific embodiments, but is not intended to limit the protection scope of the present invention.

[0054] Embodiment 1:

[0055] 1) Remove sizing agent and dust from the surface of carbon fiber. Wrap the fiber around a smooth and clean glass frame, put it into a container and soak it in an organic solvent for 24 hours, then wash it with deionized water and soak it for 24 hours, place the fiber in an oven at 100-120°C for 2-3 hours, and bake it until it is fully dry to obtain pretreated carbon fiber.

[0056] 2) After drying the PEKK powder, mix it evenly with concentrated sulfuric acid in a mass ratio of 1:10, and heat it at 80°C for 4 hours. After the reaction is completed, place it in an ice water bath for replacement reaction. After standing, take the precipitate and wash it repeatedly with deionized water until the deionized water is neutral. After vacuum drying until the water is completely removed, SPEKK powder is obtained. The degree of sulfonation is measured by acid-base titration to be 4-6%. The SPEKK powder is dissolved in water to prepare a sizing agent solution with a concentration of 0.1wt%. The pretreated carbon fiber is immersed in the SPEKK sizing agent solution, taken out, and heated and dried at 80°C for 8 hours.

[0057] 3) Use plasma equipment to treat carbon fiber with SPEKK sizing agent, the gas medium is air, the distance between the plasma electrode and the carbon fiber surface is 1.5 cm, the power is 650 W, and the processing speed is 10 mm / s.

[0058] 4) The grafted modified CF is immersed in a PAEKs (PEEK) resin tank, and after drying, it is layered and formed to obtain a composite material unidirectional laminate. The interlaminar shear strength is tested, and the ILSS value is increased by 5-7%.

[0059] Embodiment 2:

[0060] 1) Remove sizing agent and dust from the surface of carbon fiber. Wrap the fiber around a smooth and clean glass frame, put it into a container and soak it in an organic solvent for 24 hours, then wash it with deionized water and soak it for 24 hours, place the fiber in an oven at 100-120°C for 2-3 hours, and bake it until it is fully dry to obtain pretreated carbon fiber.

[0061] 2) After drying the PEKK powder, mix it evenly with concentrated sulfuric acid in a mass ratio of 1:10, and heat it at 100°C for 6 hours. After the reaction is completed, place it in an ice water bath for replacement reaction. After standing, take the precipitate and wash it repeatedly with deionized water until the deionized water is neutral. After vacuum drying until the water is completely removed, SPEKK powder is obtained. The degree of sulfonation is measured by acid-base titration to be 10-14%. The SPEKK powder is dissolved in water to prepare a sizing agent solution with a concentration of 0.15wt%. The pretreated carbon fiber is immersed in the SPEKK sizing agent solution, taken out, and heated and dried at 80°C for 8 hours.

[0062] 3) Use plasma equipment to treat carbon fiber with SPEKK sizing agent, the gas medium is air, the distance between the plasma electrode and the carbon fiber surface is 1.5 cm, the power is 650 W, and the processing speed is 8 mm / s.

[0063] 4) The grafted modified CF is immersed in a PAEKs (PEEK) resin tank, and after drying, the layers are laid and formed to obtain a composite material unidirectional laminate. The interlaminar shear strength is tested and the ILSS value is increased by 10-13%.

[0064] Embodiment 3:

[0065] 1) Remove sizing agent and dust from the surface of carbon fiber. Wrap the fiber around a smooth and clean glass frame, put it into a container and soak it in an organic solvent for 24 hours, then wash it with deionized water and soak it for 24 hours, place the fiber in an oven at 100-120°C for 2-3 hours, and bake it until it is fully dry to obtain pretreated carbon fiber.

[0066] 2) After drying the PEKK powder, mix it evenly with concentrated sulfuric acid in a mass ratio of 1:10, and heat it at 100°C for 10 hours. After the reaction is completed, place it in an ice water bath for replacement reaction. After standing, take the precipitate and wash it repeatedly with deionized water until the deionized water is neutral. After vacuum drying until the water is completely removed, SPEKK powder is obtained. The degree of sulfonation is measured by acid-base titration to be 16-20%. The SPEKK powder is dissolved in water to prepare a sizing agent solution with a concentration of 0.15wt%. The pretreated carbon fiber is immersed in the SPEKK sizing agent solution, taken out, and heated and dried at 80°C for 8 hours.

[0067] 3) Use plasma equipment to treat carbon fiber with SPEKK sizing agent, the gas medium is air, the distance between the plasma electrode and the carbon fiber surface is 1.5 cm, the power is 650 W, and the processing speed is 6 mm / s.

[0068] 4) The grafted modified CF is immersed in a PAEKs (PEKK) resin tank, and after drying, the layers are laid and formed to obtain a composite material unidirectional laminate. The interlaminar shear strength is tested and the ILSS value is increased by 16-20%.

[0069] Example 4

[0070] 1) Remove sizing agent and dust from the surface of carbon fiber. Wrap the fiber around a smooth and clean glass frame, put it into a container and soak it in an organic solvent for 24 hours, then wash it with deionized water and soak it for 24 hours, place the fiber in an oven at 100-120°C for 2-3 hours, and bake it until it is fully dry to obtain pretreated carbon fiber.

[0071] 2) After drying the PEKK powder, mix it evenly with concentrated sulfuric acid at a ratio of 1:10, and heat it at 100°C for 12 hours. After the reaction is completed, place it in an ice water bath for replacement reaction. After standing, take the precipitate and wash it repeatedly with deionized water until the deionized water is neutral. After vacuum drying until the water is completely removed, SPEKK powder is obtained. The degree of sulfonation is measured by acid-base titration to be 25-35%. The SPEKK powder is dissolved in water to prepare a sizing agent solution with a concentration of 0.15wt%. The pretreated carbon fiber is immersed in the SPEKK sizing agent solution, taken out, and heated and dried at 80°C for 8 hours.

[0072] 3) Use plasma equipment to treat carbon fiber with SPEKK sizing agent, the gas medium is air, the distance between the plasma electrode and the carbon fiber surface is 1.5cm, the power is 650W, and the processing speed is 4mm / s. The surface morphology of the carbon fiber after treatment is as follows Figure 2 As shown in Figure 2, the surface of the carbon fiber precursor without plasma treatment is Figure 1 Compared with the above, it can be observed that the surface morphology has changed significantly, with many unevenly distributed groove structures and significantly deeper surface grooves. In addition, there are some large agglomerates and protrusions on the surface. This shows that the high-energy particle bombardment in the plasma treatment improves the surface roughness of the carbon fiber and can further improve the interface performance of the composite material.

[0073] 4) The modified CF is immersed in a PAEKs (PEKK) resin tank, and after drying, the layers are laid, and the composite unidirectional laminate is obtained after molding. The interlaminar shear strength is tested, and the ILSS value is increased by 23-27%. The best effect is obtained in this embodiment, and the reasons are: the SPEKK sulfonation degree is appropriate, and the SPEKK sizing agent prepared within this sulfonation degree range has good thermal properties, is soluble in water or organic solvents, and can improve the wettability and mechanical properties of carbon fiber; the sizing agent concentration is moderate, and the sizing agent can be evenly dispersed on the surface of the carbon fiber to form a thin coating at this concentration; the plasma modification treatment improves the surface roughness and wettability of the fiber, and has little effect on the performance of the fiber body.

[0074] Example 5

[0075] 1) Remove sizing agent and dust from the surface of carbon fiber. Wrap the fiber around a smooth and clean glass frame, put it into a container and soak it in an organic solvent for 24 hours, then wash it with deionized water and soak it for 24 hours, place the fiber in an oven at 100-120°C for 2-3 hours, and bake it until it is fully dry to obtain pretreated carbon fiber.

[0076] 2) After drying the PEKK powder, mix it evenly with concentrated sulfuric acid in a mass ratio of 1:10, and heat it at 100°C for 16 hours. After the reaction is completed, place it in an ice water bath for replacement reaction. After standing, take the precipitate and wash it repeatedly with deionized water until the deionized water is neutral. After vacuum drying until the water is completely removed, SPEKK powder is obtained. The degree of sulfonation is measured by acid-base titration to be 45-60%. The SPEKK powder is dissolved in water to prepare a sizing agent solution with a concentration of 0.2wt%. The pretreated carbon fiber is immersed in the SPEKK sizing agent solution, taken out, and heated and dried at 80°C for 8 hours.

[0077] 3) Use plasma equipment to treat carbon fiber with SPEKK sizing agent, the gas medium is air, the distance between the plasma electrode and the carbon fiber surface is 1.5 cm, the power is 650 W, and the processing speed is 2 mm / s.

[0078] 4) The plasma grafted modified CF is immersed in a PAEKs (PEKK) resin tank, and after drying, it is layered and formed to obtain a composite material unidirectional laminate. The interlaminar shear strength is tested, and the ILSS value is increased by 16-19%.

[0079] Comparative Example 1

[0080] Remove sizing agent and dust from the surface of carbon fiber. Wrap the fiber on a smooth and clean glass frame, put it in a container and soak it in organic solvent for 24 hours, then wash it with deionized water and soak it for 24 hours, place the fiber in an oven at 100-120℃ for 2-3 hours, and bake it until it is fully dry to obtain pretreated carbon fiber.

[0081] The carbon fiber was pretreated using a plasma device, the gas medium was air, the distance between the plasma electrode and the carbon fiber surface was 1.5 cm, the power was 650 W, and the processing speed was 10 mm / s.

[0082] The plasma treated carbon fiber is immersed in a PAEKs resin tank, dried and layered, and then formed to obtain a composite unidirectional laminate. The interlaminar shear strength is tested and the ILSS value is increased by 3-4%.

[0083] Comparative Example 2

[0084] Remove sizing agent and dust from the surface of carbon fiber. Wrap the fiber on a smooth and clean glass frame, put it in a container and soak it in organic solvent for 24 hours, then wash it with deionized water and soak it for 24 hours, place the fiber in an oven at 100-120℃ for 2-3 hours, and bake it until it is fully dry to obtain pretreated carbon fiber.

[0085] After drying the PEKK powder, mix it evenly with concentrated sulfuric acid at a ratio of 1:10 and heat it at 100°C for 16 hours. After the reaction is completed, place it in an ice water bath for replacement reaction. After standing, take the precipitate and wash it repeatedly with deionized water until the deionized water is neutral. After vacuum drying until the water is completely removed, SPEKK powder is obtained. The degree of sulfonation is measured by acid-base titration and is 4-6%. The SPEKK powder is dissolved in water to prepare a sizing agent solution with a concentration of 0.1wt%.

[0086] The pretreated carbon fiber was immersed in the SPEKK sizing agent solution. After being taken out, it was heated and dried at 80℃ for 8 hours. The sizing-modified CF was immersed in a PAEKs (PEKK) resin tank, and after drying, it was layered and formed to obtain a composite material unidirectional laminate. The interlaminar shear strength was tested, and its ILSS value increased by 2-3%.

[0087] Those skilled in the art will readily appreciate other embodiments of the present invention after considering the specification and practicing the invention disclosed herein. This application is intended to cover any variations, uses or adaptations of the present invention that follow the general principles of the present invention and include common knowledge or customary techniques in the art that are not disclosed by the present invention. The specification and examples are to be considered exemplary only, and the true scope and spirit of the present invention are indicated by the following claims.

[0088] It should be understood that the present invention is not limited to what has been described above and that various modifications and changes may be made without departing from its scope. The scope of the present invention is limited only by the appended claims.

Claims

1. A method for improving the interface of continuous carbon fiber reinforced PAEKs resin-based composite materials online, characterized in that: include: The sulfonated polyetherketoneketone (SPEKK) sizing agent is coated on the surface of the carbon fiber to obtain the sized carbon fiber; The sized carbon fibers are then treated with a plasma surface treatment method to finally obtain grafted modified carbon fibers, and the interface of the carbon fiber reinforced PAEKs resin-based composite material is improved online through the grafted modified carbon fibers.

2. The method for online improving the interface of continuous carbon fiber reinforced PAEKs resin-based composite materials according to claim 1, characterized in that: Before the sulfonated polyetherketoneketone SPEKK sizing agent is coated on the carbon fiber, if there is a sizing agent on the surface of the carbon fiber, the carbon fiber precursor needs to be pretreated: first remove the sizing agent and dust on the surface of the carbon fiber, and then remove the original sizing agent on the surface of the carbon fiber; The method for removing the original sizing agent on the surface of the carbon fiber is as follows: soaking the carbon fiber in an organic solution for 24 hours, washing it with deionized water, taking it out after soaking it for 24 hours, drying it thoroughly, and taking it out; The organic solution is one or a mixture of methanol, ethanol, acetone and ethyl acetate; The drying parameters are: drying temperature is 100-120° C., and drying time is 2-3 hours.

3. The method for online improving the interface of continuous carbon fiber reinforced PAEKs resin-based composite materials according to claim 1, characterized in that: The preparation method of the sulfonated polyetherketoneketone SPEKK sizing agent is as follows: the dried PEKK powder is mixed with concentrated sulfuric acid in a mass ratio of 1:10, and heated for reaction; after the reaction is completed, it is placed in an ice water bath for replacement reaction; after standing, the precipitate is taken, and it is repeatedly washed with deionized water until the deionized water is neutral; and the SPEKK powder is obtained after vacuum drying; The SPEKK powder was dissolved in a solvent at 80-100° C. to prepare sizing agent solutions with different concentrations.

4. The method for online improving the interface of continuous carbon fiber reinforced PAEKs resin-based composite materials according to claim 3, characterized in that: The drying temperature of the PEKK powder is 100-120°C, and the drying time is 2-3h; the temperature of the heating reaction of the PEKK powder and concentrated sulfuric acid is 80-100°C, and the reaction time is 4-16h; the vacuum drying parameters are: temperature is 100-150°C, and the drying time is 8-10h; the solvent is one or a mixture of water, acetone, butanone, N,N-dimethylformamide, N,N-dimethylacetamide, methanol, dimethyl sulfoxide, etc.

5. The method for online improving the interface of continuous carbon fiber reinforced PAEKs resin-based composite materials according to claim 1, characterized in that: The process of grafting carbon fiber with SPEKK sizing agent by plasma surface treatment is as follows: the distance between the plasma electrode and the carbon fiber surface is 0.5-2cm, the operating power is 300-1000W, and the plasma treatment speed is 0-10mm / s; wherein the plasma is a normal pressure continuous plasma, and the gas used to excite the plasma is any one or a mixture of several of air, oxygen with a mass purity of ≥99.999%, argon with a mass purity of ≥99.999%, and nitrogen with a mass purity of ≥99.999%.

6. The method for online improving the interface of continuous carbon fiber reinforced PAEKs resin-based composite materials according to claim 1, characterized in that: The method of coating the sulfonated polyetherketoneketone SPEKK sizing agent on the surface of the carbon fiber is: immersing the carbon fiber in the SPEKK sizing agent solution, taking it out and heating and drying it; the heating and drying conditions are: the temperature is 50-120° C., and the drying time is 8-12 hours.

7. The method for online improving the interface of continuous carbon fiber reinforced PAEKs resin-based composite materials according to claim 1, characterized in that: The grafted modified carbon fiber is immersed in a PAEKs resin tank, and is layered after being dried, and is formed to obtain a composite material unidirectional laminate.

8. The method for online improving the interface of continuous carbon fiber reinforced PAEKs resin-based composite materials according to claim 1, characterized in that: The PAEKs resin is one of polyetheretherketone PEEK, polyetherketone PEK, polyetherketoneketone PEKK, polyetheretherketoneketone PEEKK, and polyetherketoneetherketoneketone PEKEKK, or a mixture of several of them.

Citation Information

Cited By

  • Composite material containing high-temperature-resistant PEKK coating and preparation method thereof