Modified white carbon black, modification method thereof, method for producing defluorinating agent and application

By modifying silica, the problem of low efficiency caused by impurities and hydrophilicity in the application of silica as a defluorination agent is solved. Through modification, the viscosity and agglomeration are reduced, and the defluorination effect and reactivity are improved. More efficient phosphoric acid defluorination and fluosilicic acid yields were achieved.

CN118851185AInactive Publication Date: 2024-10-29YUNNAN THREE CIRCLES SINOCHEM FERTILIZERS CO LTD

Patent Information

Application Number
CN202410857347.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Due to the high impurity content and hydrophilicity of existing white carbon black, it is difficult to be directly used as a defluorination agent, resulting in poor defluorination effect. In addition, soluble fluorine is brought into the wet phosphoric acid process, affecting the defluorination efficiency.

Method used

By adding deionized water, stearate and sodium carbonate to silica for reaction, and then using a tri-block aromatic derivative silane coupling agent for graft modification to form hydrophobic silica and reduce water solubility. The impurity content and reaction activity are improved, and modified white carbon black is prepared for use in dilute acid preparation of defluoridation agent.

Benefits of technology

It can effectively remove impurities in white carbon black, reduce its viscosity and agglomeration, improve defluorination effect, enhance the reactivity and filler performance of silica, and increase the fluorosilicic acid yield of phosphoric acid and the overflow rate of silicon tetrafluoride.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118851185A_ABST
    Figure CN118851185A_ABST
Patent Text Reader

Abstract

The invention provides modified white carbon black, a modification method thereof, a method for producing a defluorination agent and application, relates to the technical field of comprehensive utilization of industrial solid wastes, and solves the technical problem that the defluorination effect is limited due to self-agglomeration and phosphoric acid viscosity when the existing white carbon black is used for the defluorination agent. The method comprises the following steps: adding sufficient deionized water into white carbon black to obtain white carbon black turbid liquid, heating and dissolving stearate and sodium carbonate to obtain modified solution, adding the modified solution into the white carbon black turbid liquid, and stirring for reaction; adding a triblock aromatic derivative silane coupling agent into the white carbon black turbid solution after reaction, and heating and grafting to obtain a modified silicon dioxide turbid solution; carrying out solid-liquid separation, and drying a solid phase to obtain modified white carbon black; dilute acid is added into the modified white carbon black for activating and pulping to obtain the defluorinating agent. According to the method, impurities in the white carbon black are effectively removed, and the defluorinating agent is prepared after the white carbon black is activated, so that fluorine ions in phosphoric acid can be effectively removed under the conditions of reducing self-agglomeration and reducing the viscosity of the phosphoric acid.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of comprehensive utilization and detection of industrial solid wastes, and in particular to a modified white carbon black and a modification method thereof, and a method for producing a defluorination agent and application thereof. Background Art

[0002] The direct method of producing aluminum fluoride by fluorosilicic acid has been widely used due to its advantages of simple process, easy operation, few raw material varieties and low production cost. However, a large amount of white carbon black by-product will be produced in the production process. The by-product white carbon black has a high impurity content, such as fluorosilicic acid, aluminum fluoride, aluminum fluorosilicate, etc. It is difficult to be directly used as a rubber compound or a filler for plastics and shoes. It is even more difficult to be directly used in the pesticide, feed, toothpaste, medicine, and food industries. However, if it is directly discarded, it cannot meet the requirements of environmental protection and is not conducive to the comprehensive utilization of resources. The raw materials for the direct method of producing aluminum fluoride by fluorosilicic acid are generally by-products from the wet phosphoric acid industry. In the concentration and pre-purification processes of wet phosphoric acid, excessive silicon dioxide is often required to defluorinate phosphoric acid. On the other hand, the dry-based white carbon black produced by the direct method of producing aluminum fluoride by fluorosilicic acid has a silicon dioxide content of more than 70%, which is a better defluorination agent for wet phosphoric acid. However, if untreated silica is directly used as a defluorination agent for wet-process phosphoric acid, not only will the activity of silica be low, but a certain amount of soluble fluorine will also be introduced, which is not conducive to the defluorination of wet-process phosphoric acid.

[0003] For example, the patent with publication number CN110395703A proposes a method for producing phosphoric acid defluorinating agent from aluminum fluoride byproduct white carbon black, in which white carbon black is mixed with sodium carbonate and then dried, ground, screened, etc. to obtain a wet phosphoric acid defluorinating agent. After sodium carbonate reacts with harmful impurities in the byproduct white carbon black, the dried product also contains 10% to 30% of sodium carbonate (Na2CO3). Sodium carbonate and silicon dioxide have a synergistic effect in the wet phosphoric acid defluorination process, which can enhance the defluorination process.

[0004] However, since there are many silicon hydroxyl groups remaining on the surface of silica, especially precipitated silica, which has more surface hydroxyl groups, silica is hydrophilic, resulting in untreated silica being easily absorbing moisture and agglomerating, making it difficult to infiltrate and disperse in the organic phase, and its application is greatly restricted. In the process of concentrating dilute phosphoric acid into concentrated phosphoric acid, the viscosity of phosphoric acid is relatively large, which further limits the defluorination effect of silica in phosphoric acid, resulting in poor actual defluorination effect. Summary of the invention

[0005] The invention provides a modified white carbon black and a modification method thereof, a method for producing a defluorinating agent and an application thereof, so as to solve the technical problem that the defluorinating effect of the existing white carbon black used as a defluorinating agent is limited due to self-agglomeration and phosphoric acid viscosity.

[0006] The embodiments of the present invention are implemented by the following technical solutions:

[0007] A method for modifying white carbon black comprises the following steps:

[0008] S1: adding sufficient deionized water to white carbon black to obtain a white carbon black turbid liquid, heating to dissolve stearate and sodium carbonate to obtain a modified solution, and adding the modified solution to the white carbon black turbid liquid to stir for reaction;

[0009] S2: adding a triblock aromatic derivative silane coupling agent to the white carbon black turbid liquid after the reaction and heating for grafting to obtain a modified silicon dioxide turbid liquid;

[0010] S3: separating the modified silica turbid liquid into solid-liquid phases, and drying the solid phase to obtain modified white carbon black.

[0011] Preferably, in step S1, the stearate is one or more of sodium stearate, potassium stearate, zinc stearate and calcium stearate.

[0012] Preferably, in step S1, the amount of stearate added is 8wt% to 12wt% based on the mass of white carbon black, the amount of sodium carbonate added is 10wt% to 20wt% based on the mass of white carbon black, and the dissolution temperature of the stearate is 82°C to 88°C.

[0013] Preferably, in step S2, the aromatic derivative silane coupling agent is written as RnSiX(4-n), wherein R is a functional group of an aromatic ring derivative, which is one of benzene ring, pyridine, furan, acid anhydride and catechol.

[0014] Preferably, in the step S2, in the tri-block aromatic derivative silane coupling agent, the block monomers are polyethylene glycol, halogenated alcohol and styrene in a monomer ratio of 1:0.8 to 1:1 to 1.2.

[0015] Preferably, in the step S2, the triblock aromatic derivative silane coupling agent is 2-6 wt% based on the mass of white carbon black, and the heating grafting temperature is 140°C-160°C.

[0016] A modified white carbon black is prepared by the white carbon black modification method.

[0017] A method for producing a defluorinating agent by modifying white carbon black also includes step S4: adding dilute acid to the modified white carbon black for activation and pulping to obtain the defluorinating agent.

[0018] Preferably, in the step S4, the amount of the modified silica added is 5wt% to 10wt% based on the weight of the diluted acid.

[0019] The invention discloses an application of modified white carbon black in producing a defluorinating agent. The defluorinating agent prepared by the method of producing a defluorinating agent by modified white carbon black is used for concentrated defluorination of phosphoric acid. The addition amount of the defluorinating agent is 0.5wt% to 1.1wt% based on the weight of the phosphoric acid.

[0020] When dilute phosphoric acid is concentrated, it is indirectly heated by steam in the heat exchanger and then enters the flash chamber. Due to the sudden drop in pressure, a large amount of water in the acid evaporates, and the acid concentration is increased. At the same time, a large amount of fluoride in the acid is decomposed and escapes into the water vapor to form fluorine-containing gas. The fluorine-containing gas is recycled and washed with washing liquid. When the fluorosilicic acid concentration of the monofluorine washing circulating liquid reaches the index requirement, part of it is taken out from the circulating liquid to become the fluorosilicic acid product.

[0021] When the fluorosilicic acid in phosphoric acid decomposes and escapes due to heat, the ratio of HF to SiF4 in the gas changes with the change of phosphoric acid concentration. Since SiF4 is more likely to evaporate from the system, it is necessary to add silicon dioxide to the system and react according to reaction formulas (2) and (3) to increase the overflow rate of fluorosilicic acid and silicon tetrafluoride, thereby increasing the fluorosilicic acid yield of the phosphoric acid system.

[0022] H2SiF6 = SiF4 + 2HF (heat decomposition) (1)

[0023] SiF4+2HF=H2SiF6 (2)

[0024] 6HF+SiO2=H2SiF6+H2O (3)

[0025] 3SiF4+(n+2)H2O=2H2SiF6+SiO2.nH2O(water washing absorption) (4)

[0026] By adopting the technical scheme, modified silica is obtained by removing impurities from silica and modifying it, and water-soluble impurities are removed while modifying silica, and hydrophilic silica is modified into hydrophobic silica, which effectively prevents the silica from absorbing water and agglomerating, and improves its reaction activity, and then adds dilute acid to prepare a defluorination agent, which can effectively reduce the viscosity of phosphoric acid and remove fluoride ions when concentrating phosphoric acid;

[0027] Aromatic derivative silane coupling agents embedded with polyethylene glycol, halogenated alcohol and styrene segments are heated and grafted into silica, chemical grafting is completed under high temperature and high-speed stirring, and block copolymers containing polyethylene glycol segments, halogenated alcohol segments and styrene segments are grafted onto the surface of nano-silicon dioxide using the silane coupling agent as a "bridge" to obtain a novel nanoscale enhancement system. The block copolymer of the present invention and silica synergistically play the role of activating and enhancing toughness and reducing viscosity, thereby forming a modified white carbon black with strong mechanical properties and low viscosity, embedded with polyethylene glycol molecular segments, and repeated alkoxy chain structural units with flexibility, large aromatic ring rigidity, low molecular mobility, and can reduce its thermal expansion coefficient and viscosity and increase elastic modulus; halohydrins grafted onto the surface of silica can enhance its reactivity and chemical resistance. Heat resistance and mechanical properties can prevent the grafted functional groups from reacting with dilute acid when the defluorination agent is subsequently prepared with dilute acid; at the same time, aromatic hydrogen conjugated molecules have a larger spatial structure, larger steric hindrance, and stronger repulsive force, which can greatly reduce the agglomeration between particles, improve the dispersion of silica filler in epoxy resin, and improve the mechanical and rheological properties of packaging materials. Even at a high grafting rate, the viscosity of silica will not increase;

[0028] Modified silica removes most of the water-soluble impurities, such as fluorosilicic acid and aluminum fluorosilicate, and reduces the degree of its water absorption and agglomeration, improves its reaction activity, and reduces its viscosity; it is then prepared with dilute acid to remove water-insoluble impurities, such as aluminum fluoride, and its silicon dioxide can effectively react to remove fluoride ions.

[0029] The technical solution of the embodiment of the present invention has at least the following advantages and beneficial effects:

[0030] 1. The present invention effectively removes impurities in white carbon black, and prepares a defluorination agent after activating white carbon black, so that the defluorination agent can effectively remove fluoride ions in phosphoric acid while reducing self-agglomeration and lowering the viscosity of phosphoric acid;

[0031] 2. When modifying white carbon black, the present invention firstly adopts water-soluble and stearate and sodium carbonate reaction to remove some impurities in white carbon black, and then modifies it with a triblock aromatic derivative silane coupling agent, so that it has a larger steric hindrance, and at the same time, it has a higher reaction activity during activation, and effectively prevents the addition of dilute acid, so that the grafted tube energy group reacts with the dilute acid;

[0032] 3. The aromatic derivative silane coupling agent of the present invention is three-blocked and respectively embedded with polyethylene glycol, halohydrin and styrene segments, which are grafted onto the surface of silica to increase steric hindrance and reduce particle agglomeration, which can effectively reduce the viscosity of white carbon black and improve its reactivity. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0034] Figure 1 Schematic diagram of the modified silica and its modification method and the method for producing a defluorinating agent provided in Example 1 of the present invention. DETAILED DESCRIPTION

[0035] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.

[0036] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.

[0038] In the description of the present invention, it should be noted that if the terms "center", "up", "down", "left", "right", "vertical", "horizontal", "inside", "outside" and the like appear, the orientation or position relationship indicated is based on the orientation or position relationship shown in the accompanying drawings, or is the orientation or position relationship in which the product of the application is usually placed when used. It is only for the convenience of describing the present invention and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.

[0039] In the description of the present invention, it is also necessary to explain that, unless otherwise clearly specified and limited, the terms "set", "install", "connect", and "connect" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0040] Example 1

[0041] A method for modifying white carbon black comprises the following steps:

[0042] S1: adding sufficient deionized water to white carbon black to obtain a white carbon black turbid liquid, heating to dissolve stearate and sodium carbonate to obtain a modified solution, and adding the modified solution to the white carbon black turbid liquid to stir for reaction;

[0043] S2: adding a triblock aromatic derivative silane coupling agent to the white carbon black turbid liquid after the reaction and heating for grafting to obtain a modified silicon dioxide turbid liquid;

[0044] S3: separating the modified silica turbid liquid into solid-liquid phases, and drying the solid phase to obtain modified white carbon black.

[0045] In this embodiment, in the step S1, the stearate is sodium stearate.

[0046] In this embodiment, in the step S1, the amount of stearate added is 10 wt % based on the mass of white carbon black, the amount of sodium carbonate added is 15 wt % based on the mass of white carbon black, and the dissolution temperature of the stearate is 86°C.

[0047] In this embodiment, in the step S2, in the tri-block aromatic derivative silane coupling agent, the block monomers are polyethylene glycol, halogenated alcohol and styrene in a monomer ratio of 1:1:1.

[0048] In this embodiment, in the step S2, the triblock aromatic derivative silane coupling agent is 4 wt% based on the mass of white carbon black, and the heating grafting temperature is 150°C.

[0049] A modified white carbon black is prepared by the white carbon black modification method.

[0050] A method for producing a defluorinating agent by modifying white carbon black also includes step S4: adding dilute acid to the modified white carbon black for activation and pulping to obtain the defluorinating agent.

[0051] In this embodiment, the dilute acid is dilute phosphoric acid.

[0052] In this embodiment, in the step S4, the amount of the modified silica added is 8 wt % based on the weight of the diluted acid.

[0053] The invention discloses an application of modified white carbon black in producing a defluorinating agent. The defluorinating agent prepared by the method of producing a defluorinating agent by modified white carbon black is used for concentrated defluorination of phosphoric acid. The addition amount of the defluorinating agent is 0.8wt% based on the weight of the phosphoric acid.

[0054] Example 2

[0055] The difference between this embodiment and embodiment 1 is that, in step S1, the amount of stearate added is 12 wt % based on the mass of white carbon black, and the amount of sodium carbonate added is 20 wt % based on the mass of white carbon black.

[0056] Example 3

[0057] The difference between this embodiment and embodiment 1 is that, in step S1, the amount of stearate added is 8 wt % based on the mass of white carbon black, and the amount of sodium carbonate added is 10 wt % based on the mass of white carbon black.

[0058] Example 4

[0059] The difference between this embodiment and embodiment 1 is that, in step S1, the amount of stearate added is 12 wt % based on the mass of white carbon black, and the amount of sodium carbonate added is 10 wt % based on the mass of white carbon black.

[0060] Example 5

[0061] The only difference between this embodiment and embodiment 1 is that in step S2, in the tri-block aromatic derivative silane coupling agent, the block monomers are polyethylene glycol, halogenated alcohol and styrene in a monomer ratio of 1:0.8:1.

[0062] Example 6

[0063] The only difference between this embodiment and embodiment 1 is that in step S2, in the tri-block aromatic derivative silane coupling agent, the block monomers are polyethylene glycol, halogenated alcohol and styrene in a monomer ratio of 1:1:1.2.

[0064] Example 7

[0065] The difference between this embodiment and embodiment 1 is that, in this embodiment, in step S2, the triblock aromatic derivative silane coupling agent is 2 wt % based on the mass of white carbon black.

[0066] Example 8

[0067] The difference between this embodiment and embodiment 1 is that, in step S2, the triblock aromatic derivative silane coupling agent is 6 wt % based on the mass of white carbon black.

[0068] Example 9

[0069] The only difference between this embodiment and embodiment 1 is that in step S2, the amount of modified white carbon black added is 5 wt % based on the weight of the diluted acid.

[0070] Example 10

[0071] The only difference between this embodiment and embodiment 1 is that in step S2, the amount of modified white carbon black added is 10 wt % based on the weight of the diluted acid.

[0072] Embodiment 11

[0073] The only difference between this embodiment and embodiment 1 is that in step S2, the amount of modified white carbon black added is 0.5 wt % based on the weight of the diluted acid.

[0074] Example 12

[0075] The only difference between this embodiment and embodiment 1 is that in step S2, the amount of modified white carbon black added is 1.1 wt % based on the weight of the diluted acid.

[0076] Comparative Example 1

[0077] The difference between this comparative example and Example 1 is that in step S1, the modification of the next step is directly carried out after the white carbon black is dissolved in water, without adding stearate and sodium carbonate solution.

[0078] Comparative Example 2

[0079] The difference between this comparative example and Example 1 is that in step S2, the modification is performed using a common non-block copolymer silane coupling agent.

[0080] Comparative Example 3

[0081] The difference between this comparative example and Example 1 is that the modified silica is directly added into the phosphoric acid as a defluorinating agent.

[0082] The composition analysis of the white carbon black raw material and the diluted acid raw material used in the above embodiments and comparative examples is shown in Table 1 below:

[0083] Table 1. Experimental data related to raw material components of Examples 1-10 and Comparative Examples 1-3 (%)

[0084] serial number White Carbon Black Dilute acid <![CDATA[Al2O3]]> 0.004 1.35 CaO - 0.19 <![CDATA[Fe2O3]]> 1.03 1.08 MgO 2.6 0.057 <![CDATA[P2O5]]> 0.18 26.12 <![CDATA[SiO2]]> - 15 As 89.96 0.84 Cd - 0.0001 Cr 0.002 0.0025 Pb 0.0152 0.0023 Hg 0.0033 0.0004 F 13.36 1.93

[0085] The relevant data of the above embodiments and comparative examples are shown in Table 2 as follows:

[0086] Table 2. Experimental data related to Examples 1-10 and Comparative Examples 1-3

[0087]

[0088] The above embodiments and comparison examples are shown in Table 3:

[0089] Table 3. Related test and calculation data of modified white carbon black and defluorinated phosphoric acid obtained in Examples 1-10 and Comparative Examples 1-3

[0090]

[0091] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for modifying white carbon black, characterized in that: The steps include: S1: adding sufficient deionized water to white carbon black to obtain a white carbon black turbid liquid, heating to dissolve stearate and sodium carbonate to obtain a modified solution, and adding the modified solution to the white carbon black turbid liquid to stir for reaction; S2: adding a triblock aromatic derivative silane coupling agent to the white carbon black turbid liquid after the reaction and heating for grafting to obtain a modified silicon dioxide turbid liquid; S3: separating the modified silica turbid liquid into solid-liquid phases, and drying the solid phase to obtain modified white carbon black.

2. A method for modifying white carbon black according to claim 1, characterized in that: In the step S1, the stearate is one or more of sodium stearate, potassium stearate, zinc stearate and calcium stearate.

3. A method for modifying white carbon black according to claim 1, characterized in that: In the step S1, the amount of stearate added is 8wt% to 12wt% based on the mass of white carbon black, the amount of sodium carbonate added is 10wt% to 20wt% based on the mass of white carbon black, and the dissolution temperature of the stearate is 82°C to 88°C.

4. A method for modifying white carbon black according to claim 1, characterized in that: In step S2, the aromatic derivative silane coupling agent is written as R n SiX (4-n) , wherein R is a functional group of an aromatic ring derivative, which is one of a benzene ring, pyridine, furan, anhydride and catechol.

5. A method for modifying white carbon black according to claim 1, characterized in that: In the step S2, in the tri-block aromatic derivative silane coupling agent, the block monomers are monomers in a ratio of 1: 0.8~1:1~1.2 of polyethylene glycol, halogenated alcohol and styrene.

6. A method for modifying white carbon black according to claim 1, characterized in that: In the step S2, the triblock aromatic derivative silane coupling agent is 2-6 wt% based on the mass of white carbon black, and the heating grafting temperature is 140°C-160°C.

7. A modified white carbon black, characterized in that: The white carbon black is prepared by the white carbon black modification method according to any one of claims 1 to 7.

8. A method for producing a defluorinating agent from modified silica according to claim 7, characterized in that: The method further comprises step S4: adding dilute acid to the modified silica to activate pulping to obtain a defluorinating agent.

9. The method for producing a defluorinating agent from modified white carbon black according to claim 8, characterized in that: In the step S4, the amount of the modified white carbon black added is 5wt% to 10wt% based on the weight of the diluted acid.

10. An application of modified white carbon black in producing a defluorinating agent, characterized in that: The defluorinating agent prepared by the method for producing a defluorinating agent by modifying white carbon black as claimed in claim 8 or 9 is used for concentrated defluorination of phosphoric acid, and the added amount of the defluorinating agent is 0.5wt% to 1.1wt% based on the weight of the phosphoric acid.

Citation Information

Patent Citations

  • Method for producing phosphoric acid defluorinating agent from aluminum fluoride byproduct white carbon black

    CN110395703A

  • Preparation method of surface grafted vinyl modified white carbon black

    CN111072034A

  • Preparation method of nano white carbon black

    CN114105152A

  • Production method of high-dispersion silicon dioxide

    CN114368760A

  • Silicon dioxide surface modification method, modified silicon dioxide and application

    CN117229653A

Cited By

  • Phosphoric acid defluorination method

    CN119683586A

  • A method for defluorination of phosphoric acid

    CN119683586B